Carbon nanotube modified silicone rubber, preparation method and application of carbon nanotube modified silicone rubber in polycarbonate material
Through the combination of carbon nanotube modified silicone rubber and polycarbonate materials, the problem of taking into account both toughness and flame retardant properties of polycarbonate materials is solved, and crack resistance and flame retardant properties are improved, which is suitable for electronic and electrical appliance fields.
Patent Information
- Application Number
- CN202410897192.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult for polycarbonate materials to take into account both toughness and flame retardant properties. Especially in applications in the field of electronic and electrical appliances, traditional modification methods have problems with environmental protection and insufficient flame retardant properties.
Using carbon nanotube modified silicone rubber, silicone rubber with surface grafted carbon nanotubes was prepared by reacting silicone rubber with aminosilane coupling agent and acidified carbon nanotubes under ultrasonic conditions, and the silicone rubber with polycarbonate material was prepared. Combined, it improves the crack resistance and flame retardant properties of the material, and at the same time adds fluorescent agent to improve the brightness and whiteness of the material.
It significantly improves the crack resistance, flame retardant properties and mechanical properties of the material, and has excellent chemical resistance and light stability, and is suitable for high-demand electronics and electrical fields.
Smart Images

Figure BDA0004929342240000091 
Figure BDA0004929342240000101 
Figure BDA0004929342240000102
Abstract
Description
Technical Field
[0001] The invention belongs to the field of plastics, and specifically relates to a carbon nanotube modified silicone rubber and a preparation method thereof, and a crack-resistant flame-retardant polycarbonate material prepared therefrom and a preparation method thereof. Background Art
[0002] Polycarbonate (PC) is a high molecular polymer containing carbonate groups in the molecular chain. It is one of the five major engineering plastics. It has the advantages of being colorless, transparent, heat-resistant, impact-resistant, and UL 94 V-2. However, it has high notch sensitivity and is prone to stress cracking among similar products. In addition, the dripping liquid during burning can easily cause nearby materials to catch fire, making it difficult to meet the higher requirements of special fields. Therefore, PC materials are usually modified in fields with flame retardant requirements.
[0003] In the field of electronic appliances, flame-retardant polycarbonate materials have been widely used, such as instruments, meters, high and low voltage switch cabinet panels, home wall switches, security camera housings and power tool housings. The current difficulty of this type of product is to take into account both toughness and flame retardancy. Since product parts usually need to include screw columns for fastening and installation, the screw column structure has concentrated stress and is usually added with lubricants and other substances, which are prone to cracking. Therefore, the material is required to have good toughness and a certain degree of chemical resistance. The flame retardancy requirements for electronic product housings are high, so the flame retardancy of the material also needs to be improved on the basis of improving toughness.
[0004] CN101628983A discloses a method for improving the crack resistance of colored polycarbonate, by chemically treating the pigment, then extruding and granulating, the product is injection molded into a product and immersed in CCL4, and the product does not crack, but the invention does not involve flame retardant properties and antistatic properties, and the pre-treatment is not environmentally friendly. In order to achieve the color effect, the traditional method is adopted to add color powder, which causes serious pollution to the site and does not meet the conditions for mass production. CN 106046740 A discloses a ternary rubber blended PC composite flame retardant crack resistance and its preparation method and application. By adding EPDM rubber, basalt fiber, chlorinated polyethylene, etc., the mechanical properties and stability of the product are greatly improved, but the flame retardant properties of the composite material prepared by the invention are not involved, which will greatly limit its application range. CN111138822B discloses a flame-retardant polycarbonate composite material, which is obtained by compounding common engineering plastic PC with a rare earth phenylphosphonate-loaded metal organic framework, using flaky rare earth phenylphosphonate as a template, allowing the metal organic framework (Zr-BDC) to be loaded and grown thereon, and by melt blending, a polycarbonate composite material with good dispersion, improved flame retardancy and improved thermal stability is obtained. However, the mechanical properties of the composite material prepared by this invention are not involved. For some application fields with high requirements for crack resistance, the products prepared by this method will be subject to certain limitations. Summary of the invention
[0005] In view of the problem that polycarbonate materials in the prior art are difficult to balance toughness and flame retardancy, the purpose of the present invention is first to provide a carbon nanotube modified silicone rubber and a preparation method. The modified silicone rubber has the characteristics of good high and low temperature resistance, excellent oil resistance, wear resistance and certain flame retardancy, and can be used to prepare modified polycarbonate materials and improve the performance of composite materials.
[0006] The purpose of the present invention is also to provide a crack-resistant flame-retardant polycarbonate material and a preparation method thereof. The introduction of the above-mentioned carbon nanotube-modified silicone rubber into the flame-retardant polycarbonate material can significantly improve the material's crack resistance and at the same time improve the material's flame retardant properties. The material can absorb ultraviolet rays and emit blue or purple light, thereby increasing the brightness and whiteness of plastic products.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0008] In a first aspect, the present invention provides a method for preparing a carbon nanotube-modified silicone rubber, the steps comprising:
[0009] 1) mixing silicone rubber with an alcohol solution of an aminosilane coupling agent to react, and then washing with alcohol to obtain a surface amino silicone rubber;
[0010] 2) placing the carbon nanotubes in concentrated acid for ultrasonic acidification, and then filtering, washing, and drying to obtain acidified carbon nanotubes;
[0011] 3) The surface amino-modified silicone rubber in step 1) and the acidified carbon nanotubes in step 2) are mixed with N,N-dimethylformamide, reacted under ultrasonic conditions, and then filtered, washed and dried to obtain carbon nanotube-modified silicone rubber.
[0012] In a specific embodiment, the silicone rubber in step 1) is selected from at least one of methyl silicone rubber, methyl vinyl silicone rubber, methyl vinyl phenyl silicone rubber, fluorosilicone rubber, etc., preferably methyl vinyl silicone rubber.
[0013] In a specific embodiment, in step 1), the alcohol solution of the aminosilane coupling agent, the solvent alcohol is selected from C1 to C4 alcohols, preferably ethanol or methanol;
[0014] Preferably, the concentration of the aminosilane coupling agent solution is 0.5-1wt%, such as 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, etc.;
[0015] Preferably, the aminosilane coupling agent is selected from at least one of a monoaminosilane coupling agent, a bisaminosilane coupling agent, a triaminosilane coupling agent, etc. according to the number of amino groups, preferably a bisaminosilane coupling agent.
[0016] In a specific embodiment, the mass ratio of the silicone rubber to the alcohol solution of the aminosilane coupling agent in step 1) is 1:(1-2.5), for example, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.5, etc., and the alcohol solution of the aminosilane coupling agent is calculated based on the mass of the aminosilane coupling agent therein.
[0017] In a specific embodiment, the reaction in step 1) has no particular requirement for the temperature, room temperature is sufficient, and the reaction time is 1-3 h, for example, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, etc.
[0018] In a specific embodiment, in step 1), the alcohol washing is selected from at least one of methanol and ethanol, preferably ethanol.
[0019] In a specific embodiment, the carbon nanotubes in step 2) are selected from single-walled carbon nanotubes;
[0020] Preferably, the length of the carbon nanotubes is 5-15 um, such as 5 um, 7 um, 9 um, 11 um, 13 um, 15 um, etc., and the average outer diameter of the carbon nanotubes is 1.6±0.04 nm.
[0021] In a specific embodiment, the concentration of the concentrated acid in step 2) is 70-98wt%, such as 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, 95wt%, 98wt%, etc.;
[0022] Preferably, the concentrated acid is selected from at least one of concentrated sulfuric acid and concentrated nitric acid.
[0023] In a specific embodiment, in step 2), the ultrasonic acidification has an acidification temperature of 40-80°C, such as 40°C, 50°C, 60°C, 70°C, 80°C, etc., and an acidification time of 4-12h, such as 4h, 6h, 8h, 10h, 12h, etc.
[0024] In a specific embodiment, in step 3), the mass ratio of the surface amino silicone rubber to the acidified carbon nanotubes is 1:1-3, for example, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, etc.
[0025] In a specific embodiment, the concentration of the acidified carbon nanotubes in N,N-dimethylformamide in step 3) is 0.1-0.5 g / ml, such as 0.1 g / ml, 0.2 g / ml, 0.3 g / ml, 0.4 g / ml, 0.50 g / ml, etc.
[0026] In a specific embodiment, in step 3), the reaction temperature is 80-100°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, etc., and the reaction time is 4-6h, for example, 4h, 4.5h, 5h, 5.5h, 6h, etc.
[0027] In the present invention, the conditions of the ultrasonic operation, such as frequency, are not specifically limited; the above preparation method also includes post-processing processes such as filtration, washing, and drying, which can all be conventionally performed in the field, and the present invention has no special requirements.
[0028] In a second aspect, the present invention provides a carbon nanotube-modified silicone rubber prepared by the above method, wherein the carbon nanotube-modified silicone rubber is silicone rubber with carbon nanotubes grafted on the surface.
[0029] In a third aspect, the present invention provides the use of the carbon nanotube-modified silicone rubber described above in a polycarbonate material.
[0030] Specifically, a crack-resistant flame-retardant polycarbonate material comprises the following raw materials in parts by weight:
[0031] Polycarbonate 79.6-96.75 parts, for example 79.6, 82, 85, 88, 90, 92, 95, 96.75 parts, etc., preferably 85.4-94.3 parts;
[0032] 0.5-5.0 parts of toughening agent, for example 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 parts, etc., preferably 1.0-3.0 parts;
[0033] 1.0-8.0 parts of carbon nanotube modified silicone rubber, such as 1, 2, 3, 4, 5, 6, 7, 8 parts, etc., preferably 2.0-6.0 parts;
[0034] Sulfonate flame retardant 0.05-0.4 parts, such as 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4 parts, etc., preferably 0.1-0.3 parts;
[0035] 0.2-1.0 part of anti-dripping agent, such as 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 part, etc., preferably 0.3-0.8 part;
[0036] 1-3 parts of fluorescent agent, such as 1, 1.5, 2, 2.5, 3 parts, etc., preferably 1.5-2.5 parts;
[0037] Processing aid 0-3.0 parts, such as 0, 0.5, 1, 1.5, 2, 2.5, 3 parts, etc., preferably 0.8-2.0 parts.
[0038] In a specific embodiment, the polycarbonate is selected from one or more of aromatic polycarbonates and aliphatic polycarbonates, preferably bisphenol A polycarbonate;
[0039] Preferably, when the test conditions are 300°C and 1.2kg, the melt flow index of the polycarbonate is 3-65g / 10min, for example, 3g / 10min, 10g / 10min, 20g / 10min, 30g / 10min, 40g / 10min, 50g / 10min, 60g / 10min, 65g / 10min, etc., preferably 5-50g / 10min, and more preferably 7-35g / 10min.
[0040] In a specific embodiment, the toughening agent is selected from one or more of ethylene-acrylate-glycidyl methacrylate copolymer, methacrylate-butadiene-styrene copolymer, and ethylene-methacrylate copolymer, preferably ethylene-methacrylate-glycidyl methacrylate random block copolymer, methyl methacrylate-butadiene-styrene core-shell structure copolymer, and ethylene-methacrylate random block copolymer; wherein the mass proportion of methacrylate in the ethylene-methacrylate random block copolymer is preferably 15-25%, for example 15%, 18%, 21%, 23%, and 25%.
[0041] In a specific embodiment, the toughening agent is selected from MBS (methyl methacrylate-butadiene-styrene terpolymer) coated polyethylene;
[0042] In the present invention, the MBS-coated polyethylene can be prepared by any method. Unless otherwise specified, the preparation method can refer to the prior art. In a preferred embodiment, the MBS-coated polyethylene is prepared by the following method:
[0043] The polyethylene, MBS and initiator are mixed evenly, added into a twin-screw extruder for melting, and then extruded and granulated to obtain MBS-coated polyethylene.
[0044] Preferably, the barrel temperature of the twin-screw extruder is 160-220°C, for example, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, etc., and the screw speed is 220-450 rpm, for example, 220 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, etc.
[0045] Preferably, the weight percentage of the raw material polyethylene, MBS and initiator is as follows:
[0046] 84 to 97.8 parts, for example 84, 86, 88, 90, 92, 95, 97.8 parts, etc., preferably 89.6 to 94.7 parts of polyethylene;
[0047] 2 to 15 parts, such as 2, 4, 6, 8, 10, 12, 15 parts, etc., preferably 5 to 10 parts of MBS;
[0048] 0.2-1 part, such as 0.2, 0.4, 0.6, 0.8, 1 part, etc., preferably 0.3-0.4 part of initiator.
[0049] Preferably, the polyethylene, MBS and initiator are mixed in a high-speed mixer for 3-5 minutes, for example, 3 minutes, 4 minutes, 5 minutes, etc.
[0050] Preferably, the polyethylene is selected from one or more of linear low-density polyethylene (LDPE) and high-density polyethylene (HDPE), more preferably high-density polyethylene;
[0051] More preferably, when the test conditions are 190°C and 2.16kg, the melt flow index of the polyethylene is 0.20-20g / 10min, for example 0.2g / 10min, 1g / 10min, 5g / 10min, 10g / 10min, 15g / 10min, 20g / 10min, etc., preferably 1-4g / 10min.
[0052] Preferably, the initiator is selected from one or more of dicumyl peroxide (DCP) and dibenzoyl peroxide (BPO), more preferably DCP.
[0053] In a specific embodiment, the sulfonate-based flame retardant is selected from one or more of perfluorobutane sulfonic acid (PFBS) such as flame retardant EF42, potassium 3-phenylsulfonylbenzenesulfonate (KSS), and isethionic acid (HES).
[0054] In a specific embodiment, the anti-dripping agent is selected from high molecular weight polytetrafluoroethylene, preferably one or more of FD3100, SN3310, and TF1645.
[0055] In a specific embodiment, the fluorescent agent is selected from one or more of KSN, OB, and organosilicon fluorescent polymer, preferably an organosilicon fluorescent polymer.
[0056] In a specific embodiment, the processing aid is conventionally selected in the field, for example, one or a combination of two or more selected from antioxidants, lubricants, light stabilizers, heat stabilizers, antistatic agents, fillers, antifogging agents, light diffusers and infrared absorbers.
[0057] Preferably, the antioxidant is one or a combination of two or more of hindered phenols, phosphites, thioesters, benzofurans, acryl-modified phenols, and hydroxylamine antioxidants.
[0058] Preferably, the lubricant is one or a combination of two or more of fatty alcohols, metal soaps, fatty acids, fatty acid esters, amide waxes, saturated hydrocarbons, polyolefin waxes and their derivatives, silicones and silicone powders, and organic fluorines, and preferably a fatty acid ester lubricant is used.
[0059] In a fourth aspect, the present invention further provides a method for preparing the aforementioned crack-resistant flame-retardant polycarbonate material, specifically using a conventional melt extrusion method, comprising the following steps:
[0060] S1: polycarbonate, toughening agent, carbon nanotube modified silicone rubber, sulfonate flame retardant, anti-dripping agent, fluorescent agent and optional processing aid are mixed uniformly, preferably added together into a high-speed mixer and mixed for 3-5 minutes, for example, 3 minutes, 4 minutes, 5 minutes, etc.;
[0061] S2: adding the mixed material into a twin-screw extruder for melting, and then extruding and granulating to obtain a crack-resistant flame-retardant polycarbonate material; preferably, the barrel temperature of the twin-screw extruder is 250-280°C, for example, 250°C, 260°C, 270°C, 280°C, etc., and the screw speed is 200-600 rpm, for example, 200 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, etc.
[0062] Compared with the prior art, the present invention has the following technical advantages:
[0063] 1) Traditional silicone rubber has serious defects in heat resistance and mechanical properties due to the poor cohesive energy of the silicone molecular chain, which seriously restricts its development. The present invention uses filler carbon nanotubes to graft silicone rubber, which can effectively improve the mechanical properties and heat resistance of silicone rubber, and also solve the agglomeration problem of carbon nanotubes. In addition, the silicon element in silicone rubber can promote the carbonization of PC in the condensed phase during the combustion of the composite material, and then form a significant flame retardant synergistic effect with carbon nanotubes and sulfonates. Secondly, carbon nanotubes, as an inorganic nanoparticle, can form an exfoliated layer structure in the PC composite material. It plays a supporting role as the skeleton of the carbon layer, effectively improving the flame retardant properties of the composite material. Through the combination of the two, the flame retardant properties, crack resistance and mechanical properties of the composite material can be effectively improved.
[0064] 2) In a preferred embodiment of the present invention, MBS is also used to coat polyethylene for toughening. Compared with directly adding PE, it has better compatibility with the PC substrate and greatly improves the dispersion ability of the toughening structure in the substrate. At the same time, the crystallization ability of polyethylene can significantly improve the chemical resistance of the material, so that the product can still maintain crack resistance when exposed to chemical reagents and stress at the same time.
[0065] 3) The present invention adds a fluorescent agent to the PC modified formula. Compared with the traditional method of adding color powder, it has the advantages of high production efficiency, stable fluorescent effect and low cost, and can be widely used in home appliances, electronic appliances, new energy vehicles and other fields. DETAILED DESCRIPTION
[0066] The present invention is further explained below by more specific examples, but does not constitute any limitation.
[0067] In each embodiment and comparative example of the present invention, the sources of the main raw materials used are as shown in Table 1 below:
[0068] Table 1
[0069]
[0070]
[0071] Unless otherwise specified, other raw materials and reagents were purchased from commercial sources.
[0072] In each embodiment and comparative example of the present invention, the performance test parameters and corresponding test methods of the polycarbonate material are as shown in Table 2 below:
[0073] Table 2
[0074]
[0075] The main equipment used in the present invention is:
[0076] Twin-screw extruder, Coperion, model KM 28*40D BP series, aspect ratio 40:1, screw diameter 28 cm;
[0077] Injection molding machine, 100-ton Demag injection molding machine, model Systec 100 / 420-310C;
[0078] German ZWICK Z010TE universal testing machine;
[0079] German ZWICK HIT25P pendulum impact tester;
[0080] Wester RH6033A combustion test chamber.
[0081] Toughening agent preparation example 1-3:
[0082] The toughening agent (MBS coated polyethylene) PBS-1 was prepared by adding 84 g of polyethylene LLDPE DFDA 7042, 15 g of MBS and 1 g of initiator BPO into a high mixer and mixing for 3 min, and then adding them to the main feed of a twin-screw extruder. The extrusion conditions were: screw speed of 220 rpm, and the barrel temperature of the twin-screw extruder was set in stages to: 160°C, 160°C, 160°C, 160°C, 160°C, 160°C, 160°C, 170°C, 170°C, 170°C, to obtain toughening agent PBS-1.
[0083] The toughening agent (MBS coated polyethylene) PBS-2 was prepared by adding 97.8 g of polyethylene HDPE 5000s, 2 g of MBS and 0.2 g of initiator DCP into a high mixer and mixing for 5 min, and then adding the mixture to the main feed of a twin-screw extruder. The extrusion conditions were as follows: the screw speed was 450 rpm, and the barrel temperature of the twin-screw extruder was set in stages to 180°C, 210°C, 210°C, 210°C, 210°C, 210°C, 210°C, 210°C, 220°C, and 220°C to obtain the toughening agent PBS-2.
[0084] The toughening agent (MBS coated polyethylene) PBS-3 is prepared by adding 90g polyethylene HDPE 6100G, 9.4g MBS and 0.6g initiator BPO into a high mixer and mixing for 4 minutes, and then adding it to the main feed of a twin-screw extruder. The extrusion conditions are: screw speed 300rpm, and the barrel temperature of the twin-screw extruder is set in stages as follows: 180°C, 180°C, 185°C, 180°C, 180°C, 180°C, 180°C, 185°C, 185°C, to obtain a PBS-3 modified toughening agent.
[0085] Example 1
[0086] Preparation of carbon nanotube modified silicone rubber:
[0087] 1) 50 g of methyl vinyl silicone rubber was immersed in 50 g of 0.5 wt % monoaminosilane coupling agent ethanol solution, reacted at room temperature for 1 hour, and then rinsed with ethanol to obtain surface amino silicone rubber.
[0088] 2) 100 g of single-walled carbon nanotubes (length 5 μm, average outer diameter 1.56 nm) were placed in 70 wt% concentrated sulfuric acid, ultrasonically acidified at 40°C for 4 h, filtered, and repeatedly washed with water until the filtrate was neutral. The product was dried in an oven at 60°C to obtain acidified carbon nanotubes SM-MWNT.
[0089] 3) Take 10g of SM-MWNT and mix it with 80ml of DMF to make a solution with a concentration of 0.125g / ml, then add 10g of surface amino silicone rubber, react with ultrasound at 80°C for 4h, filter, wash with water, and then dry to constant weight to obtain silicone rubber with surface grafted carbon nanotubes (carbon nanotube modified silicone rubber-1).
[0090] Preparation of crack-resistant flame-retardant polycarbonate materials:
[0091] S1: 79.6 g polycarbonate PC2100, 5.0 g toughening agent PBS-1, 8.0 g carbon nanotube modified silicone rubber-1, 0.4 g sulfonate flame retardant KSS, 1.0 g anti-dripping agent FD3100, 3.0 g Glucose-PEG-PMMA, 0.5 g antioxidant 1076, 2 g antioxidant 168 and 0.5 g lubricant PETs were added into a high mixer and mixed for 5 min.
[0092] S2: Add the mixed materials in S1 into the main feed of the twin-screw extruder. The extrusion conditions are: screw speed 200rpm, screw temperature from feed port to die head is set in sections as follows: 260℃, 260℃, 265℃, 265℃, 270℃, 270℃, 265℃, 265℃, 260℃, 260℃.
[0093] Example 2
[0094] Preparation of carbon nanotube modified silicone rubber:
[0095] 1) 40 g of methyl vinyl phenyl silicone rubber was immersed in 100 g of a 1 wt % methanol solution of a bisaminosilane coupling agent, reacted at room temperature for 3 h, and then rinsed with methanol to obtain a surface amino silicone rubber.
[0096] 2) 200 g of single-walled carbon nanotubes (length 15 μm, average outer diameter 1.64 nm) were placed in 98 wt% concentrated nitric acid, ultrasonically acidified at 80°C for 12 h, filtered, and repeatedly washed with water until the filtrate was neutral. The product was dried in an oven at 120°C to obtain acidified carbon nanotubes SM-MWNT.
[0097] 3) 150 g of SM-MWNT was mixed with 500 ml of DMF to form a solution with a concentration of 0.5 g / ml, and then 50 g of surface amino-modified silicone rubber was added. The solution was subjected to ultrasonic reaction at 100°C for 6 h, filtered, washed with water, and then dried to constant weight to obtain silicone rubber with surface grafted carbon nanotubes (carbon nanotube-modified silicone rubber-2).
[0098] Preparation of crack-resistant flame-retardant polycarbonate materials:
[0099] S1: 96.75 g polycarbonate PC2200, 0.5 g toughening agent PBS-2, 1.0 g carbon nanotube modified silicone rubber-2, 0.05 g sulfonate flame retardant EF-42, 0.2 g anti-dripping agent TF1645, 1.0 g fluorescent brightener KSN, 0.1 g antioxidant 1076, 0.2 g antioxidant 168, and 0.2 g lubricant PETs were added into a high mixer and mixed for 3 min.
[0100] S2: Add the mixed materials in S1 into the main feed of the twin-screw extruder. The extrusion conditions are: screw speed 600rpm, and the screw temperature from the feed port to the die is set in sections as follows: 255℃, 265℃, 270℃, 275℃, 275℃, 280℃, 280℃, 275℃, 275℃, 270℃, 270℃.
[0101] Example 3
[0102] Preparation of carbon nanotube modified silicone rubber:
[0103] 1) 50 g of methyl silicone rubber was immersed in 75 g of 0.8 wt % triaminosilane coupling agent ethanol solution, reacted at room temperature for 2 h, and then rinsed with ethanol to obtain surface amino silicone rubber.
[0104] 2) 120 g of single-walled carbon nanotubes (length 10 μm, average outer diameter 1.60 nm) were placed in 90 wt% concentrated sulfuric acid, ultrasonically acidified at 60°C for 8 h, filtered, and repeatedly washed with water until the filtrate was neutral. The product was dried in an oven at 90°C to obtain acidified carbon nanotubes SM-MWNT.
[0105] 3) 60 g of SM-MWNT was mixed with 120 ml of DMF to form a solution with a concentration of 0.3 g / ml, and then 40 g of surface amino-modified silicone rubber was added. The solution was subjected to ultrasonic reaction at 90°C for 5 h, filtered, washed with water, and then dried to constant weight to obtain silicone rubber with surface grafted carbon nanotubes (carbon nanotube-modified silicone rubber-3).
[0106] Preparation of crack-resistant flame-retardant polycarbonate materials:
[0107] S1: 91.8 g polycarbonate PC2150, 2.0 g toughening agent PBS-3, 3.0 g carbon nanotube modified silicone rubber-2, 0.1 g sulfonate flame retardant HES, 0.6 g anti-dripping agent SN3310, 1.5 g fluorescent brightener OB, 0.3 g antioxidant 1076, 0.4 g antioxidant 168 and 0.3 g lubricant PETs were added into a high mixer and mixed for 4 min.
[0108] S2: Add the mixed materials in S1 into the main feed of the twin-screw extruder. The extrusion conditions are: screw speed 500rpm, and the screw temperature from the feed port to the die is set in sections as follows: 255℃, 265℃, 270℃, 275℃, 275℃, 280℃, 280℃, 275℃, 275℃, 270℃, 270℃.
[0109] Example 4
[0110] The crack-resistant flame-retardant polycarbonate material was prepared by referring to the method of Example 2, except that the toughening agent PBS-2 was replaced by an equal amount of toughening agent AX8900, and other operations and conditions remained unchanged.
[0111] Comparative Example 1
[0112] The crack-resistant flame-retardant polycarbonate material was prepared by referring to the method of Example 1, except that the toughening agent PBS-1 was replaced by an equal amount of MBS, and other operations and conditions remained unchanged.
[0113] Comparative Example 2
[0114] The crack-resistant flame-retardant polycarbonate material was prepared by referring to the method of Example 1, except that the toughening agent PBS-1 was replaced by a mixture of the raw materials HDPE 5000s and MBS, and other operations and conditions remained unchanged.
[0115] Comparative Example 3
[0116] The crack-resistant flame-retardant polycarbonate material was prepared by referring to the method of Example 1, except that the carbon nanotube-modified silicone rubber-1 was replaced with an equal amount of unmodified silicone rubber, and other operations and conditions remained unchanged.
[0117] Comparative Example 4
[0118] The crack-resistant flame-retardant polycarbonate material was prepared by referring to the method of Example 1, except that the carbon nanotube-modified silicone rubber-1 was replaced by a mixture of carbon nanotubes and silicone rubber as its preparation raw materials, and other operations and conditions remained unchanged.
[0119] The polycarbonate materials in Examples 1-3 of the present invention and Comparative Examples 1-4 were tested for performance according to the aforementioned method, and the results are shown in Table 3 below:
[0120] Table 3 Performance test results of Examples 1-3 and Comparative Examples 1-4
[0121]
[0122] It can be seen from Comparative Examples 1-4 and Examples 1-4 that the composite materials prepared in the examples of the present invention have excellent comprehensive performance, can significantly improve the crack resistance and flame retardancy of the materials, and at the same time have excellent resistance to chemical agents.
[0123] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention. Those skilled in the art will appreciate that, under the guidance of this specification, some modifications or adjustments may be made to the present invention. These modifications or adjustments should also be within the scope defined by the claims of the present invention.
Claims
1. A method for preparing carbon nanotube-modified silicone rubber, characterized in that the steps include: 1) mixing silicone rubber with an alcohol solution of an aminosilane coupling agent to react, and then washing with alcohol to obtain a surface amino silicone rubber; 2) placing the carbon nanotubes in concentrated acid for ultrasonic acidification, and then filtering, washing, and drying to obtain acidified carbon nanotubes; 3) The surface amino-modified silicone rubber in step 1) and the acidified carbon nanotubes in step 2) are mixed with N,N-dimethylformamide, reacted under ultrasonic conditions, and then filtered, washed and dried to obtain carbon nanotube-modified silicone rubber.
2. The preparation method according to claim 1, characterized in that: Step 1) the silicone rubber is selected from at least one of methyl silicone rubber, methyl vinyl silicone rubber, methyl vinyl phenyl silicone rubber and fluorosilicone rubber, preferably methyl vinyl silicone rubber; and / or Step 1) the alcohol solution of the aminosilane coupling agent, wherein the solvent alcohol is selected from C1 to C4 alcohols, preferably ethanol or methanol; Preferably, the concentration of the aminosilane coupling agent solution is 0.5-1wt%; Preferably, the aminosilane coupling agent is selected from monoaminosilane coupling agent, bisaminosilane coupling agent and triaminosilane coupling agent, preferably bisaminosilane coupling agent; and / or Step 1) The mass ratio of the silicone rubber to the alcohol solution of the aminosilane coupling agent is 1:(1-2.5), and the alcohol solution of the aminosilane coupling agent is calculated based on the mass of the aminosilane coupling agent therein; and / or Step 1) The reaction time is 1-3h; and / or In step 1), the alcohol washing is selected from at least one of methanol and ethanol, preferably ethanol.
3. The preparation method according to claim 1 or 2, characterized in that: Step 2) the carbon nanotubes are selected from single-walled carbon nanotubes; Preferably, the carbon nanotubes have a length of 5-15 um and an average outer diameter of 1.6±0.04 nm; and / or Step 2) The concentrated acid has a concentration of 70-98 wt %; Preferably, the concentrated acid is selected from at least one of concentrated sulfuric acid and concentrated nitric acid; and / or In step 2), the ultrasonic acidification temperature is 40-80° C. and the acidification time is 4-12 h.
4. The preparation method according to any one of claims 1 to 3, characterized in that Step 3) the mass ratio of the surface amino silicone rubber to the acidified carbon nanotubes is 1:1-3; and / or Step 3) The concentration of the acidified carbon nanotubes in N,N-dimethylformamide is 0.1-0.5 g / ml; and / or In step 3), the reaction temperature is 80-100° C. and the reaction time is 4-6 h.
5. A carbon nanotube-modified silicone rubber prepared by the method according to any one of claims 1 to 4.
6. Use of the carbon nanotube-modified silicone rubber prepared by the method according to any one of claims 1 to 4 in polycarbonate materials.
7. A crack-resistant flame-retardant polycarbonate material, characterized in that: Contains the following raw materials by weight: The carbon nanotube-modified silicone rubber is selected from the carbon nanotube-modified silicone rubber prepared by the method according to any one of claims 1 to 4.
8. The crack-resistant flame-retardant polycarbonate material according to claim 7, characterized in that: The polycarbonate is selected from one or more of aromatic polycarbonate and aliphatic polycarbonate, preferably bisphenol A polycarbonate; Preferably, when the test conditions are 300°C and 1.2 kg, the melt flow index of the polycarbonate is 3-65 g / 10 min, preferably 5-50 g / 10 min, more preferably 7-35 g / 10 min; and / or The toughening agent is selected from one or more of ethylene-acrylate-glycidyl methacrylate copolymer, methacrylate-butadiene-styrene copolymer, and ethylene-methacrylate copolymer, preferably one or more of ethylene-methacrylate-glycidyl methacrylate random block copolymer, methyl methacrylate-butadiene-styrene core-shell copolymer, and ethylene-methacrylate random block copolymer; wherein the mass proportion of methacrylate in the ethylene-methacrylate random block copolymer is preferably 15-25wt%; and / or The toughening agent is selected from MBS coated polyethylene.
9. The crack-resistant flame-retardant polycarbonate material according to claim 7, characterized in that: The sulfonate flame retardant is selected from one or more of perfluorobutane sulfonic acid, potassium 3-phenylsulfonylbenzenesulfonate, and isethionic acid; and / or The anti-dripping agent is selected from high molecular weight polytetrafluoroethylene, preferably one or more of FD3100, SN3310, and TF1645; and / or The fluorescent agent is selected from one or more of KSN, OB, and organic silicon fluorescent polymer, preferably organic silicon fluorescent polymer; and / or The processing aid is selected from one or a combination of two or more of an antioxidant, a lubricant, a light stabilizer, a heat stabilizer, an antistatic agent, a filler, an antifogging agent, a light diffuser and an infrared absorber; Preferably, the antioxidant is one or a combination of two or more of hindered phenols, phosphites, thioesters, benzofurans, acryl-modified phenols, and hydroxylamine antioxidants; Preferably, the lubricant is one or a combination of two or more of fatty alcohols, metal soaps, fatty acids, fatty acid esters, amide waxes, saturated hydrocarbons, polyolefin waxes and their derivatives, silicones and silicone powders, and organic fluorines, preferably fatty acid ester lubricants.
10. A method for preparing the crack-resistant flame-retardant polycarbonate material according to any one of claims 7 to 9, characterized in that: The following steps are involved: S1: uniformly mix polycarbonate, toughening agent, carbon nanotube modified silicone rubber, sulfonate flame retardant, anti-dripping agent, fluorescent agent and optional processing aid, preferably add them together into a high-speed mixer and mix for 3-5 minutes; S2: adding the mixed material into a twin-screw extruder for melting, and then extruding and granulating to obtain a crack-resistant flame-retardant polycarbonate material; preferably, the barrel temperature of the twin-screw extruder is 250-280° C., and the screw speed is 200-600 rpm.
Citation Information
Patent Citations
Halogen-free flame-retardant cold-resistant polycarbonate alloy and preparation method thereof
CN103509326A
Flame-retardant polycarbonate composition and preparation method thereof
CN104497536A
Preparation method of reactive carbon nanotube flame retardant
CN105037734A
Dew point corrosion resistant coating and preparation method thereof
CN113088159A
Cited By
Preparation method of extra-high-viscosity PE film
CN121064509A