Degradable and recyclable TPE composite material and preparation method thereof

By adding specific formula ingredients to the TPE composite materials to improve their biodegradation efficiency and mechanical properties, the problem of difficulty in recycling existing TPE composite materials is solved, and environmentally friendly degradation and safety improvement are achieved.

CN119019790APending Publication Date: 2024-11-26GUANGDONG DONGDA TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411158983.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing TPE composite materials are difficult to recycle, resulting in environmental pollution because their polymer compounds are difficult to degrade in the natural environment.

Method used

Using a type of thermoplastic elastomer, polylactic acid, talc, hydrogenated styrene elastomer, antioxidant, cellulose aerogel, compatible flame retardant copolymer, polyolefin grafted maleic anhydride and natural fillers Degradable TPE composites, improving the biodegradation efficiency and mechanical properties of the materials through specific formulations and preparation methods.

Benefits of technology

The good biodegradation efficiency, flexibility, tear resistance, flexibility and flame retardant properties of TPE composite materials are achieved, reducing the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019790A_ABST
    Figure CN119019790A_ABST
Patent Text Reader

Abstract

The invention discloses a degradable and recyclable TPE composite material and a preparation method thereof. Comprising the following raw materials in parts by weight: 6-10 parts of a thermoplastic elastomer, 12-15 parts of polylactic acid, 10-12 parts of talcum powder, 12-25 parts of a hydrogenated styrene elastomer, 2-4 parts of an antioxidant, 3-6 parts of cellulose aerogel, 18-22 parts of a compatible flame-retardant copolymer, 6-12 parts of polyolefin grafted maleic anhydride, 1-3 parts of a stabilizer and 8-35 parts of natural filler. By compounding the carboxymethyl starch, the chitosan derivative, the fetal shell adhesive protein, the water-white rosin and the carboxymethyl starch, the performance is synthesized, and under the auxiliary dissolution of absolute ethyl alcohol and water, the obtained compatilizer can easily form a coating film on the surface of the natural filler, so that the compatibility of the natural filler and the cellulose aerogel is further improved, and the cellulose aerogel is prepared. The obtained TPE composite material has better biodegradation efficiency and better mechanical properties, such as flexibility and tear strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of TPE composite materials, in particular to a degradable and recyclable TPE composite material and a preparation method thereof. Background Art

[0002] As we all know, TPE is a thermoplastic elastomer material with high strength, high resilience, injection molding, wide application range, environmental protection, non-toxic and safe, excellent colorability, soft touch, weather resistance, fatigue resistance and temperature resistance, excellent processing performance, no need for vulcanization, can be recycled to reduce costs, can be secondary injection molding, coated and bonded with PP, PE, PC, PS, ABS and other base materials, or can be molded alone. TPE is widely used in medical, sports equipment, instruments and tools, household daily necessities, food packaging, electronic products, automobiles and other fields.

[0003] However, the TPE composite materials in the prior art are generally difficult to recycle and are usually directly discarded, because TPE materials are difficult to degrade in the natural environment because they are a polymer compound and are not easily decomposed by microorganisms. A large amount of TPE materials accumulate, causing environmental pollution. Therefore, we propose a degradable and recyclable TPE composite material and its preparation method to solve the above-mentioned problems. Summary of the invention

[0004] The object of the present invention is to provide a biodegradable and recyclable TPE composite material and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A biodegradable and recyclable TPE composite material comprises the following raw materials in parts by weight: 6-10 parts of thermoplastic elastomer, 12-15 parts of polylactic acid, 10-12 parts of talc, 12-25 parts of hydrogenated styrene elastomer, 2-4 parts of antioxidant, 3-6 parts of cellulose aerogel, 18-22 parts of compatible flame-retardant copolymer, 6-12 parts of polyolefin grafted maleic anhydride, 1-3 parts of stabilizer and 8-35 parts of natural filler.

[0007] As a further solution of the present invention: the natural filler is a natural filler treated with a compatibilizer, and the compatibilizer includes the following raw materials in parts by weight: 0.5-1 part of carboxymethyl starch, 10-18 parts of water, 2-5 parts of chitosan derivatives, 0.2-0.8 parts of fetal shell mucin, 0.5-1.5 parts of water-white rosin, and 20-30 parts of anhydrous ethanol.

[0008] As a further solution of the present invention: the compatible flame-retardant copolymer comprises the following components in parts by weight: 6-12 parts of lignin, 8-9 parts of coconut shell powder, and 2-6 parts of modified waste rubber powder.

[0009] As a further solution of the present invention: the preparation method of the compatible flame-retardant copolymer comprises the following steps: the first step is to cut the coconut shell into strips with a width of 3-5 mm, immerse the cut coconut shell strips in a sodium hydroxide solution with a volume fraction of 10%, and soak for 2-3 hours, take out the coconut shell strips, rinse with distilled water until neutral, put them into a vacuum drying oven for drying, the drying temperature is 55-65°C, the drying time is 20-25 hours, and then crush them, the mesh size is 45-60 mesh, and coconut shell powder is obtained; the second step is to add the waste rubber powder into a toluene solution and soak it for 24 hours, and at a temperature of 25-35°C, dropwise add a volume fraction of 15% peracetic acid solution, stirring reaction for 3-5h, washing the oxidatively modified rubber powder with acetic acid solution for 1-2 times, and then washing with distilled water until neutral, putting it into a vacuum drying oven for drying, the drying temperature is 55-60°C, the drying time is 3-5h, and modified waste rubber powder is obtained; the third step is to mix lignin, coconut shell powder and modified waste rubber powder evenly, melt blend the mixture at a temperature of 150-250°C, melt the blend at a temperature of 160-250°C, and inject the obtained mixture into a long strip mold, the mold temperature is 22-52°C, and cool to obtain a compatible flame retardant copolymer.

[0010] As a further solution of the present invention: the polyolefin grafted with maleic anhydride is one or more of high-density polyethylene grafted with maleic anhydride and linear low-density polypropylene grafted with maleic anhydride.

[0011] As a further solution of the present invention: the natural filler is one or more of wine lees powder, jute fiber powder, banana fiber powder and corn silk powder.

[0012] As a further solution of the present invention: the natural filler is composed of wine lees powder and jute fiber powder in a weight ratio of 1: (1-2.2), or is composed of banana fiber powder and corn silk powder in a weight ratio of 1: (0.6-1.3).

[0013] As a further embodiment of the present invention: the natural filler is composed of distiller's grains powder, jute fiber powder, and banana fiber powder in a weight ratio of 1: (1-2.8): (2.3-4.4), or is composed of distiller's grains powder, jute fiber powder, and corn silk powder in a weight ratio of 1: (1.2-2.1): (1.3-3.2).

[0014] As a further solution of the present invention: the natural filler is composed of wine lees powder, jute fiber powder, corn silk powder and banana fiber powder in a weight ratio of 1: (0.6-1.2): (1.3-1.8): (1.5-2.5).

[0015] A method for preparing a degradable and recyclable TPE composite material comprises the following steps:

[0016] Step 1: weigh the natural filler and the cellulose aerogel in proportion, stir and react at a temperature of 125-135° C. for 3-5 hours to obtain a mixture;

[0017] Step 2: Weigh the remaining thermoplastic elastomer, polylactic acid, talcum powder, hydrogenated styrene elastomer, antioxidant, compatible flame retardant copolymer, polyolefin grafted maleic anhydride, stabilizer and other materials in proportion, and stir and blend them with the mixture obtained in step 1 to obtain a uniform mixture;

[0018] Step 3: The uniformly mixed material obtained in step 2 is transferred to an extruder for extrusion, and then granulated by a granulator to obtain a biodegradable and recyclable TPE composite material.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The degradable and recyclable TPE composite material and preparation method thereof are compounded by carboxymethyl starch, chitosan derivatives, fetal shell mucin, water white rosin and carboxymethyl starch, and their properties are integrated. Under the auxiliary dissolution of anhydrous ethanol and water, the obtained compatibilizer is easy to form a coating film on the surface of the natural filler, thereby further improving the compatibility of the natural filler and the cellulose aerogel, so that the obtained TPE composite material has better biodegradation efficiency and better mechanical properties, such as softness and tearing strength.

[0021] The biodegradable and recyclable TPE composite material and preparation method thereof improve the compatibility of each component, enhance the flexibility and wear resistance of the composite material, and make the composite material have good flame retardancy, thereby improving product safety, by adding a compatible flame retardant copolymer into the TPE composite material; in the compatible flame retardant copolymer, lignin, coconut shell powder and modified waste rubber powder form a compatibilizer; the hydrophilic coconut shell powder forms hydrogen bonds with the surface of lignin and is coated on the surface of its particles, thereby reducing the surface tension of lignin; the modified waste rubber powder is a non-polar substance, and is compatible with a polylactic acid matrix according to the principle of "like dissolves like", thereby promoting the dispersion of lignin in the matrix, effectively improving the interface compatibility between the copolymer and the matrix, thereby improving and optimizing properties such as toughness and strength, effectively enhancing flexibility and wear resistance, and also improving the flame retardancy of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The figure is a schematic flow chart of a method for preparing a degradable and recyclable TPE composite material according to the present invention. DETAILED DESCRIPTION

[0023] In one embodiment, Figure 1As shown, a biodegradable and recyclable TPE composite material includes the following raw materials in parts by weight: 6-10 parts of thermoplastic elastomer, 12-15 parts of polylactic acid, 10-12 parts of talc, 12-25 parts of hydrogenated styrene elastomer, 2-4 parts of antioxidant, 3-6 parts of cellulose aerogel, 18-22 parts of compatible flame retardant copolymer, 6-12 parts of polyolefin grafted maleic anhydride, 1-3 parts of stabilizer, and 8-35 parts of natural filler;

[0024] By compounding carboxymethyl starch, chitosan derivatives, fetal shell mucin, water-white rosin, and carboxymethyl starch, and combining their properties, and with the auxiliary dissolution of anhydrous ethanol and water, the obtained compatibilizer can easily form a coating film on the surface of the natural filler, thereby further improving the compatibility of the natural filler with the cellulose aerogel, so that the obtained TPE composite material has better biodegradation efficiency and better mechanical properties, such as softness and tear strength.

[0025] The compatible flame-retardant copolymer comprises the following components in parts by weight: 6-12 parts of lignin, 8-9 parts of coconut shell powder, and 2-6 parts of modified waste rubber powder;

[0026] The preparation method of the compatible flame-retardant copolymer comprises the following steps: the first step is to cut the coconut shell into strips with a width of 3-5 mm, immerse the cut coconut shell strips in a sodium hydroxide solution with a volume fraction of 10%, and the immersion time is 2-3 hours, take out the coconut shell strips, rinse them with distilled water until they are neutral, put them into a vacuum drying oven for drying, the drying temperature is 55-65°C, the drying time is 20-25 hours, and then crush them, the mesh size is 45-60 mesh, and coconut shell powder is obtained; the second step is to add the waste rubber powder into a toluene solution and immerse it for 24 hours, and drop 15% peroxide with a volume fraction at a temperature of 25-35°C. Acid solution, stirring reaction for 3-5h, washing the oxidized modified rubber powder with acetic acid solution for 1-2 times, and then washing with distilled water until neutral, putting it into a vacuum drying oven for drying, the drying temperature is 55-60℃, the drying time is 3-5h, and modified waste rubber powder is obtained; the third step, lignin, coconut shell powder and modified waste rubber powder are mixed evenly, the mixed materials are melted and blended at a temperature of 150-250℃, the blend is melted at a temperature of 160-250℃, and the obtained mixture is injected into a long strip mold, the mold temperature is 22-52℃, and cooled to obtain a compatible flame retardant copolymer;

[0027] The weight ratio of the coconut shell strips to the sodium hydroxide solution is 1:9-9.5, the weight ratio of the waste rubber powder to the toluene solution is 1:6-8, and the weight ratio of the waste rubber powder to the peracetic acid solution is 1:3-4.

[0028] By adding compatible flame-retardant copolymers into TPE composite materials, the compatibility of each component is improved, the flexibility and wear resistance of the composite materials are enhanced, and the composite materials have good flame retardancy, thereby improving product safety; in the compatible flame-retardant copolymers, lignin, coconut shell powder and modified waste rubber powder form a compatibilizer, the hydrophilic coconut shell powder forms hydrogen bonds with the surface of lignin and coats the surface of its particles, reducing the surface tension of lignin, and the modified waste rubber powder is a non-polar substance, which is compatible with the polylactic acid matrix according to the "like dissolves like" principle, promotes the dispersion of lignin in the matrix, effectively improves the interface compatibility between the copolymer and the matrix, thereby improving and optimizing properties such as toughness and strength, effectively enhancing flexibility and wear resistance, and also improving the flame retardant properties of the composite materials.

[0029] The polyolefin grafted maleic anhydride is one or more of high-density polyethylene grafted maleic anhydride and linear low-density polypropylene grafted maleic anhydride; the natural filler is one or more of vinasse powder, jute fiber powder, banana fiber powder and corn silk powder; the natural filler is composed of vinasse powder and jute fiber powder in a weight ratio of 1: (1-2.2), or of banana fiber powder and corn silk powder in a weight ratio of 1: (0.6-1.3); the natural filler is vinasse powder, jute fiber powder, banana fiber powder, corn silk powder, etc. The natural filler is composed of vinasse powder, jute fiber powder, and banana fiber powder in a weight ratio of 1: (1-2.8): (2.3-4.4), or vinasse powder, jute fiber powder, and corn silk powder in a weight ratio of 1: (1.2-2.1): (1.3-3.2); the natural filler is composed of vinasse powder, jute fiber powder, corn silk powder, and banana fiber powder in a weight ratio of 1: (0.6-1.2): (1.3-1.8): (1.5-2.5);

[0030] The natural filler is a natural filler treated with a compatibilizer, and the compatibilizer comprises the following raw materials in parts by weight: 0.5-1 part of carboxymethyl starch, 10-18 parts of water, 2-5 parts of chitosan derivatives, 0.2-0.8 parts of fetal shell mucin, 0.5-1.5 parts of water-white rosin, and 20-30 parts of anhydrous ethanol; the chitosan derivative is one or more of carboxymethyl chitosan, chitosan-sodium alginate complex, and chitosan-polyethylene glycol copolymer; the usage ratio of carboxymethyl chitosan, chitosan-sodium alginate complex, and chitosan-polyethylene glycol copolymer is 1: (0.3-0.8): (1-2);

[0031] The method for treating a natural filler with a compatibilizer comprises: weighing fetal mucin in parts by weight, dissolving it in water, heating it to 65-80°C, adding carboxymethyl starch and stirring for 10-20 minutes to obtain a first mixture; weighing water white rosin and chitosan derivatives and dissolving them in anhydrous ethanol to obtain a second mixture; adding all of the first mixture to the second mixture in parts by weight, stirring for 35-50 minutes, then adding the natural filler, stirring for 10-20 minutes, heating it to 100°C, and performing reduced pressure distillation for 30-40 minutes, drying the obtained solid, crushing it, and sieving it through 120-130 meshes to obtain the natural filler treated with a compatibilizer.

[0032] A method for preparing a degradable and recyclable TPE composite material comprises the following steps:

[0033] Step 1: weigh the natural filler and the cellulose aerogel in proportion, stir and react at a temperature of 125-135° C. for 3-5 hours to obtain a mixture;

[0034] Step 2: Weigh the remaining thermoplastic elastomer, polylactic acid, talcum powder, hydrogenated styrene elastomer, antioxidant, compatible flame retardant copolymer, polyolefin grafted maleic anhydride, stabilizer and other materials in proportion, and stir and blend them with the mixture obtained in step 1 to obtain a uniform mixture;

[0035] Step 3: The uniformly mixed material obtained in step 2 is transferred to an extruder for extrusion, and then granulated by a granulator to obtain a biodegradable and recyclable TPE composite material.

[0036] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A degradable and recyclable TPE composite material, characterized in that: The invention comprises the following raw materials in parts by weight: 6-10 parts of thermoplastic elastomer, 12-15 parts of polylactic acid, 10-12 parts of talc, 12-25 parts of hydrogenated styrene elastomer, 2-4 parts of antioxidant, 3-6 parts of cellulose aerogel, 18-22 parts of compatible flame-retardant copolymer, 6-12 parts of polyolefin grafted maleic anhydride, 1-3 parts of stabilizer and 8-35 parts of natural filler.

2. The degradable and recyclable TPE composite material according to claim 1, characterized in that: The natural filler is a natural filler treated with a compatibilizer, and the compatibilizer comprises the following raw materials in parts by weight: 0.5-1 part of carboxymethyl starch, 10-18 parts of water, 2-5 parts of chitosan derivatives, 0.2-0.8 parts of fetal shell mucin, 0.5-1.5 parts of water-white rosin, and 20-30 parts of anhydrous ethanol.

3. The degradable and recyclable TPE composite material according to claim 1, characterized in that: The compatible flame-retardant copolymer comprises the following components in parts by weight: 6-12 parts of lignin, 8-9 parts of coconut shell powder, and 2-6 parts of modified waste rubber powder.

4. The biodegradable and recyclable TPE composite material according to claim 3, characterized in that: The preparation method of the compatible flame-retardant copolymer comprises the following steps: the first step is to cut the coconut shell into strips with a width of 3-5 mm, immerse the cut coconut shell strips in a sodium hydroxide solution with a volume fraction of 10% for 2-3 hours, take out the coconut shell strips, rinse them with distilled water until they are neutral, put them into a vacuum drying oven for drying at a drying temperature of 55-65° C. for 20-25 hours, then crush them with a sieve aperture of 45-60 meshes to obtain coconut shell powder; the second step is to add the waste rubber powder into a toluene solution and immerse it for 24 hours, dropwise add a peroxide solution with a volume fraction of 15% at a temperature of 25-35° C., and pulverize the waste rubber powder. Acetic acid solution, stirring reaction for 3-5h, washing the oxidized modified rubber powder with acetic acid solution for 1-2 times, and then washing with distilled water until neutral, putting it into a vacuum drying oven for drying, the drying temperature is 55-60℃, the drying time is 3-5h, and modified waste rubber powder is obtained; the third step, lignin, coconut shell powder and modified waste rubber powder are mixed evenly, the mixture is melted at a temperature of 150-250℃, the blend is melted at a temperature of 160-250℃, and the obtained mixture is injected into a long strip mold, the mold temperature is 22-52℃, and cooled to obtain a compatible flame retardant copolymer.

5. The degradable and recyclable TPE composite material according to claim 1, characterized in that: The polyolefin grafted with maleic anhydride is one or more of high-density polyethylene grafted with maleic anhydride and linear low-density polypropylene grafted with maleic anhydride.

6. The biodegradable and recyclable TPE composite material according to claim 1, characterized in that: The natural filler is one or more of wine lees powder, jute fiber powder, banana fiber powder and corn silk powder.

7. The biodegradable and recyclable TPE composite material according to claim 6, characterized in that: The natural filler is composed of wine lees powder and jute fiber powder in a weight ratio of 1: (1-2.2), or of banana fiber powder and corn silk powder in a weight ratio of 1: (0.6-1.3).

8. The biodegradable and recyclable TPE composite material according to claim 6, characterized in that: The natural filler is composed of distiller's grains powder, jute fiber powder and banana fiber powder in a weight ratio of 1:(1-2.8):(2.3-4.4), or is composed of distiller's grains powder, jute fiber powder and corn silk powder in a weight ratio of 1:(1.2-2.1):(1.3-3.2).

9. The biodegradable and recyclable TPE composite material according to claim 6, characterized in that: The natural filler is composed of wine lees powder, jute fiber powder, corn silk powder and banana fiber powder in a weight ratio of 1: (0.6-1.2): (1.3-1.8): (1.5-2.5).

10. A method for preparing a biodegradable and recyclable TPE composite material, characterized in that: Applicable to the TPE composite material according to any one of claims 1 to 9, the preparation method comprises the following steps: Step 1: weigh the natural filler and the cellulose aerogel in proportion, stir and react at a temperature of 125-135° C. for 3-5 hours to obtain a mixture; Step 2: Weigh the remaining thermoplastic elastomer, polylactic acid, talcum powder, hydrogenated styrene elastomer, antioxidant, compatible flame retardant copolymer, polyolefin grafted maleic anhydride, stabilizer and other materials in proportion, and stir and blend them with the mixture obtained in step 1 to obtain a uniform mixture; Step 3: The uniformly mixed material obtained in step 2 is transferred to an extruder for extrusion, and then granulated by a granulator to obtain a biodegradable and recyclable TPE composite material.

Citation Information

Cited By

  • Degradable mobile phone protective film and preparation method thereof

    CN120424483A