Elastic flame-retardant material, preparation method thereof and chemical power supply module

By using a combination of organic elastic foam and inorganic expansion coating in the battery module, the problems of poor flame retardant and thermal insulation effect and low safety performance are solved, and the effect of efficient thermal insulation and buffering battery cell expansion is achieved, reducing the effect of reducing the The risk of thermal runaway.

CN119019756APending Publication Date: 2024-11-26FOSHAN YUNG SHUN NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411340350.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing flame retardant and heat-insulating materials have poor flame retardant and heat-insulating effects, low compression rate and poor safety performance in battery modules, and cannot effectively buffer the expansion and stress of the battery cell, resulting in a high risk of thermal runaway spread.

Method used

Using elastic flame retardant material composed of organic elastic foam and inorganic expansion coating, two layers of inorganic expansion coatings are coated on the surface of organic elastic foam, combined with ammonium salt/amine salt as high-temperature foaming agent to form high-temperature resistance and low-temperature resistance. The heat-conducting fire-proof insulation layer buffers the expansion and stress of the battery cell and foams and expands at high temperatures to prevent heat transfer.

Benefits of technology

It achieves high compression rate, high porosity and high resilience, reduces thermal runaway spread, improves heat insulation and flame retardant performance, reduces overall density, and enhances the safety of the battery module.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019756A_ABST
    Figure CN119019756A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flame-retardant fireproof products, in particular to an elastic flame-retardant material, a preparation method thereof and a chemical power module, the elastic flame-retardant material comprises organic elastic foam and inorganic expansion coatings, and the upper surface and the lower surface of the organic elastic foam are coated with the two inorganic expansion coatings respectively; according to the volume fraction, the organic elastic foam accounts for 50%-95% of the total volume of the elastic flame-retardant material, and the two inorganic expansion coatings account for 5%-50% of the total volume of the elastic flame-retardant material; the inorganic expansion coating comprises the following components in parts by weight: 100 parts of water, 40-80 parts of phosphate, 1-20 parts of oxalate, 10-30 parts of carbonate, 1-5 parts of borate, 1-5 parts of magnesium oxide, 1-20 parts of boehmite, 0.5-5 parts of a dispersing agent and 5-10 parts of a stabilizer. The elastic flame-retardant material has flexibility, compressibility and flame retardance at the same time, the inorganic expansion coating is large in foaming space, low in density after foaming and good in foaming effect, the heat insulation effect is improved, and the technical problems that an existing flame-retardant heat insulation material is poor in flame-retardant heat insulation effect, low in compression rate and poor in safety are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant and fireproof products, and in particular to an elastic flame retardant material and a preparation method thereof, and a chemical power supply module. Background Art

[0002] Fire-retardant materials play an important role in dealing with fires. Commonly used fire-retardant materials such as fire-proof boards, fire-proof doors, fire-proof glass, and fire-retardant coatings are widely used in buildings. However, in the application of new energy batteries, the requirements for fire-retardant materials used in battery cells are higher than those for ordinary building materials. On the one hand, battery modules are often in motion. When electric vehicles are starting, changing speeds, or braking, there will be force transmission between battery modules, especially when they are subjected to unexpected external impacts and collisions, which can easily induce battery combustion accidents. The temperature of a battery fire rises very quickly, and the temperature can rise by hundreds of degrees within 1 minute, which can easily induce further combustion of adjacent cells, resulting in thermal runaway and fire and explosion. In order to avoid the entire battery pack or even the entire vehicle catching fire due to thermal runaway of a single cell, fire-proof and heat-insulating materials are usually required to be used to separate the cells to avoid the rapid spread of thermal runaway. On the other hand, since chemical power sources such as lithium batteries will expand or shrink in volume during the charge and discharge process, if adjacent battery cells are in rigid contact, extrusion stress is likely to occur, which can easily accelerate the capacity decay of the battery; for soft-pack batteries, rigid fireproof materials can also easily puncture the flexible packaging of soft-pack batteries.

[0003] Among the current battery insulation materials, aerogel products have good insulation effects, but their own strength is poor. They often need to add reinforcing fibers such as pre-oxidized silk, glass fiber, ceramic fiber, etc. to increase their strength. This results in the rigidity of aerogel insulation sheets, which are difficult to adapt to the expansion and sealing of battery cells. It is easy to generate extrusion stress between adjacent battery cells and do not have good buffering performance. In addition, in order to avoid the harm of aerogel dust to human health, aerogels need to be packaged in plastic bags. Plastic sealing not only increases the cost of aerogel use, but also fails to improve its fragile nature. The plastic bag itself will also burn at high temperatures. Although polymer silicone foam has a certain compression rate and elasticity, it is not resistant to high temperatures and has poor flame retardant effect. Flames can easily burn through silicone foam and cannot delay the heat spread of the battery. In addition, the performance of materials such as foamed silicone and aerogel will decrease with the increase of temperature. For example, glass fiber reinforced aerogel materials can only be used below 800 degrees, while foamed silicone will become hard, brittle, and even cracked when the temperature exceeds 400 degrees. The insulation effect deteriorates with the increase of temperature. Summary of the invention

[0004] In response to the problems raised by the background technology, the first purpose of the present invention is to propose an elastic flame retardant material that can simultaneously take into account flexibility, compressibility and flame retardancy, and the inorganic expansion coating has a large foaming space, low density after foaming, good foaming effect, and improved thermal insulation effect, thereby solving the technical problems of poor flame retardant and thermal insulation effect, low compressibility and poor safety performance of existing flame retardant and thermal insulation materials.

[0005] The second purpose of the present invention is to propose a method for preparing the above-mentioned elastic flame retardant material. The prepared elastic flame retardant material can simultaneously take into account flexibility, compressibility and flame retardancy, thereby solving the technical problems of poor flame retardant and thermal insulation effect, low compressibility and poor safety performance of existing flame retardant and thermal insulation materials.

[0006] The third purpose of the present invention is to propose a chemical power source module, in which elastic flame-retardant material is pasted or clamped between two adjacent lithium battery modules, which can buffer the volume expansion of the battery cell during the charging and discharging process and the stress exerted on the battery module during use, reduce thermal runaway induced by stress factors, improve the safety of the chemical power source module, and solve the technical problems of poor flame-retardant and thermal-insulating effect, low compression rate, and poor safety performance of existing flame-retardant and thermal-insulating materials in the application of chemical power source modules.

[0007] To achieve the above-mentioned purpose, the elastic flame retardant material proposed in the present invention comprises an organic elastic foam and an inorganic expansion coating, wherein the inorganic expansion coating is provided with two layers, and the two layers of the inorganic expansion coating are respectively coated on the upper and lower surfaces of the organic elastic foam; in terms of volume fraction, the organic elastic foam accounts for 50% to 95% of the total volume of the elastic flame retardant material, and the two layers of the inorganic expansion coating account for 5% to 50% of the total volume of the elastic flame retardant material; in terms of weight fraction, the inorganic expansion coating comprises the following components: 100 parts of water, 40 to 80 parts of phosphate, 1 to 20 parts of oxalate, 10 to 30 parts of carbonate, 1 to 5 parts of borate, 1 to 5 parts of magnesium oxide, 1 to 20 parts of boehmite, 0.5 to 5 parts of dispersant and 5 to 10 parts of stabilizer.

[0008] Optionally, both the phosphate and the borate are ammonium salts.

[0009] Optionally, the carbonate is an ammonium salt, and the oxalate is an ammonium salt or a compound formed by oxalic acid and an organic amine.

[0010] Optionally, the material of the organic elastic foam is selected from one or more combinations of polyurethane, polyimide, nitrile rubber, ethylene-vinyl acetate copolymer foam, chloroprene rubber foam, polyether, polyester and polyphenylene sulfide; the porosity of the organic elastic foam is 30% to 95%.

[0011] Optionally, the total thickness d of the elastic flame retardant material is set to 0.5 mm to 50 mm, wherein the thickness d1 of the organic elastic foam is set to 0.45 mm to 45 mm, and the total thickness d2 of the two layers of the inorganic expansion coating is set to 0.05 mm to 5 mm.

[0012] Optionally, the thickness d21 of a single layer of the inorganic expansion coating is ≥ 0.05 mm.

[0013] Optionally, the surface of the inorganic expansion coating is further provided with a coating layer.

[0014] The present invention also provides a method for preparing an elastic flame retardant material, which is used to prepare any of the above elastic flame retardant materials, comprising the following steps:

[0015] Step S1, preparing an inorganic intumescent coating according to the component dosage of the inorganic intumescent coating: adding the phosphate, the oxalate, the carbonate and the borate into water, stirring to dissolve part of the salt, and preparing slurry A; adding the boehmite and the magnesium oxide into the slurry A, and then respectively adding the dispersant and the stabilizer, and mixing them evenly to obtain an inorganic intumescent coating;

[0016] Step S2, one-time coating: uniformly coating the inorganic expansion coating on one surface of the organic elastic foam, drying in an oven to remove moisture, and then rolling up to prepare an intermediate coil;

[0017] Step S3, secondary coating: uniformly coating the inorganic expanding coating on the side of the intermediate coil that is not coated with the inorganic expanding coating, drying in an oven to remove moisture, and then rolling up. After drying in an oven to remove moisture, the inorganic expanding coating forms the inorganic expanding coating on the surface of the organic elastic foam to prepare the elastic flame retardant material.

[0018] Optionally, the step S3 further includes the following steps:

[0019] Step S4, coating: coating the surface of the inorganic expansion coating with a coating layer;

[0020] Step S5, die-cutting: die-cutting is performed according to the required size specifications.

[0021] The present invention also proposes a chemical power source module: the chemical power source module comprises a plurality of lithium battery modules and an elastic flame retardant material as described in any one of the above items, wherein the elastic flame retardant material is pasted or clamped between two adjacent lithium battery modules.

[0022] Compared with the prior art, the embodiments of the present invention have the following beneficial effects:

[0023] 1. Under normal use, the elastic flame retardant material exhibits high compression rate, high porosity and high resilience, which can cope with the internal and external stresses and impact forces generated or received by the battery cell during charging, discharging and movement under normal use, and reduce thermal runaway caused by force effect;

[0024] 2. When the battery core burns due to thermal runaway, the organic elastic foam disappears, while the inorganic expansion coating undergoes a foaming reaction at high temperature, and the volume expansion fills the space of the organic elastic foam, playing an organic-inorganic replacement and filling role, and forming a high-temperature resistant, low-thermal-conductivity fireproof and heat-insulating layer, which prevents heat transfer and prevents the spread of thermal runaway;

[0025] 3. The organic elastic foam will disappear at high temperatures, making the inorganic expansion coating have a larger foaming space, a lower density after foaming, and more pores, thereby improving the thermal insulation effect and flame retardant properties and avoiding the rapid spread of thermal runaway.

[0026] 4. By using ammonium salt / amine salt as a high-temperature foaming agent, the decomposition of ammonium salt / amine salt at high temperature will absorb a large amount of heat to play a cooling role. At the same time, the ammonia produced by the decomposition of ammonium salt / amine salt can inhibit free radical reactions and terminate chain combustion reactions, which can play an active fire extinguishing effect and improve the flame retardant and heat insulation effects.

[0027] 5. By using the organic elastic foam as the elastic base layer, the density of the organic elastic foam is relatively small, which reduces the overall density of the elastic flame retardant material, thus facilitating lightweight design and reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a schematic structural diagram of an elastic flame retardant material according to an embodiment of the present invention;

[0029] Figure 2 is a schematic structural diagram of an elastic flame retardant material according to another embodiment of the present invention;

[0030] Figure 3 This is a schematic diagram of the structure of an elastic flame retardant material after foaming and expansion after being heated in one embodiment of the present invention;

[0031] Figure 4 This is a real picture of Example 1 of the elastic flame retardant material of the present invention when it is burned by flame;

[0032] Figure 5 This is a real picture of Example 1 of the elastic flame retardant material of the present invention after being burned by flame;

[0033] Figure 6 This is a cross-sectional view of Example 1 of the elastic flame-retardant material of the present invention after being burned by flame and broken;

[0034] Figure 7This is a diagram showing the back temperature measurement result of Example 1 of the elastic flame retardant material of the present invention after flame burning;

[0035] Figure 8 This is a real picture of the elastic flame-retardant material of Example 1 of the present invention when it is rolled and bent;

[0036] Fig. 9 is a physical diagram of Example 2 of the elastic flame retardant material of the present invention;

[0037] Fig.10 This is a real picture of Example 2 of the elastic flame retardant material of the present invention after being bent 90°;

[0038] Fig.11 This is a real picture of Example 2 of the elastic flame retardant material of the present invention after being burned by flame;

[0039] Fig.12 This is a diagram showing the back temperature measurement result of Example 3 of the elastic flame retardant material of the present invention after flame burning;

[0040] Fig.13 This is a real picture of the comparative example 1 of the elastic flame retardant material of the present invention after being burned by flame;

[0041] Fig.14 This is a graph showing the back temperature measurement results of comparative example 1 of the elastic flame retardant material of the present invention after flame burning;

[0042] Fig.15 This is a graph showing the back temperature measurement results of comparative example 2 of the elastic flame retardant material of the present invention after flame burning;

[0043] Fig.16 This is a real picture of the comparative example 3 of the elastic flame retardant material of the present invention after being burned by flame;

[0044] Fig.17 This is a graph showing the back temperature measurement results of comparative example 3 of the elastic flame retardant material of the present invention after flame burning;

[0045] Fig.18 This is a real picture of the commercially available pre-oxidized silk aerogel sample of Comparative Example 4 being burned by a butane torch flame;

[0046] Fig.19 The present invention is a flow chart of the preparation process of the elastic flame retardant material. DETAILED DESCRIPTION

[0047] In order to facilitate the understanding of the present invention, the present invention is described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0048] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0049] See also Figure 1 The present invention proposes an elastic flame retardant material, comprising an organic elastic foam 1 and an inorganic expansion coating 2, wherein the inorganic expansion coating 2 is provided with two layers, and the two layers of the inorganic expansion coating 2 are respectively coated on the upper and lower surfaces of the organic elastic foam 1; in terms of volume fraction, the organic elastic foam 1 accounts for 50% to 95% of the total volume of the elastic flame retardant material, and the two layers of the inorganic expansion coating 2 account for 5% to 50% of the total volume of the elastic flame retardant material; in terms of weight fraction, the inorganic expansion coating 2 comprises the following components: 100 parts of water, 40 to 80 parts of phosphate, 1 to 20 parts of oxalate, 10 to 30 parts of carbonate, 1 to 5 parts of borate, 1 to 5 parts of magnesium oxide, 1 to 20 parts of boehmite, 0.5 to 5 parts of dispersant and 5 to 10 parts of stabilizer.

[0050] The present invention arranges two layers of the inorganic expansion coating 2 and coats them on the upper and lower surfaces of the organic elastic foam 1 respectively. The organic elastic foam 1 acts as a buffer matrix material. The inorganic expansion coating 2 sandwiches the organic elastic foam 1 with poor heat resistance therebetween to play a protective role, so that the elastic flame retardant material can simultaneously take into account flexibility, compressibility and flame retardancy. Under normal use, the elastic flame retardant material exhibits the properties of the organic elastic foam 1, that is, it has high compression rate, high porosity and high resilience to cope with the internal and external stresses and impact forces generated or received by the battery cell during charging, discharging and movement under normal use; when the battery cell burns due to thermal runaway, the temperature rises rapidly to hundreds of degrees or even thousands of degrees, wherein the organic elastic foam 1 will soften, melt, decompose and degrade, while the inorganic expansion coating 2 undergoes a foaming reaction at high temperature, and the volume expansion fills the space of the organic elastic foam 1, playing an organic-inorganic replacement and filling role, so that the elastic flame retardant material can achieve the transition from the organic foam state to the inorganic foam state while maintaining the original structure unchanged, and form a high temperature resistant, low thermal conductivity fireproof and heat-insulating layer, which has the effect of preventing heat transfer and preventing the spread of thermal runaway, and solves the technical problems of poor flame retardant and heat-insulating effect, low compression rate and poor safety performance of existing flame retardant and heat-insulating materials.

[0051] It is further explained that the carbonate and the oxalate act as high-temperature foaming agents to achieve foaming, expansion and heat insulation; the boehmite and the magnesium oxide act to resist high temperatures and provide heat insulation; the phosphate decomposes under heat to produce phosphorus pentoxide, which is a gas flame retardant and can react with combustion products in combustibles to form a protective film on the surface, isolating oxygen from the combustibles, thereby preventing the flame from further spreading and playing a flame retardant role; the borate decomposes under heat to produce boron oxide glass, which has a low melting point and is a viscous liquid at high temperatures, and forms a low-melting-point viscous glass together with the phosphate. The phosphate and the borate can play a high-temperature bonding role, so that the two layers of the inorganic expansion coating 2 form a coupled whole after foaming and expansion, thereby improving the flame retardant and heat insulation effect; by adding a high content of the phosphate, the expansion reaction of the inorganic expansion coating 2 can be catalyzed at high temperatures, the expansion ratio can be increased, and the structural stability of the inorganic expansion coating 2 during the high-temperature expansion process can be maintained, thereby preventing the expansion layer from rupturing or falling off prematurely, thereby preventing the transfer of flame and heat.

[0052] It is further explained that the disappearance of the organic elastic foam 1 at high temperature can make the foaming space of the inorganic expansion coating 2 larger and the density after foaming lower, effectively improving the foaming effect of the inorganic expansion coating 2, thereby improving the thermal insulation effect and flame retardant performance, avoiding the rapid spread of thermal runaway, and significantly improving the final fire resistance temperature and thermal insulation effect of the elastic flame retardant material.

[0053] Since the organic elastic foam 1 has a relatively low density, the overall density of the elastic flame retardant material can be reduced, which is helpful for lightweight design.

[0054] Specifically, optionally, the dispersant is one of sodium tripolyphosphate, polyethylene glycol or sodium tartrate, and the stabilizer is acrylic emulsion or sodium carboxymethyl cellulose solution.

[0055] To further illustrate, both the phosphate and the borate are ammonium salts.

[0056] When ammonium phosphate is decomposed by heat, it will produce phosphorus pentoxide and ammonia. Usually, phosphorus pentoxide is a gas flame retardant, which can react with the combustion products in the combustibles to form phosphates, forming a protective film on the surface to prevent the flame from spreading further. When ammonium borate is decomposed by heat, it will produce boron oxide glass and ammonia. Boron oxide has a low melting point and is a viscous liquid at high temperatures. Together with phosphates, it forms a low-melting viscous glass and becomes a high-temperature adhesive. By setting the phosphate and the borate as ammonium salts, after the organic elastic foam 1 disappears at high temperature, due to the formation of the high-temperature adhesive, the two layers of the inorganic expansion coating 2 can be foamed and expanded to form a coupled whole, thereby improving the flame retardant and heat insulation effect.

[0057] To further illustrate, the carbonate is an ammonium salt, and the oxalate is an ammonium salt or a compound formed by oxalic acid and an organic amine.

[0058] The carbonate is an ammonium salt, and the oxalate is a compound formed by an ammonium salt or oxalic acid and an organic amine. That is, ammonium salt / amine salt is used as a high-temperature foaming agent. The ammonium salt / amine salt decomposes at high temperature and absorbs a large amount of heat to cool the temperature. At the same time, the ammonia gas produced by the decomposition of the ammonium salt / amine salt can inhibit free radical reactions and terminate chain combustion reactions, thereby achieving an active fire extinguishing effect and improving the flame retardant and heat insulating effects.

[0059] To further illustrate, the material of the organic elastic foam 1 is selected from one or more combinations of polyurethane, polyimide, nitrile rubber, ethylene-vinyl acetate copolymer foam, chloroprene rubber foam, polyether, polyester and polyphenylene sulfide; the porosity of the organic elastic foam 1 is 30% to 95%.

[0060] The porosity of the organic elastic foam 1 is 30% to 95%, which can take into account both flexibility and compressibility, and has a low density and light weight, which helps to achieve lightweight.

[0061] To further illustrate, the total thickness d of the elastic flame retardant material is set to 0.5 mm to 50 mm, wherein the thickness d1 of the organic elastic foam 1 is set to 0.45 mm to 45 mm, and the total thickness d2 of the two layers of the inorganic expansion coating 2 is set to 0.05 mm to 5 mm.

[0062] By setting the total thickness d of the elastic flame retardant material to 0.5 mm to 50 mm, wherein the thickness d1 of the organic elastic foam 1 is 0.45 mm to 45 mm, the requirements on the compression rate and resilience of the elastic flame retardant material can be met.

[0063] For further explanation, see Figure 1 , Figure 3 The thickness of the two layers of the inorganic expansion coating 2 after thermal expansion is greater than the thickness of the organic elastic foam 1, and the space of the organic elastic foam 1 can be effectively utilized for the foaming and expansion of the inorganic expansion coating 2, so that the foaming and expansion space of the inorganic expansion coating 2 is larger and the density after foaming is lower, thereby improving the heat insulation effect and flame retardant performance.

[0064] To further illustrate, the thickness d21 of a single layer of the inorganic expansion coating 2 is ≥ 0.05 mm.

[0065] By setting the thickness d21 of a single layer of the inorganic expansion coating 2 to be ≥ 0.05 mm, the difficulty of coating a single layer of the inorganic expansion coating 2 can be reduced.

[0066] Specifically, optionally, the two layers of the inorganic expansion coating 2 have the same thickness, so that the flame retardant and heat insulating capabilities of the two surfaces of the elastic flame retardant material are relatively even.

[0067] See also Figure 2 , further explained, the surface of the inorganic expansion coating 2 is also provided with a coating layer 3.

[0068] By providing the coating layer 3, it is possible to prevent the elastic flame retardant material from being damaged by the external environment, thereby extending the service life of the elastic flame retardant material.

[0069] Specifically, optionally, the coating layer 3 is a double-sided tape, which is sticky and can firmly adhere the elastic flame retardant material to a designated position of the battery system, eliminating additional fixings or installation steps, simplifying the installation process, and improving installation efficiency. At the same time, it can prevent the elastic flame retardant material from loosening or falling off under vibration or impact.

[0070] Specifically, optionally, the coating layer 3 is a plastic protective film, which can provide a physical barrier for the elastic flame retardant material to prevent erosion by external factors such as dust, moisture, and chemicals. The plastic protective film has good chemical corrosion resistance and is easy to clean.

[0071] See also Fig.19 The present invention also provides a method for preparing an elastic flame retardant material, which is used to prepare any of the above elastic flame retardant materials, comprising the following steps:

[0072] Step S1, preparing an inorganic intumescent coating according to the component dosage of the inorganic intumescent coating 2: adding the phosphate, the oxalate, the carbonate and the borate into water, stirring to dissolve part of the salt, and preparing slurry A; adding the boehmite and the magnesium oxide into the slurry A, and then respectively adding the dispersant and the stabilizer, and mixing them evenly to obtain an inorganic intumescent coating;

[0073] Step S2, one-time coating: uniformly coating the inorganic expansion coating on one surface of the organic elastic foam 1, drying in an oven to remove moisture, and then rolling up to prepare an intermediate coil;

[0074] Step S3, secondary coating: the inorganic expanding coating is evenly coated on the side of the intermediate coil that is not coated with the inorganic expanding coating, and the coil is rolled up after being dried in an oven to remove moisture. After the inorganic expanding coating is dried in an oven to remove moisture, the inorganic expanding coating forms the inorganic expanding coating 2 on the surface of the organic elastic foam 1 to prepare the elastic flame retardant material.

[0075] The elastic flame-retardant material prepared by the present invention uses the organic elastic foam 1 as a buffer matrix material, and the inorganic expansion coating 2 sandwiches the organic elastic foam 1 with poor heat resistance to play a protective role, so that the elastic flame-retardant material can take into account flexibility, compressibility and flame retardancy at the same time, and can buffer the volume expansion of the battery cell during the charging and discharging process and the stress of the battery module during use, reduce thermal runaway induced by stress factors, improve the safety of the battery, and solve the technical problems of low compression rate, poor buffering effect, and poor flame retardant and heat-insulating effect of existing flame-retardant and heat-insulating materials.

[0076] The inorganic expansion coating of the present invention uses water as a solvent, is environmentally friendly and non-toxic, and helps to reduce environmental pollution.

[0077] To further illustrate, the step S3 further includes the following steps:

[0078] Step S4, coating: coating the surface of the inorganic expansion coating with a coating layer 3;

[0079] Step S5, die-cutting: die-cutting is performed according to the required size specifications.

[0080] By coating both sides of the elastic flame retardant material prepared in step S4 with a coating layer 3, it is possible to prevent the elastic flame retardant material from being damaged by the external environment and extend the service life of the elastic flame retardant material. Specifically, the coating layer 3 is a double-sided adhesive or a plastic protective film;

[0081] The elastic flame retardant material of different specifications and sizes can be prepared by die-cutting to meet the installation requirements between battery packs or battery cells of different specifications and sizes.

[0082] The present invention further provides a chemical power source module, which includes a plurality of lithium battery modules and an elastic flame retardant material as described in any one of the above items, wherein the elastic flame retardant material is pasted or clamped between two adjacent lithium battery modules.

[0083] Specifically, the elastic flame retardant material can be applied in the form of a coil or sheet. The elastic flame retardant material has good elasticity and flexibility. By pasting or clamping the elastic flame retardant material between two adjacent lithium battery modules, the volume expansion of the battery cell during the charging and discharging process and the stress of the battery module during use can be buffered, reducing thermal runaway induced by stress factors and improving the safety of the chemical power source module.

[0084] In extreme cases, such as when a single battery cell burns due to thermal runaway, the organic elastic foam 1 will soften, melt, decompose, and degrade, while the inorganic expansion coating 2 will undergo a foaming reaction at high temperature, and the volume expansion will fill the space of the organic elastic foam 1, forming a high temperature resistant, low thermal conductivity fireproof and heat insulating layer, which has the effect of preventing heat transfer and preventing the spread of thermal runaway. Since the disappearance of the organic elastic foam 1 provides a certain foaming space for the inorganic expansion coating 2, the extrusion of the inorganic expansion coating 2 on the adjacent battery cells after foaming and expansion is reduced, so that the inorganic expansion coating 2 has a larger foaming space, a lower density after foaming, and a better foaming effect, thereby improving the thermal insulation effect and flame retardant performance, avoiding the rapid spread of thermal runaway, and improving the safety of the chemical power module.

[0085] (I) Embodiment:

[0086] (1) Example 1: An elastic flame retardant material, comprising an organic elastic foam 1 and an inorganic expansion coating 2, wherein the organic elastic foam 1 is an ethylene-vinyl acetate copolymer foam (porosity is 80%, compression rate is 60%), and the inorganic expansion coating 2 is provided with two layers, and the two layers of the inorganic expansion coating 2 are respectively coated on the upper and lower surfaces of the organic elastic foam 1; in terms of volume fraction, the organic elastic foam 1 accounts for 83.33%, and the two layers of the inorganic expansion coating 2 account for 16.67%; the total thickness of the elastic flame retardant material is designed to be d=3 mm, the thickness of the organic elastic foam 1 is d1=2.5mm, the thickness of the two layers of the inorganic expansion coating 2 is d2=0.5mm, and the thickness of the single layer of the inorganic expansion coating 2 is d21=0.25mm; the inorganic expansion coating 2 comprises the following components: 100 parts of water, 60 parts of phosphate (ammonium polyphosphate), 15 parts of oxalate (ammonium oxalate), 3 parts of borate (ammonium borate), 20 parts of carbonate (ammonium bicarbonate), 5 parts of magnesium oxide, 15 parts of boehmite, 1 part of dispersant (sodium tripolyphosphate), and 10 parts of stabilizer (acrylic emulsion).

[0087] The preparation method of Example 1 is:

[0088] Step S1, preparing an inorganic expansion coating according to the component dosage of the inorganic expansion coating 2: adding 60 parts of ammonium polyphosphate, 15 parts of ammonium oxalate, 3 parts of ammonium borate, and 20 parts of ammonium bicarbonate to 100 parts of water, stirring for 1 hour to dissolve part of the salt, and preparing slurry A; adding 15 parts of boehmite and 5 parts of magnesium oxide to the slurry A, and then adding 1 part of a dispersant (sodium tripolyphosphate) respectively, stirring for 10 minutes, and finally adding 10 parts of a stabilizer (acrylic emulsion), stirring and transferring to a ball mill, ball milling at a speed of 120 rpm for 2 hours to mix evenly, to obtain the inorganic expansion coating;

[0089] Step S2, one-time coating: feeding the organic elastic foam 1 into a coating machine, uniformly coating the inorganic expansion coating prepared in step S1 on one surface of the organic elastic foam 1, adjusting the gap of the scraper to control the coating thickness of the inorganic expansion coating, drying in an oven to remove moisture and then rolling up to prepare an intermediate coil;

[0090] Step S3, secondary coating: the intermediate coil prepared in step S2 is fed into the coating machine again, with the side of the intermediate coil not coated with the inorganic expansion coating facing upward, and the inorganic expansion coating prepared in step S1 is uniformly coated on the surface of the organic elastic foam 1 again, and the gap of the scraper is adjusted to control the coating thickness of the inorganic expansion coating. After being dried in an oven to remove moisture, the coil is rolled up. After being dried in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating 2 on the surface of the organic elastic foam 1 to prepare the elastic flame retardant material.

[0091] (2) Example 2: An elastic flame retardant material, comprising an organic elastic foam 1 and an inorganic expansion coating 2, wherein the organic elastic foam 1 is a polyurethane foam coil (porosity is 90%, compression rate is 75%), and the inorganic expansion coating 2 is provided with two layers, and the two layers of the inorganic expansion coating 2 are respectively coated on the upper and lower surfaces of the organic elastic foam 1; in terms of volume fraction, the organic elastic foam 1 accounts for 83.33%, and the two layers of the inorganic expansion coating 2 account for 16.67%; the total thickness of the elastic flame retardant material is designed to be d=2.4 m m, the thickness of the organic elastic foam 1 is d1=2mm, the thickness of the two layers of the inorganic expansion coating 2 is d2=0.4mm, and the thickness of the single layer of the inorganic expansion coating 2 is d21=0.2mm; the inorganic expansion coating 2 includes the following components: 100 parts of water, 50 parts of phosphate (ammonium polyphosphate), 10 parts of oxalate (ammonium oxalate), 10 parts of carbonate (ammonium bicarbonate), 5 parts of borate (ammonium borate), 5 parts of magnesium oxide, 15 parts of boehmite, 0.5 parts of dispersant (sodium tripolyphosphate), and 8 parts of stabilizer (acrylic emulsion). The surface of the elastic flame retardant material is also covered with a coating layer 3, and the coating layer 3 is a double-sided adhesive layer.

[0092] The preparation method of Example 2 is:

[0093] Step S1, preparing an inorganic expansion coating according to the component dosage of the inorganic expansion coating 2: adding 50 parts of ammonium polyphosphate, 10 parts of ammonium oxalate, 10 parts of ammonium bicarbonate and 5 parts of ammonium borate to 100 parts of water, stirring for 1 hour to dissolve part of the salt, and preparing slurry A; adding 15 parts of boehmite and 5 parts of magnesium oxide to the slurry A, and then adding 0.5 parts of dispersant (sodium tripolyphosphate) respectively, stirring for 10 minutes, and finally adding 8 parts of stabilizer (acrylic emulsion), stirring and transferring to a ball mill, ball milling at a speed of 120 rpm for 2 hours to mix evenly, to obtain the inorganic expansion coating;

[0094] Step S2, one-time coating: feeding the organic elastic foam 1 into a coating machine, uniformly coating the inorganic expansion coating prepared in step S1 on one surface of the organic elastic foam 1, adjusting the gap of the scraper to control the coating thickness of the inorganic expansion coating, drying in an oven to remove moisture and then rolling up to prepare an intermediate coil;

[0095] Step S3, secondary coating: the intermediate coil prepared in step S2 is fed into the coating machine again, with the side of the intermediate coil not coated with the inorganic expansion coating facing upward, and the inorganic expansion coating prepared in step S1 is uniformly coated on the surface of the organic elastic foam 1 again, and the gap of the scraper is adjusted to control the coating thickness of the inorganic expansion coating, and the coil is rolled up after being dried in an oven to remove moisture. After the inorganic expansion coating is dried in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating 2 on the surface of the organic elastic foam 1, thereby preparing the elastic flame retardant material;

[0096] Step S4, coating: using a coating machine, coating the surface of the inorganic expansion coating of the elastic flame retardant material prepared in step S3 with a coating layer 3, wherein the coating layer 3 is a double-sided adhesive layer;

[0097] Step S5, die-cutting: Die-cutting is performed according to the required size specification (200 mm*170 mm).

[0098] (3) Example 3: An elastic flame retardant material, comprising an organic elastic foam 1 and an inorganic expansion coating 2, wherein the organic elastic foam 1 is a chloroprene rubber foam (porosity is 50%, compression rate is 40%), and the inorganic expansion coating 2 is provided with two layers, and the two layers of the inorganic expansion coating 2 are respectively coated on the upper and lower surfaces of the organic elastic foam 1; in terms of volume fraction, the organic elastic foam 1 accounts for 86.21%, and the two layers of the inorganic expansion coating 2 account for 13.79%; the total thickness of the elastic flame retardant material is designed to be d=2.9 mm, and the organic elastic foam 1 is 0.1 mm thick. The thickness d1 of the organic elastic foam 1 is 2.5 mm, the thickness d2 of the two layers of the inorganic expansion coating 2 is 0.4 mm, and the thickness d21 of the single layer of the inorganic expansion coating 2 is 0.2 mm; the inorganic expansion coating 2 comprises the following components: 100 parts of water, 60 parts of phosphate (ammonium polyphosphate), 15 parts of oxalate (oxalamide), 2 parts of borate (ammonium borate), 20 parts of carbonate (ammonium bicarbonate), 5 parts of magnesium oxide, 15 parts of boehmite, 1 part of dispersant (polyethylene glycol PEG-10000), and 10 parts of stabilizer (acrylic emulsion).

[0099] The preparation method of Example 3 is:

[0100] Step S1, preparing an inorganic expansion coating according to the component dosage of the inorganic expansion coating 2: adding 60 parts of ammonium polyphosphate, 15 parts of oxalamide, 2 parts of ammonium borate, and 20 parts of ammonium bicarbonate to 100 parts of water, stirring for 1 hour to dissolve part of the salt, and preparing slurry A; adding 15 parts of boehmite and 5 parts of magnesium oxide to the slurry A, and then adding 1 part of a dispersant (polyethylene glycol PEG-10000) respectively, stirring for 10 minutes, and finally adding 10 parts of a stabilizer (acrylic emulsion), stirring and transferring to a ball mill, ball milling at a speed of 120 rpm for 2 hours to mix evenly, to obtain the inorganic expansion coating;

[0101] Step S2, one-time coating: feeding the organic elastic foam 1 into a coating machine, uniformly coating the inorganic expansion coating prepared in step S1 on the upper surface of the organic elastic foam 1, adjusting the gap of the scraper to control the coating thickness of the inorganic expansion coating, drying in an oven to remove moisture and then rolling up to prepare an intermediate coil;

[0102] Step S3, secondary coating: the intermediate coil prepared in step S2 is fed into the coating machine again, with the side of the intermediate coil not coated with the inorganic expansion coating facing upward, and the inorganic expansion coating prepared in step S1 is uniformly coated on the surface of the organic elastic foam 1 again, and the gap of the scraper is adjusted to control the coating thickness of the inorganic expansion coating. After being dried in an oven to remove moisture, the coil is rolled up. After being dried in an oven to remove moisture, the inorganic expansion coating forms the inorganic expansion coating 2 on the surface of the organic elastic foam 1 to prepare the elastic flame retardant material.

[0103] (4) The difference between Examples 4 to 7 and Example 1 is that the volume ratio of the organic elastic foam 1 and the inorganic expansion coating 2 in Examples 4 to 7, as well as the thickness of the elastic flame retardant material are designed according to the data in Table 1:

[0104] Table 1 Volume ratio and thickness design of organic elastic foam and inorganic expansion coating

[0105]

[0106] (5) The difference between Examples 8 and 9 and Example 1 is that the component contents of the inorganic expansion coating 2 in Examples 8 and 9 are different. The component contents of the inorganic expansion coating 2 are as shown in Table 2:

[0107] Table 2 Component contents of inorganic expansion coating (unit: in parts by weight)

[0108]

[0109]

[0110] (II) Comparative Example:

[0111] (1) Comparative Examples 1 to 3 differ from Example 1 in that the components and contents of the inorganic expansion coating 2 are different. The components and contents of the inorganic expansion coating 2 are as shown in Table 3 (where “-” indicates that the component is not added):

[0112] Table 3 Components and contents of inorganic expansion coating (unit: in parts by weight)

[0113]

[0114] The difference between the preparation methods of Comparative Examples 1 to 3 and the preparation method of Example 1 lies in step S1, and the remaining steps are the same as those of the preparation method of Example 1:

[0115] Step S1, preparing the inorganic intumescent coating according to the component dosage of the inorganic intumescent coating 2 in Table 1, and the remaining steps are the same as the preparation method of Example 1.

[0116] (2) Comparative Example 4: a commercially available pre-oxidized silk aerogel sample.

[0117] (III) Performance test and result analysis:

[0118] The elastic flame retardant materials prepared in Examples 1 to 9, Comparative Examples 1 to 3, and the pre-oxidized silk aerogel samples of Comparative Example 4 were cut into 10 cm×10 cm samples, and then performance tests were performed. The experimental methods and results are analyzed as follows:

[0119] (1) Flexibility test: When a force of 1 kg is applied to the elastic flame retardant material, the thickness change of the elastic flame retardant material is observed and measured, and the time for the elastic flame retardant material to return to its original thickness after the external force is removed is recorded.

[0120] Result analysis: Flexibility results are shown in Table 4:

[0121] Table 4 Flexibility results

[0122]

[0123] The actual picture of the elastic flame retardant material prepared in Example 1 is shown in Figure 8 The elastic flame retardant material can be rolled and bent, showing good flexibility. Under the action of an external force of 1 kg, the thickness of the elastic flame retardant material can be compressed from 3 mm to 2.5 mm, and after the external force is removed, it recovers to the original thickness within 30 seconds, showing good room temperature elasticity and flexibility. The elastic flame retardant materials prepared in Examples 8 to 9 and Comparative Examples 1 to 3 also show good room temperature elasticity and flexibility.

[0124] Please refer to the actual picture of the elastic flame retardant material prepared in Example 2 Figures 9 and 10 The elastic flame retardant material can be bent into 90 degrees under the action of an external force and has excellent flexibility.

[0125] From the flexibility test results, it can be seen that the elastic flame retardant material prepared in Examples 3-7 also exhibits good compression resilience and flexibility. As the thickness of the organic elastic foam 1 increases, the ability to resist deformation due to external forces is also enhanced accordingly.

[0126] (2) Flame burning test: The elastic flame retardant materials prepared in Examples 1 to 9 and Comparative Examples 1 to 3, and the commercially available pre-oxidized silk aerogel sample of Comparative Example 4 were directly sprayed with a butane spray gun flame (the elastic flame retardant material prepared in Example 2 was sprayed with a butane spray gun flame after removing the release paper on the surface of the double-sided adhesive tape). The spraying was continued for 10 minutes, and the back temperature was monitored with a thermocouple. Three K-type thermocouples were attached to the elastic flame retardant material for temperature measurement, and the temperature change was measured in real time.

[0127] Result analysis: The test results of the back temperature of the sample are recorded in Table 5:

[0128] Table 5 Test results of back surface temperature of samples

[0129] Sample Maximum backside temperature (unit: ℃) Example 1 180 Example 2 210 Example 3 230 Example 4 290 Example 5 45 Example 6 56 Example 7 85 Example 8 250 Example 9 230 Comparative Example 1 530 Comparative Example 2 450 Comparative Example 3 430 Comparative Example 4 480

[0130] See also Figures 4 to 18 As well as the results of Table 3 above, the analysis is as follows:

[0131] The elastic flame retardant material prepared in Example 1 can be found in Figures 4 to 6 In the absence of a protective film, it can be clearly seen that the inorganic expansion coating 2 on the surface of the elastic flame retardant material undergoes significant volume expansion when the flame burns, and the part of the elastic flame retardant material that is in direct contact with the flame after the flame burns has an obvious expansion bulge; after breaking the elastic flame retardant material after burning, please refer to Figure 6 It can be seen that the original organic elastic foam 1 has completely disappeared, and the expanded inorganic expansion coating 2 not only occupies the original space (2.5mm) of the organic elastic foam 1, but also has a larger volume and a thickness of 8 to 10mm. After burning with a butane torch flame for 10 minutes, please refer to Figure 7 The maximum back surface temperature of the elastic flame retardant material is only 180° C., which indicates that the elastic flame retardant material prepared by the present invention has good fire retardant properties.

[0132] The elastic flame retardant material prepared in Example 2 can be found in Fig.11 It can be seen that obvious foaming occurred in the flame-sprayed part, while the entire elastic flame-retardant material sample maintained its original shape, did not collapse due to the disappearance of the organic elastic foam 1, and was not burned through; after continuous burning with a butane spray gun flame for 10 minutes, the back temperature reached a maximum of 210°C, which has good fire-retardant properties.

[0133] The elastic flame retardant material prepared in Example 3 can be found in Fig.12 After burning with a butane spray gun flame for 10 minutes, the maximum temperature on the back is 230°C, which has good fire retardant properties.

[0134] The elastic flame retardant material prepared in Example 4-9 has a maximum back surface temperature of 45°C to 290°C after being burned by a butane spray gun flame for 10 minutes, and also has good fire retardant properties. The thicker the elastic flame retardant material, the better its flame retardant and heat insulating effect.

[0135] The elastic flame retardant material prepared in Comparative Example 1 can be found in Fig.13 , it will expand under high temperature flame burning, but its high temperature resistance and heat insulation performance are very poor. After 3 minutes of burning with a butane spray gun, it has already shown signs of burning through; a thermocouple is used to monitor the back temperature, please refer to Fig.14 , the temperature of the back of the elastic flame retardant material can reach up to 530° C. It can be seen that the inorganic intumescent coating can still expand at high temperatures without boehmite and magnesium oxide, but due to the lack of high temperature resistant boehmite and magnesium oxide, the heat resistance and heat insulation are poor and cannot prevent high temperature flames.

[0136] The elastic flame retardant material prepared in Example 2 has a significantly reduced expansion thickness after flame burning, which is only 2-3 mm. The back temperature is monitored by a thermocouple. Fig.15 , the back temperature can reach up to 450°C, and the thermal insulation performance is poor. It can be seen that since ammonium carbonate and ammonium oxalate are used as high-temperature foaming agents, they will decompose into water vapor, carbon dioxide and ammonia during the heating process, and have a foaming and expansion effect. When the inorganic expansion coating 2 lacks ammonium carbonate and ammonium oxalate in its components, the inorganic expansion coating 2 has a poor foaming effect when heated, resulting in an insufficient thickness of the foaming expansion layer, a high density, and a poor thermal insulation effect.

[0137] The elastic flame retardant material prepared in Comparative Example 3 can be found in Fig.16 After the flame is burned, it can expand, but the thickness of the expansion is small, only 5-6mm, and the expansion layer is discontinuous, and there is a partial separation between the expansion layers on the front and back. Use a thermocouple to monitor the back temperature, please refer to the attached Fig.17 , the back temperature can reach up to 430°C, and the thermal insulation performance is poor. Since ammonium phosphate salts will produce phosphorus pentoxide and ammonia when they are thermally decomposed, phosphorus pentoxide is usually a gas flame retardant, which can react with the combustion products in combustibles to form phosphates, forming a protective film on the surface to prevent the flame from spreading further; ammonium borate salts will produce boron oxide glass and ammonia when they are thermally decomposed. Boron oxide has a low melting point and is a viscous liquid at high temperatures. Together with phosphates, it forms a low-melting-point viscous glass and becomes a high-temperature adhesive. It can be seen that due to the reduction in the content of ammonium phosphate salts and ammonium borate salts, the expansion ratio of the inorganic expansion coating is reduced, and the inorganic expansion coating 2 produces less glass liquid when it is thermally decomposed. After the organic elastic foam 1 in the middle disappears due to heat, the two layers of the inorganic expansion coating 2 are separated from each other and do not form a coupled whole, resulting in insufficient expansion thickness and poor thermal insulation effect.

[0138] For the pre-oxidized silk aerogel sample of Comparative Example 4, please refer to Fig.18 After only 1 minute of burning, the pre-oxidized silk aerogel sample had obviously bent and deformed, and peeling occurred within the layer, losing its integrity. After continuing to burn for 2 minutes, the double-sided adhesive layer on the back of the pre-oxidized silk aerogel sample had turned black and partially carbonized, and the measured back temperature reached 480°C, indicating that its high temperature resistance and flame retardant and heat insulation effects were poor.

[0139] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. An elastic flame retardant material, characterized in that: It comprises an organic elastic foam and an inorganic expansion coating, wherein the inorganic expansion coating is provided with two layers, and the two layers of the inorganic expansion coating are respectively coated on the upper and lower surfaces of the organic elastic foam; in terms of volume fraction, the organic elastic foam accounts for 50% to 95% of the total volume of the elastic flame retardant material, and the two layers of the inorganic expansion coating account for 5% to 50% of the total volume of the elastic flame retardant material; The inorganic expansion coating comprises the following components by weight: 100 parts of water, 40 to 80 parts of phosphate, 1 to 20 parts of oxalate, 10 to 30 parts of carbonate, 1 to 5 parts of borate, 1 to 5 parts of magnesium oxide, 1 to 20 parts of boehmite, 0.5 to 5 parts of dispersant and 5 to 10 parts of stabilizer.

2. The elastic flame retardant material according to claim 1, characterized in that: The phosphate and the borate are both ammonium salts.

3. The elastic flame retardant material according to claim 1, characterized in that: The carbonate is an ammonium salt, and the oxalate is an ammonium salt or a compound formed by oxalic acid and an organic amine.

4. The elastic flame retardant material according to claim 1, characterized in that: The material of the organic elastic foam is selected from one or more combinations of polyurethane, polyimide, nitrile rubber, ethylene-vinyl acetate copolymer foam, chloroprene rubber foam, polyether, polyester and polyphenylene sulfide; the porosity of the organic elastic foam is 30% to 95%.

5. The elastic flame retardant material according to claim 1, characterized in that: The total thickness d of the elastic flame retardant material is set to 0.5 mm to 50 mm, wherein the thickness d1 of the organic elastic foam is set to 0.45 mm to 45 mm, and the total thickness d2 of the two layers of the inorganic expansion coating is set to 0.05 mm to 5 mm.

6. The elastic flame retardant material according to claim 5, characterized in that: The thickness d21 of a single layer of the inorganic expansion coating is ≥0.05 mm.

7. The elastic flame retardant material according to claim 1, characterized in that: The surface of the inorganic expansion coating is also provided with a coating layer.

8. A method for preparing an elastic flame retardant material, for preparing the elastic flame retardant material according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step S1, preparing an inorganic intumescent coating according to the component dosage of the inorganic intumescent coating: adding the phosphate, the oxalate, the carbonate and the borate into water, stirring to dissolve part of the salt, and preparing slurry A; Adding the boehmite and the magnesium oxide to the slurry A, and then respectively adding the dispersant and the stabilizer, and mixing them evenly to obtain an inorganic intumescent coating; Step S2, one-time coating: uniformly coating the inorganic expansion coating on one surface of the organic elastic foam, drying in an oven to remove moisture, and then rolling up to prepare an intermediate coil; Step S3, secondary coating: uniformly coating the inorganic expanding coating on the side of the intermediate coil that is not coated with the inorganic expanding coating, drying in an oven to remove moisture, and then rolling up. After drying in an oven to remove moisture, the inorganic expanding coating forms the inorganic expanding coating on the surface of the organic elastic foam to prepare the elastic flame retardant material.

9. The method for preparing the elastic flame retardant material according to claim 8, characterized in that: The step S3 further includes the following steps: Step S4, coating: coating the surface of the inorganic expansion coating with a coating layer; Step S5, die-cutting: die-cutting is performed according to the required size specifications.

10. A chemical power source module, characterized in that: The chemical power source module comprises a plurality of lithium battery modules and the elastic flame retardant material as claimed in any one of claims 1 to 7, wherein the elastic flame retardant material is pasted or clamped between two adjacent lithium battery modules.