Method for preparing biomass micro-nano fiber oriented modified plastic through wet feeding method extrusion
Through the wet feed extrusion method, the dry pollution and agglomeration problems in the preparation of biomass micro-nano fiber reinforced plastics are solved, and the directional distribution of biomass micro-nano fibers in the plastic matrix is realized, which improves the mechanical properties and heat of composite materials. Stability, suitable for green production in high-value fields.
Patent Information
- Application Number
- CN202411175781.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-26
AI Technical Summary
There are problems of drying pollution, agglomeration, dust pollution and poor toughness of composite materials in the preparation of existing biomass micro-nano fiber reinforced plastics. The drying process is time-consuming and labor-intensive and affects dispersion and interface compatibility.
Using the wet feed extrusion method, plastic particles and additives are added to the wet slurry containing biomass micro-nano fibers and stirred and then melted and kneaded and extruded. The drying step is cancelled, and water is used as the conveying medium and fiber-dissolving agent to achieve biogenesis. Directional distribution of material micro-nano fibers in plastic matrix.
Simplify the process, improve the mechanical properties and thermal stability of composite materials, reduce dust pollution, enhance interface binding capabilities, and achieve green and clean production, suitable for high-value fields.
Smart Images

Figure CN119019775A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing modified plastics, in particular to a method for preparing biomass micro-nano fiber directional modified plastics by extrusion using a wet feed method. Background Art
[0002] At present, the research on using biomass micro-nano fibers (MNF) to reinforce polymers mainly has the following problems: (1) Chemical defibration is easy to pollute the environment; (2) MNF is easy to agglomerate after drying; (3) Dried MNF fibers are fluffy and too light, making it difficult to mix them evenly with plastics; (4) The interface between the two phases is not firmly bonded; (5) The strength and toughness of the composite materials are poor. MNF-reinforced composites are usually prepared by mixing and molding, which is to blend MNF and plastics and melt them, and then process them into shapes by mechanical methods such as extrusion, injection molding, and molding; in most studies, MNF is dried before compounding, and commonly used methods include freeze drying, spray drying, vacuum drying, and oven drying. In most drying methods, MNF agglomeration will occur, which directly affects the uniform dispersion of MNF in the polymer matrix. Although the drying methods are different, the method of mixing dry MNF with polymer for extrusion (i.e., dry extrusion) has many common disadvantages: first, the drying process of MNF is time-consuming and labor-intensive, and is prone to dust pollution; second, since MNF has a strong hydrophilicity, the drying process may lead to irreversible agglomeration and produce micron-sized or larger particles.
[0003] The degree of dispersion of MNF in the polymer matrix and the interfacial compatibility of the two phases are the key to ensuring the high performance of composite materials. How to solve the problems of agglomeration and dust pollution in the production process of MNF composite materials and simplify the production process while ensuring the performance of the composite materials is of great significance to the application of fiber composite materials in a wider range of fields. Summary of the invention
[0004] Purpose of the invention: The present invention aims to provide a method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion, which has the advantages of simplifying the process and being beneficial to improving the mechanical properties and thermal stability of the modified plastics. The biomass micro-nano fibers can be oriented in the plastic matrix during extrusion melt mixing, which can effectively reduce the agglomeration of the biomass micro-nano fibers when they are blended and melted with the plastic.
[0005] Technical solution: The method for preparing biomass micro-nano fiber directional modified plastic by wet feed extrusion according to the present invention comprises the following steps:
[0006] Plastic particles and additives are added to a wet slurry containing biomass micro-nano fibers, and a blend is obtained after stirring, wherein the solid content of the biomass micro-nano fibers in the wet slurry is 25-40wt%; the obtained blend is then melt-mixed and extruded to obtain a biomass micro-nano fiber directional modified plastic.
[0007] Furthermore, the preparation method of the wet slurry containing biomass micro-nano fibers includes: pre-treating the biomass raw material with alkali and washing and swelling it with water to obtain biomass fibers, then crushing, stirring and dispersing the biomass fibers to obtain biomass micro-nano fibers, and then filtering the dispersible suspension to a wet slurry state without dripping water to obtain the wet slurry containing biomass micro-nano fibers.
[0008] Furthermore, the biomass raw material is treated in an alkali solution in a water bath for 2 to 6 hours, then soaked at room temperature for 10 to 24 hours, and then taken out and washed with water to neutrality to obtain swollen biomass fibers, wherein the concentration of the alkali solution is 1 to 5 wt%.
[0009] Furthermore, the defibration process includes defibration in a high-speed mixer at a speed of 8000 to 12000 r / min for 3 to 5 minutes.
[0010] Furthermore, the diameter of the biomass micro-nano fiber is 100 nm to 100 μm.
[0011] Furthermore, in the biomass micro-nano fiber directional modified plastic, the content of plastic particles is 15-95%, the content of additives is 2-10%, the content of biomass micro-nano fibers is 3-75%, and the additives include coupling agents and / or lubricants.
[0012] Furthermore, the temperature of the extrusion process is controlled at 158-165° C., the screw speed is 20-40 rpm, and the extrusion process is performed while vacuuming and exhausting.
[0013] Furthermore, the plastic particles are thermoplastic plastics, including at least one of polyethylene, polypropylene, nylon, polyvinyl chloride, polyethylene terephthalate, polystyrene, polycarbonate, polymethyl methacrylate, polytetrafluoroethylene, polyetheretherketone, acrylonitrile-styrene-butadiene copolymer, polylactic acid or polybutylene terephthalate. The raw materials for preparing the biomass micro-nano fibers include at least one of wood, bamboo, straw, rice husk, hemp, cotton, coconut shell or sugarcane.
[0014] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0015] (1) It is beneficial to enhance the mechanical properties of modified plastics; wet feeding is adopted, wherein water can not only play a role of plasticization, but also serve as a conveying medium for biomass micro-nano fiber feeding, promoting further fibrillation of biomass micro-nano fibers during the meshing process of the extruder screw, so as to improve the dispersibility of biomass micro-nano fibers in composite materials, improve the mixing effect, solve the fiber agglomeration problem in the production process of biomass micro-nano fiber reinforced plastic composites, realize the orientation of biomass micro-nano fibers in the plastic matrix during extrusion melt mixing, improve the interface bonding ability between the two phases, and greatly enhance the mechanical properties of the composite material; different from the traditional biomass raw materials in the plastic matrix as a filling role, the present invention uses wet feeding mixing extrusion molding, the biomass micro-nano fibers are fully combined with the plastic matrix, and the fibers realize directional flow in the barrel flow channel, and the biomass micro-nano fibers have a directional reinforcement effect;
[0016] (2) The modified plastic has high strength and low thermal expansion coefficient; by using the oriented arrangement of biomass micro-nano fibers in a wet state, the defects of poor stress support capacity and poor stability of most plastics can be overcome, and a new type of micro-nano fiber modified plastic with high strength and low thermal expansion coefficient can be developed; breaking through the bottleneck of traditional plastics that are limited by stability and cannot be applied on a large scale in high-value fields;
[0017] (3) Simplify the process; wet extrusion eliminates the step of drying biomass micro-nano fibers, which saves energy and time, avoids dust pollution, and can achieve green and clean production. It has good industrialization prospects in high-value fields such as high-strength engineering materials and automotive body materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a transmission electron microscope image of wood micro-nano fibers;
[0019] Figure 2 This is a scanning electron microscope image of 30% wood micro-nano fiber modified polyethylene;
[0020] Figure 3 The flexural mechanical properties of polyethylene composites modified with wood micro-nano fibers in different proportions;
[0021] Figure 4 is the linear thermal expansion coefficient of polyethylene modified with wood micro-nano fibers in different proportions. DETAILED DESCRIPTION
[0022] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0023] Example 1
[0024] (1) After the poplar wood shavings are mechanically crushed, they are placed in a 2 wt% concentration of industrial caustic soda in a 95°C water bath for 2 h, then soaked at room temperature for 10 h, and then taken out and washed with deionized water until neutral, thereby obtaining swollen poplar wood fibers;
[0025] (2) The poplar wood fiber in step (1) is placed in a high-speed defibration mixer for defibration and stirred for 5 minutes at a speed of 12000 r / min to obtain a poplar wood micro-nano fiber suspension with a diameter of 100 nm to 100 μm.
[0026] (3) vacuum filtering the poplar wood micro-nano fiber suspension in step (2) to a wet pulp state without dripping water, and controlling the solid content of the wood micro-nano fibers to be 35 wt %;
[0027] (4) mixing wood micro-nano fibers, HDPE particles, an additive maleic anhydride grafted polyethylene (MAPE) and polyethylene wax in a mass ratio of 30:63:3:4, placing in a high-speed mixer and stirring at a speed of 8000 r / min for 3 min until the mixture is uniformly blended to obtain a blend;
[0028] (5) placing the blend obtained in step (4) in a twin-screw extruder for melt mixing and extrusion molding, wherein the temperature of the extruder is set to 163° C. and the screw speed is set to 30 rpm; during the extrusion process, water vapor overflows, and vacuum and exhaust are drawn while extruding; obtaining extruded strips, and granulating them to obtain extruded pellets.
[0029] (6) The extruded pellets obtained in (5) are added to an injection molding machine for further molding, and the heating temperature of the injection molding machine is set to 167°C.
[0030] Test method for the bending resistance of wood micro-nano fiber modified plastics: injection molded samples with a length of 80 mm, a width of 10 mm, and a thickness of 4 mm were tested using a universal mechanical testing machine. The bracket span was 64 mm, the pressure rod speed was 2 mm / min, and each sample was tested six times to take the average value.
[0031] Test method for linear thermal expansion coefficient of wood micro-nano fiber modified plastics: Take a sample of 25mm long, 4.5mm wide, and 1mm thick, and test it through a static mechanical thermal analyzer (TMA), tensile mode, nitrogen atmosphere, heating rate of 5℃ / min, loading load set to 0.03N, and test each sample five times. Finally, the linear thermal expansion coefficient is calculated in the temperature range of -30℃ to 60℃, and the average value is taken.
[0032] Through the bending mechanics test, the average bending modulus of the sample in Example 1 reached 2074.9MPa, and the average bending strength reached 43.2MPa, which was 102% higher than that of the high-density polyethylene (HDPE) sample in the control group. Through the static thermomechanical analyzer test, the linear thermal expansion coefficient (CTE) of the sample in Example 1 was 85×10 -6 / K, compared with the control group, the CTE value of HDPE is reduced by half, and the thermal stability and dimensional stability are significantly improved.
[0033] Example 2
[0034] The step (4) in Example 1 is changed to: wood micro-nano fibers, HDPE particles, additive maleic anhydride grafted polyethylene (MAPE) and PE wax are mixed in a mass ratio of 20:73:3:4, placed in a high-speed mixer and stirred at a speed of 5000 r / min for 3 min until the mixture is uniformly blended to obtain a blend; the remaining steps are the same as in Example 1.
[0035] Through the bending mechanics test, the average bending modulus of the sample in Example 2 reached 1648.8MPa, and the average bending strength reached 36.0MPa, which was 68% higher than that of the pure high-density polyethylene sample. Through the static thermomechanical analyzer test, the linear thermal expansion coefficient of the sample in Example 2 was 96×10 -6 / K, compared with the control group, the CTE value of HDPE decreased by 74×10 -6 / K, thermal stability is greatly improved.
[0036] Example 3
[0037] The step (4) in Example 1 is changed to: wood micro-nano fibers, HDPE particles, additive maleic anhydride grafted polyethylene (MAPE) and PE wax are mixed in a mass ratio of 40:53:3:4, placed in a high-speed mixer and stirred at a speed of 5000 r / min for 4 min until the mixture is uniformly blended to obtain a blend; the remaining steps are the same as in Example 1.
[0038] Through the bending mechanics test, the average bending modulus of the sample in Example 3 reached 2478.5MPa, and the average bending strength reached 49.2MPa, which was 130% higher than that of the pure high-density polyethylene sample. Through the static thermomechanical analyzer test, the linear thermal expansion coefficient of the sample in Example 3 was 69×10 -6 / K, compared with the control group, the CTE value of HDPE decreased by 101×10 -6 / K, thermal stability is greatly improved.
[0039] Example 4
[0040] The step (4) in Example 1 is changed to: mix the wood micro-nano fibers, HDPE particles, the additive maleic anhydride grafted polyethylene (MAPE) and PE wax in a mass ratio of 50:43:3:4, place in a high-speed mixer and stir at a speed of 5000 r / min for 4 min until the mixture is uniformly blended to obtain a blend; the remaining steps are the same as in Example 1.
[0041] Through the bending mechanics test, the average bending modulus of the sample of Example 4 reached 3085.2MPa, and the average bending strength reached 53.9MPa, which was 152% higher than that of the pure high-density polyethylene sample. Through the static thermomechanical analyzer test, the linear thermal expansion coefficient of the sample of Example 4 was 59×10 -6 / K, compared with the control group, the CTE value of HDPE decreased by 111×10 -6 / K, the thermal stability is significantly improved.
[0042] like Figure 1 In Example 1, poplar wood shavings are used as raw materials, and the wood micro-nano fibers after defibration are obtained. It can be seen that after mechanical defibration, the micron fibers are effectively unraveled, with nanofiber branches.
[0043] like Figure 2 The figure shows a scanning electron microscope image of the surface fracture of the 30% wood micro-nano fiber modified polyethylene composite material of Example 1. It can be seen that the micro-nano fibers and the plastic are mixed evenly to form a layered assembled structure. During the wet feed extruder screw mixing process, the micro-nano fibers are well oriented in the flowing plastic matrix, which helps to improve the mechanical properties and dimensional stability of the composite material.
[0044] The composite material prepared by the present invention has a significant improvement in flexural strength compared with the polyethylene plastic of the control group, as shown in Figure 3 . Among the composite materials prepared by the present invention, the flexural strength and flexural modulus of the composite materials with 50% micro-nano fibers added reached 53.9Mpa and 3085.2MPa, respectively, which were increased by 152% and 297% respectively compared with the control group high-density polyethylene (HDPE). The flexural strength of the samples with 20%, 30%, and 40% micro-nano fibers added increased by 68%, 102%, and 130% relative to HDPE. Within the scope of the experiment, the composite material with 50% cellulose content has the best flexural performance, which provides an effective preparation method for wood micro-nano fiber modified plastic composite materials.
[0045] The composite material prepared by the present invention has excellent thermal stability, and the thermal expansion performance is significantly improved with the increase of the amount of raw material fiber. Figure 4 The linear thermal expansion coefficient (CTE) of the composite materials with 30% and 50% micro-nano fibers added is 85×10 -6 / K, 59×10 -6 / K, compared with the control group, the CTE value of HDPE dropped by more than half, and the dimensional stability was greatly improved.
[0046] The present invention efficiently utilizes the "wet feed method" to extrude and prepare wood micro-nano fiber modified plastics, solves the fiber agglomeration problem in the production process of wood micro-nano fiber reinforced plastics, greatly enhances the mechanical properties of plastics, and improves their dimensional stability, which can reduce the use of non-renewable petroleum-based plastics and effectively save costs. The method is relatively simple, green and dust-free, and is suitable for assembly line industrial production, making a contribution to the research on the use of natural biomass materials to prepare new modified plastics.
Claims
1. A method for preparing biomass micro-nano fiber directional modified plastics by wet feed extrusion, characterized in that: The steps include: Plastic particles and additives are added to a wet slurry containing biomass micro-nano fibers, and a blend is obtained after stirring, wherein the solid content of the biomass micro-nano fibers in the wet slurry is 25-40wt%; the obtained blend is then melt-mixed and extruded to obtain a biomass micro-nano fiber directional modified plastic.
2. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 1, characterized in that: The method for preparing the wet pulp containing biomass micro-nano fibers comprises: pre-treating the biomass raw material with alkali and washing and swelling it with water to obtain biomass fibers, then crushing, stirring and dispersing the biomass fibers to obtain biomass micro-nano fibers, and then filtering the dispersed suspension to a wet pulp state without dripping water to obtain the wet pulp containing biomass micro-nano fibers.
3. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 2, characterized in that: The biomass raw material is treated in an alkali solution in a water bath for 2 to 6 hours, then soaked at room temperature for 10 to 24 hours, and then taken out and washed with water to neutrality to obtain swollen biomass fibers.
4. The method for preparing biomass micro-nano fiber oriented modified plastic by wet feed extrusion according to claim 3, characterized in that: The concentration of the alkali solution is 1-5 wt %.
5. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 2, characterized in that: The deflagration process includes defibration in a high-speed mixer at a speed of 8000 to 12000 r / min for 3 to 5 minutes.
6. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 1, characterized in that: The diameter of the biomass micro-nano fiber is 100nm-100μm.
7. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 1, characterized in that: In the biomass micro-nano fiber directional modified plastic, the content of plastic particles is 15-95%, the content of auxiliary agent is 2-10%, and the content of biomass micro-nano fiber is 3-75%.
8. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 1, characterized in that: The auxiliary agent includes a coupling agent and / or a lubricant.
9. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 1, characterized in that: The temperature of the extrusion process is controlled at 158-165°C, the screw speed is 20-40rpm, and the extrusion process is carried out while vacuuming and exhausting.
10. The method for preparing biomass micro-nano fiber oriented modified plastics by wet feed extrusion according to claim 1, characterized in that: The plastic particles are thermoplastic plastics, including at least one of polyethylene, polypropylene, nylon, polyvinyl chloride, polyethylene terephthalate, polystyrene, polycarbonate, polymethyl methacrylate, polytetrafluoroethylene, polyetheretherketone, acrylonitrile-styrene-butadiene copolymer, polylactic acid or polybutylene terephthalate; the raw materials for preparing the biomass micro-nano fibers include at least one of wood, bamboo, straw, rice husk, hemp, cotton, coconut shell or sugarcane.
Citation Information
Patent Citations
Composite material
CN102652154A
Method for preparing wood-plastic composite material by using wood fibers
CN105038284A
Method for preparing plant fiber-based foamed thermoplastic masterbatch
CN106280514A
Preparation method of micro-nanocellulose modified wood-plastic composite (WPC)
CN109912875A
Preparation method of micro-nano cellulose reinforced high-density polyethylene composite material
CN112759810A