First composite material and second composite material containing same

By using the heat-resistant composite material prepared by the first ethylene lactide copolymer and ammonium polyphosphate, temporary plug particles with high sealing strength and good dissolution performance are formed, and the dissolution effect of existing temporary plugging agents in medium-temperature oil and gas fields is solved. The problem of optimal and construction complexity achieves effective sealing and simplified construction under medium temperature conditions.

CN119019827AActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310602801.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

When used in medium-temperature oil and gas fields, the dissolution effect of dissolution type temporary plugging agent is greatly affected by the mineralization degree and water volume of water, which may cause a well blockage accident when it cannot be dissolved, and the construction complexity is high, which increases costs.

Method used

Made of the first composite material from the first ethylene lactide copolymer and ammonium polyphosphate, the heat-resistant cylindrical wire is formed by extruding strips and cooling, and temporary plug particles are prepared by the second composite material of the leather core structure. , has good low temperature degradation and dissolution performance and high sealing strength.

Benefits of technology

It achieves good dissolution effect and high sealing strength in water scarce environments, reduces the requirements for underground water bodies, simplifies the construction process, and avoids the occurrence of well clogging accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019827A_ABST
    Figure CN119019827A_ABST
Patent Text Reader

Abstract

The invention provides a first composite material and a second composite material containing the same. The first composite material provided by the invention is prepared from a first glycolide-lactide copolymer and ammonium polyphosphate, can be directly extruded to form a brace, and is rolled after being cooled to form a cylindrical wire rod with good heat resistance; the second composite material provided by the invention has a skin-core structure, the first composite material is used as a core layer material, and a second glycolide-lactide copolymer is used as a skin layer material; the temporary plugging particles obtained by physically pelletizing the second composite material in the direction perpendicular to the axial direction of the cylinder have excellent low-temperature degradation dissolving performance, good dissolving effect in a water-deficient environment and high plugging strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of natural gas production increase, and in particular relates to a first composite material and a second composite material containing the first composite material. Background Art

[0002] At present, temporary plugging and diversion fracturing technology has become an important technical approach to increase production in oil and gas fields. Temporary plugging and diversion fracturing technology is to add temporary plugging agents to the working fluid or sand mixer during fracturing construction to temporarily plug old fractures or fractures with added sand, and force the fluid to divert through changes in rupture pressure and fracture extension pressure, thereby creating new fractures. Temporary plugging agents are used to temporarily plug fractures with added sand, so that repeated fractures deviate and divert relative to the original fracture orientation, thereby achieving the purpose of communicating with reservoirs with low or even unused levels. Temporary plugging and diversion fracturing technology can not only produce the effect of increasing oil and gas, but also change the direction of water drive to a certain extent and improve the utilization rate of injected water.

[0003] Common temporary plugging agents can be divided into dissolving temporary plugging agents and degradable temporary plugging agents according to the way in which their plugging fails. Dissolving temporary plugging agents refer to a type of temporary plugging agent that can dissolve in water under specific conditions to form a temporary plugging agent solution, thereby rendering the plugging ineffective. The dissolution effect of this type of temporary plugging agent is greatly affected by the mineralization of the water body, the amount of water, and the water temperature. Moreover, the so-called dissolution is not degradation, which can easily cause environmental pollution. Degradable temporary plugging agents refer to macromolecules that can break chains and degrade into small molecules under specific water environments, and finally dissolve in water, thereby rendering the plugging ineffective. Typical degradable temporary plugging agents include polyglycolic acid, polylactic acid, etc. Moreover, most degradable temporary plugging agents can be decomposed by microorganisms into non-toxic and harmless substances such as carbon dioxide and water after degradation. This type of temporary plugging agent is increasingly favored due to its excellent degradation adaptability (the degradation effect is relatively less affected by the mineralization of the water body) and environmental protection characteristics.

[0004] However, currently, the temporary plugging agents widely used in medium-temperature oil and gas fields with well temperatures ranging from 60°C to 90°C are mostly soluble temporary plugging agents (common ones are polyacrylamide, water-soluble polyacrylic acid, etc.), which require a large amount of water environment or a special mineralization environment during the dissolution process (some temporary plugging agents cannot be dissolved under high mineralization). However, the actual situation underground is extremely complicated. In some cases, the temporary plugging agent may not be able to contact a large amount of water environment or the surrounding water body has a high mineralization, which may cause the temporary plugging agent to be unable to dissolve, resulting in accidents such as well plugging.

[0005] During the use of temporary plugging agents, it is necessary to accurately survey the cracks that are planned to be plugged, and then select the appropriate particle size according to the width of the cracks. But in fact, the width of the cracks often varies, which also brings difficulties to the selection of the particle size of the temporary plugging agent, and easily leads to the waste of temporary plugging agents. In addition, in order to achieve a relatively high strength plugging of temporary plugging agents, it is often necessary to use rigid temporary plugging agents and flexible temporary plugging agents in combination, such as using rigid temporary plugging agents and flexible temporary plugging agents to inject them into the well in sequence, but this construction method also further increases the complexity of construction and increases construction costs. In addition, the flexible temporary plugging materials used are all dissolving temporary plugging agents, which are prone to well plugging accidents when used for gas well fracturing.

[0006] Therefore, it is necessary to find a high-strength temporary plugging agent that is simple to construct, has strong adaptability to cracks, has low requirements for underground water bodies, and is environmentally friendly. Summary of the invention

[0007] A first aspect of the present invention provides a first composite material comprising a first ethylene-lactide copolymer and ammonium polyphosphate.

[0008] According to a specific embodiment of the present invention, the mass ratio of the first lactide-ethylene glycol copolymer to ammonium polyphosphate is (2 to 4):1.

[0009] According to a specific embodiment of the present invention, the first glycolide-lactide copolymer is obtained by copolymerizing glycolide and lactide in a molar ratio of 85:15; and / or

[0010] The weight average molecular weight of the first ethylene-lactide copolymer is greater than 50,000;

[0011] Preferably, the weight average molecular weight of the first ethylene-lactide copolymer is 50,000 to 100,000.

[0012] According to a specific embodiment of the present invention, the degree of polymerization of the ammonium polyphosphate is 1000 to 1200.

[0013] The second aspect of the present invention provides a method for preparing the first composite material according to the first aspect of the present invention, comprising the following steps:

[0014] 1) mixing the first lactide-ethylene glycol copolymer and ammonium polyphosphate and granulating the mixture to obtain an intermediate material;

[0015] 2) Extruding the intermediate material into a strip, and rolling it up after cooling to obtain the first composite material.

[0016] According to a specific embodiment of the present invention, in step 1), the granulation is performed by a twin-screw granulator;

[0017] Preferably, the granulation conditions are melt extrusion granulation at 170°C to 190°C; and / or

[0018] The speed of the twin-screw granulator screw is 200r / min; and / or

[0019] The intermediate material is cylindrical particles with an average diameter of 3 mm and an average height of 3 mm.

[0020] According to a specific embodiment of the present invention, in step 2), the extrusion drawing is performed by a 3D printing wire machine;

[0021] Preferably, the intermediate material is extruded into a strip at 175°C to 190°C; and / or

[0022] Setting the wire diameter of the 3D printing wire machine to 1mm to 2mm; and / or

[0023] The screw speed of the 3D printing wire machine is 80r / min;

[0024] Preferably, the intermediate material is extruded into a strand and then cooled to room temperature (25° C.) for winding.

[0025] The third aspect of the present invention provides a second composite material having a skin-core structure; the material of the core layer of the skin-core structure is the first composite material; the material of the skin layer of the skin-core structure is the second ethylene-lactide copolymer;

[0026] The first composite material is the first composite material described in the first aspect of the present invention or the first composite material prepared by the method described in the second aspect of the present invention.

[0027] According to a specific embodiment of the present invention, the second glycolide-lactide copolymer is obtained by copolymerizing glycolide and lactide in a molar ratio of (30 to 70): (70 to 30); and / or

[0028] The weight average molecular weight of the second ethylene-lactide copolymer is 30,000 to 50,000;

[0029] Preferably, the second glycolide-lactide copolymer is obtained by copolymerizing glycolide and lactide in a molar ratio of 50:50.

[0030] According to a specific embodiment of the present invention, the second composite material is a cylindrical composite material having the skin-core structure;

[0031] Preferably, the core layer in the skin-core structure is a cylinder with a diameter of 1 mm to 2 mm; and / or

[0032] The thickness of the skin layer in the skin-core structure is 0.5 mm to 1 mm.

[0033] The fourth aspect of the present invention provides a method for preparing the second composite material as described in the third aspect of the present invention, comprising the following steps:

[0034] The second ethylene-lactide copolymer is coated on the surface of the core layer, pulled, and cooled to obtain the second composite material.

[0035] According to a specific embodiment of the present invention, the coating and pulling are achieved by a wire extruder;

[0036] Preferably, the temperature of the wire extruder hopper is 110° C. to 130° C.; and / or

[0037] The speed of the screw of the wire extruder is not higher than 400r / min; and / or the pulling speed is not higher than 200r / min;

[0038] Preferably, the temperature of the wire extruder hopper is 120°C to 130°C; and / or

[0039] The cooling is cooling to room temperature (25° C.); and / or

[0040] The pulling speed of the wire extruder is 60r / min.

[0041] According to a specific embodiment of the present invention, the second composite material is pelletized along a direction perpendicular to the axial direction of the cylinder to obtain temporary plugging particles;

[0042] Preferably, the temporary plugging particles are cylindrical, with a diameter of 2 mm to 4 mm; and / or a height of 3 mm to 5 mm;

[0043] Preferably, the temporary plugging particles have a diameter of 2.5 mm to 4 mm.

[0044] Application of any one of the first composite material described in the first aspect of the present invention, the first composite material prepared by the method described in the second aspect of the present invention, the second composite material described in the third aspect of the present invention, and the second composite material prepared by the method described in the fourth aspect of the present invention in the field of natural gas production enhancement technology, especially in temporary plugging and diversion fracturing. Beneficial effects of the present invention:

[0045] In view of the problems of poor adaptability to fractures, high requirements for underground water bodies, environmental pollution and complex construction of temporary plugging agents in the prior art, the present invention provides a first composite material and a second composite material containing the same. The first composite material provided by the present invention is prepared from a first ethylene-lactide copolymer and ammonium polyphosphate. The setting of the copolymerization molar ratio of glycolide and lactide in the first ethylene-lactide copolymer and the addition of ammonium polyphosphate enable the first composite material to be directly extruded into strands, which can be rolled up after cooling to form a cylindrical wire with good heat resistance; the second composite material provided by the present invention has a skin-core structure, with the first composite material as the core material and the second ethylene-lactide copolymer as the skin material; the temporary plugging particles obtained by physically pelletizing the second composite material in a direction perpendicular to the axial direction of the cylinder have excellent The temporary plugging particles have excellent low-temperature degradation and solubility performance, good dissolution effect in a water-deficient environment, and high plugging strength: the standard dissolution rate and water-deficient dissolution rate of the temporary plugging particles at 60°C are 80.3% to 96.5% and 71.5% to 90.7%, respectively; the standard dissolution rate and water-deficient dissolution rate at 90°C are 96.4% to 99.6% and 91.3% to 99.2%, respectively; the plugging strength for 1mm wide cracks is 40 to 50MPa, and the plugging strength for 2mm wide cracks is 33 to 45MPa, achieving effective plugging in temporary plugging and diverting fracturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is a schematic diagram of the skin-core structure of temporary plugging particles of the second composite material provided by the present invention, wherein 1 is the skin layer, and 2 is the core layer.

[0047] Figure 2 It is a top view of temporary plugging particles made of the second composite material provided by the present invention.

[0048] Figure 3 It is a cross-sectional view of a temporary plugging particle of the second composite material provided by the present invention, wherein h is the height of the temporary plugging particle, d2 is the diameter of the temporary plugging particle, d1 is the diameter of the core layer in the temporary plugging particle, and δ is the thickness of the skin layer in the temporary plugging particle. DETAILED DESCRIPTION

[0049] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.

[0050] The 3D printing wire machine used in the present invention was purchased from Guangzhou Sanhuiying Machinery Equipment Co., Ltd., model LXSJ45;

[0051] The wire extruder used in the present invention is purchased from Dongguan Maoxingsheng Machinery Equipment Co., Ltd., and the model is MXS50.

[0052] Example 1

[0053] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 100,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-10;

[0054] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0055] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 70:30, with a weight average molecular weight of 30,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG3070-3;

[0056] Preparation of the first composite material:

[0057] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 2:1, and melt-extruded and granulated them at 170° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0058] 2) The wire diameter of the 3D printing wire machine is set to 2 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 175° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 2 mm.

[0059] Preparation of the second composite material and temporary plugging particles:

[0060] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 125° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 r / min, while the screw speed of the wire extruder was controlled to 50 r / min to control the thickness of the skin to 1 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 2 mm and a skin layer thickness of 1 mm;

[0061] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the cylindrical axis with a specification of 3 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 2 mm and a skin layer thickness of 1 mm, with a diameter of 4 mm and a height of 3 mm.

[0062] Example 2

[0063] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0064] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0065] The second glycolide-lactide copolymer used in this example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 60:40, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG4060-5;

[0066] Preparation of the first composite material:

[0067] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 2:1, and melt-extruding and granulating the mixture in a twin-screw granulator at a screw speed of 200 r / min at 190° C. to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0068] 2) The wire diameter of the 3D printing wire machine is set to 2 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 190° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 2 mm.

[0069] Preparation of the second composite material and temporary plugging particles:

[0070] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 130° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 23 r / min to control the thickness of the skin to 0.5 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 2 mm and a skin layer thickness of 0.5 mm;

[0071] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the cylindrical axis with a specification of 3 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 2 mm and a skin layer thickness of 0.5 mm, with a diameter of 3 mm and a height of 3 mm.

[0072] Example 3

[0073] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0074] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0075] The second glycolide-lactide copolymer used in this example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 60:40, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG4060-5;

[0076] Preparation of the first composite material:

[0077] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 180° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0078] 2) The wire diameter of the 3D printing wire machine is set to 1 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 180° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1 mm.

[0079] Preparation of the second composite material and temporary plugging particles:

[0080] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 130° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30 r / min to control the thickness of the skin to 1 mm, and cooled to room temperature to obtain a second composite material with a core layer diameter of 1 mm and a skin layer thickness of 1 mm;

[0081] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the cylindrical axis with a specification of 3 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 1 mm and a skin layer thickness of 1 mm, with a diameter of 3 mm and a height of 3 mm.

[0082] Example 4

[0083] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-5;

[0084] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0085] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0086] Preparation of the first composite material:

[0087] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 180° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0088] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 180° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0089] Preparation of the second composite material and temporary plugging particles:

[0090] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 40 r / min to control the thickness of the skin to 1 mm, and cooled to room temperature 40 r / min to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 1 mm;

[0091] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the axial direction of the cylinder with a specification of 3 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 1 mm, with a diameter of 3.5 mm and a height of 3 mm.

[0092] Example 5

[0093] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0094] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0095] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 40:60, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG6040-5;

[0096] Preparation of the first composite material:

[0097] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0098] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 180° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0099] Preparation of the second composite material and temporary plugging particles:

[0100] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 130° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 40 r / min to control the thickness of the skin to 1 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 1 mm;

[0101] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the axial direction of the cylinder with a specification of 3 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 1 mm, with a diameter of 3.5 mm and a height of 3 mm.

[0102] Example 6

[0103] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0104] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0105] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0106] Preparation of the first composite material:

[0107] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0108] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 175° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0109] Preparation of the second composite material and temporary plugging particles:

[0110] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30.5 r / min to control the thickness of the skin to 0.8 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm;

[0111] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the axial direction of the cylinder with a specification of 3 mm to obtain cylindrical temporary plugging particles made of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm, with a diameter of 3.1 mm and a height of 3 mm.

[0112] Example 7

[0113] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0114] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0115] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0116] Preparation of the first composite material:

[0117] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 3:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0118] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 175° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0119] Preparation of the second composite material and temporary plugging particles:

[0120] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30.5 r / min to control the thickness of the skin to 0.8 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm;

[0121] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the axial direction of the cylinder with a specification of 3 mm to obtain cylindrical temporary plugging particles made of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm, with a diameter of 3.1 mm and a height of 3 mm.

[0122] Example 8

[0123] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0124] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0125] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0126] Preparation of the first composite material:

[0127] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0128] 2)) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 175°C in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25°C) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0129] Preparation of the second composite material and temporary plugging particles:

[0130] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30.5 r / min to control the thickness of the skin to 0.8 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm;

[0131] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the cylindrical axis with a specification of 5 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm, with a diameter of 3.1 mm and a height of 5 mm.

[0132] Example 9

[0133] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 100,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-10;

[0134] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0135] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0136] Preparation of the first composite material:

[0137] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0138] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 175° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0139] Preparation of the second composite material and temporary plugging particles:

[0140] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 17.5 r / min to control the thickness of the skin to 0.5 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.5 mm;

[0141] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the cylindrical axis with a specification of 3 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.5 mm, which were 2.5 mm in diameter and 3 mm in height.

[0142] Example 10

[0143] The first glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0144] The ammonium polyphosphate used in this embodiment was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0145] The second glycolide-lactide copolymer used in this embodiment is a regular cylindrical particle formed by copolymerization of glycolide and lactide in a molar ratio of 30:70, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG7030-5;

[0146] Preparation of the first composite material:

[0147] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0148] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 175° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0149] Preparation of the second composite material and temporary plugging particles:

[0150] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this embodiment was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30.5 r / min to control the thickness of the skin to 0.8 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm;

[0151] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the axial direction of the cylinder with a specification of 3 mm to obtain cylindrical temporary plugging particles made of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm, with a diameter of 3.1 mm and a height of 3 mm.

[0152] Comparative Example 1

[0153] The first glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 90:10, with a weight average molecular weight of 100,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1090-10;

[0154] The ammonium polyphosphate used in this comparative example was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0155] The second glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0156] Preparation of the first composite material:

[0157] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 190° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0158] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 190° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0159] Preparation of the second composite material and temporary plugging particles:

[0160] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this comparative example was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30.4 r / min to control the thickness of the skin to 0.8 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm;

[0161] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the cylindrical axis with a specification of 5 mm to obtain cylindrical temporary plugging particles of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm, with a diameter of 3.1 mm and a height of 5 mm.

[0162] Comparative Example 2

[0163] The first glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 80:20, with a weight average molecular weight of 100,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG2080-10;

[0164] The ammonium polyphosphate used in this comparative example was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 1000 to 1200 and a model number of XYL1000;

[0165] The second glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0166] Preparation of the first composite material:

[0167] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0168] 2) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 190° C. in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0169] Preparation of the second composite material and temporary plugging particles:

[0170] The second ethylene-lactide copolymer was put into the feeding hopper of a wire extruder set at a heating temperature of 110°C as the skin material, and the cylindrical first composite material prepared in this comparative example was passed through the threading hole of the wire extruder as the core material and pulled at a speed of 60m / min. At the same time, the screw speed of the wire extruder was controlled to 30.5r / min. However, because the core layer material was not heat-resistant, effective traction could not be formed, and the second composite material with a skin-core structure could not be obtained, and temporary plugging particles could not be obtained.

[0171] Comparative Example 3

[0172] The first glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0173] The nucleating agent used in this comparative example is TMC-300, purchased from Shanxi Chemical Research Institute Co., Ltd.

[0174] The second glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0175] Preparation of the first composite material:

[0176] 1) mixing the first ethylene-lactide copolymer and the nucleating agent in a mass ratio of 99:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0177] 2)) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the intermediate material obtained in step 1) is extruded into a strip at 175°C in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25°C) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0178] Preparation of the second composite material and temporary plugging particles:

[0179] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this comparative example was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30.5 r / min to control the thickness of the skin to 0.8 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm;

[0180] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the axial direction of the cylinder with a specification of 3 mm to obtain cylindrical temporary plugging particles made of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm, with a diameter of 3.1 mm and a height of 3 mm.

[0181] Comparative Example 4

[0182] The first glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0183] The ammonium polyphosphate used in this comparative example was purchased from Dongguan Xingyuan Chemical Co., Ltd., with a degree of polymerization of 20 to 100 and a model number of XYL70;

[0184] The second glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0185] Preparation of the first composite material:

[0186] 1) mixing the first ethylene-lactide copolymer and ammonium polyphosphate in a mass ratio of 4:1, and melt-extruded and granulated them at 175° C. in a twin-screw granulator at a screw speed of 200 r / min to obtain an intermediate material, which is a cylindrical granule with an average diameter of 3 mm and an average height of 3 mm;

[0187] 2) The wire diameter of the 3D printing wire machine was set to 1.5 mm, and then the intermediate material obtained in step 1) was extruded into a strip at 175°C in the 3D printing wire machine at a screw speed of 80 r / min, and then rolled up after cooling to room temperature (25°C) to obtain a cylindrical first composite material with a diameter of 1.5 mm. However, the first composite material was easily broken during the rolling process.

[0188] Preparation of the second composite material and temporary plugging particles:

[0189] The second ethylene-lactide copolymer was put into the feeding hopper of the wire extruder set at a heating temperature of 120° C. as the skin material, and the cylindrical first composite material prepared in this comparative example was passed through the threading hole of the wire extruder as the core material, and was pulled at a speed of 60 m / min, while the screw speed of the wire extruder was controlled to 30.5 r / min to control the thickness of the skin to 0.8 mm, and cooled to room temperature (25° C.) to obtain a second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm;

[0190] The obtained second composite material was pelletized with a pelletizer in a direction perpendicular to the axial direction of the cylinder with a specification of 3 mm to obtain cylindrical temporary plugging particles made of the second composite material with a core layer diameter of 1.5 mm and a skin layer thickness of 0.8 mm, with a diameter of 3.1 mm and a height of 3 mm.

[0191] Comparative Example 5

[0192] The first glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0193] The second glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0194] Preparation of the first composite material:

[0195] 1) The wire diameter of the 3D printing wire machine is set to 1.5 mm, and then the first ethylene-lactide copolymer is extruded into a strip at 175° C. at a screw speed of 80 r / min in the 3D printing wire machine, and then rolled up after cooling to room temperature (25° C.) to obtain a cylindrical first composite material with a diameter of 1.5 mm.

[0196] Preparation of the second composite material and temporary plugging particles:

[0197] The second ethylene-lactide copolymer was put into the feeding hopper of a wire extruder set at a heating temperature of 120°C as the skin material, and the cylindrical first composite material prepared in this comparative example was passed through the threading hole of the wire extruder as the core material. However, because the core material was not heat-resistant (probably because the crystalline core material was not obtained), effective traction could not be formed, the second composite material with a skin-core structure could not be obtained, and temporary plugging particles could not be obtained.

[0198] Comparative Example 6

[0199] The first glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 85:15, with a weight average molecular weight of 80,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG1585-8;

[0200] The second glycolide-lactide copolymer used in this comparative example is a regular cylindrical particle formed by copolymerization of glycolide and lactide at a molar ratio of 50:50, with a weight average molecular weight of 50,000, an average diameter of 3 mm, and an average height of 3 mm, purchased from Jinan Daigang Bioengineering Co., Ltd., with a brand name of LG5050-5;

[0201] Preparation of temporary plugging particles:

[0202] The first ethylene-lactide copolymer particles and the second ethylene-lactide copolymer particles are uniformly mixed in a glass beaker at a mass ratio of 1:1 to obtain temporary plugging particles.

[0203] Comparative Example 7

[0204] The soluble acrylic resin irregular particles used in this comparative example have a particle size of 5 to 80 meshes, purchased from Shandong Nengju Chemical Co., Ltd., with a brand name of GPAA-R-5;

[0205] The copolymer grade polyacrylamide irregular particles used in this comparative example have a particle size of 5 to 80 meshes and are purchased from Shanghai Zhenzhun Biotechnology Co., Ltd. with a brand name of AML5-80;

[0206] Preparation of temporary plugging particles:

[0207] Soluble acrylic resin irregular particles and copolymer grade polyacrylamide irregular particles were mixed evenly in a glass beaker in a mass ratio of 1:1 to obtain temporary plugging particles.

[0208] Comparative Example 8

[0209] The polylactic acid irregular particles used in this comparative example have a particle size of 5 to 80 meshes and are purchased from Zhejiang Hisun Biomaterials Co., Ltd. with a brand name of LA221-5-80;

[0210] Take irregular polylactic acid particles directly as temporary plugging particles.

[0211] The structure of the temporary plugging particles obtained by the second composite material and pelletization thereof

[0212] The second composite material prepared in Examples 1 to 10 and Comparative Examples 1, 3 and 4 has a skin-core structure, and the temporary plugging particles are obtained by physically pelletizing the second composite material along a direction perpendicular to the cylindrical axis, and also have the same skin-core structure as the second composite material. Figure 1 Schematic diagram of the skin-core structure of temporary plugging particles. Figure 2 The top view of the temporary blocking particles. Figure 3 It is a cross-sectional view of the temporary blocking particles. Figures 1 to 3 In the figure, 1 is the cortex and 2 is the core layer; Figure 3 In the figure, h is the height of the temporary plugging particle, d2 is the diameter of the temporary plugging particle, d1 is the diameter of the core layer in the skin-core structure of the temporary plugging particle, and δ is the thickness of the skin layer in the skin-core structure of the temporary plugging particle. Figures 1 to 3 It can be seen that the temporary plugging particles are cylindrical, and the skin layer with a certain thickness wraps the cylindrical core layer to form a skin-core structure.

[0213] Temporary plugging particle performance evaluation

[0214] 1. Determination of temporary plugging particle plugging strength

[0215] The DV-IV temporary plugging agent pressure bearing capacity evaluation instrument produced by Jiangsu Huaan Scientific Research Instrument Co., Ltd. was used to measure the plugging strength of the temporary plugging particles prepared in Examples 1 to 10 and Comparative Examples 1 to 8 in accordance with standard Q / SH CG0152-2021 to evaluate the pressure bearing capacity of the temporary plugging particles. The organic boron crosslinking agent used in this experiment was purchased from Dongying Shipurui Petroleum Engineering Technology Co., Ltd., model "Guar Gum Fracturing Fluid Crosslinking Agent 60°C", and implemented standard Q / SH CG0128.

[0216] The specific measurement steps are as follows:

[0217] ⅰ Preparation of guar gum base liquid: 1000 mL of distilled water was measured and poured into the sample cup of Wu Yin mixer, and then 4.0 g of hydroxypropyl guar gum was added; then Wu Yin mixer was adjusted to "low speed" gear, the voltage was adjusted to 55 V, and the mixture was stirred for 5 minutes and then poured into a beaker; then 3.0 g of sodium carbonate was added to the sample cup of Wu Yin mixer, and then the solution was poured into a wide-mouth bottle, covered, and placed in a water bath at 30° C. for 4 hours to obtain guar gum base liquid, the mass of which was calculated as 100%, and the guar gum base liquid contained 0.4 wt% hydroxypropyl guar gum, 0.3 wt% sodium carbonate and the remainder of water;

[0218] ⅱ Preparation of gel containing temporary plugging particles: Use a measuring cylinder to weigh 1000 mL of the guar gum base liquid prepared in step ⅰ into a beaker and mix at a rate of 200 kg / m 3 200g of temporary plugging particles are added to 1000mL of guar gum base liquid, mixed and stirred evenly, and then 0.5wt% of an organic boron crosslinking agent is added to react at room temperature to form a gel containing temporary plugging particles;

[0219] ⅲ Set the outlet width of the wedge-shaped steel core seam plate to 1mm, install the core holder, connect the holder to the intermediate container, and heat the core holder to 60°C. Then, place the gel containing the temporary plugging agent into a 1000mL intermediate container. Open the connecting valve of the intermediate container, start the horizontal flow pump, set the horizontal flow pump displacement to 40mL / min, and the pressure limit to 5MPa, conduct a displacement experiment, observe and record the displacement pressure increase after temporary plugging, and when the pressure increase after temporary plugging reaches 5MPa and is stable for 1h or more, it is considered that the temporary plugging particles have a qualified pressure bearing capacity for plugging 1mm width cracks;

[0220] ⅳ Based on the displacement experiment conducted in step ⅲ, the displacement of the horizontal flow pump is increased, and the displacement is gradually increased within the displacement range of 40 mL / min to 100 mL / min (specifically, starting from a displacement of 40 mL / min, the displacement is increased by 10 mL / min every 10 minutes to 100 mL / min). The displacement experiment is carried out, and within the rated maximum pressure range of the horizontal flow pump, the increase in displacement pressure after temporary plugging is observed and recorded. When the pressure rises to a certain value, the pressure decreases rapidly. The maximum pressure at this time is the plugging strength of the temporary plugging particles under the condition that the crack width is 1 mm;

[0221] ⅴ Set the outlet width of the wedge-shaped steel core seam plate to 2 mm, perform the displacement experiment in the same way as in step ⅲ, observe and record the displacement pressure increase after temporary plugging, and when the pressure increase after temporary plugging reaches 5 MPa and remains stable for 1 hour or more, it is considered that the pressure bearing capacity of the temporary plugging particles to plug the 2 mm width crack is qualified;

[0222] ⅵ Based on the displacement experiment conducted in step V, the plugging strength of the temporary plugging particles under the condition of a crack width of 2 mm is measured according to the same operation as in step IV;

[0223] According to the above method, the temporary plugging particles prepared in Examples 1 to 10 and Comparative Examples 1 to 8 were measured for their plugging strength when plugging cracks with a width of 1 mm and 2 mm. The specific results are shown in Table 1, wherein “ / ” indicates that the temporary plugging particles cannot be measured or are not prepared for measurement.

[0224] Table 1. Pressure bearing capacity of temporary plugging particles

[0225]

[0226]

[0227] From the data in Table 1, it can be seen that the temporary plugging particles made of the second composite material prepared in Examples 1 to 10 have a plugging strength of 40 to 50 MPa for 1 mm wide cracks and a plugging strength of 33 to 45 MPa for 2 mm wide cracks, and the plugging effect is good. Among them, the temporary plugging particles made of the second composite material prepared in Example 6 have a plugging strength of 50 MPa for 1 mm wide cracks and a plugging strength of 44 MPa for 2 mm wide cracks, and the best plugging effect, which proves that the temporary plugging particles made of the second composite material prepared in Examples 1 to 10 have excellent plugging pressure bearing performance. The plugging strengths of the temporary plugging particles prepared in Comparative Examples 4, 6, 7 and 8 for 1 mm wide cracks are 16 MPa, 25 MPa, 12 MPa and 26 MPa respectively; the plugging strengths of the temporary plugging particles prepared in Comparative Examples 4, 6 and 8 for 2 mm wide cracks are 11 MPa, 12 MPa and 14 MPa respectively. Since the gel containing the temporary plugging particles prepared in Comparative Example 7 was too thin and directly leaked out, the 2 mm seam plate could not be pressurized during the experiment, and thus the plugging strength for the 2 mm wide crack could not be measured. It can be seen that the plugging strengths of Comparative Examples 4, 6, 7 and 8 are significantly lower, and their pressure bearing capacity is poor or even has almost no pressure bearing capacity. From the preparation steps and the preparation process, the core material of the second composite material prepared in Comparative Example 4 is a first composite material prepared from ammonium polyphosphate with a polymerization degree of 20 to 100 and a first ethylene-lactide copolymer. The polymerization degree of ammonium polyphosphate is too low, and the first composite material is easy to break when winding; Comparative Example 6 does not prepare the temporary plugging particles of the second composite material according to the method provided by the present invention, but simply physically mixes the first ethylene-lactide copolymer and the second ethylene-lactide copolymer to obtain temporary plugging particles; Comparative Example 7 also does not use the method provided by the invention, but simply physically mixes soluble acrylic resin irregular particles and copolymer-grade polyacrylamide irregular particles to obtain temporary plugging particles; Comparative Example 8 directly uses polylactic acid irregular particles as temporary plugging particles. The above shows that the polymerization degree of ammonium polyphosphate used to prepare the first composite material will affect the strength of the first composite material; the polymerization degree of ammonium polyphosphate, the steps for preparing the first composite material and the second composite material, and the types of raw materials used will affect the pressure bearing capacity of the obtained temporary plugging particles.Comparative Examples 2 and 5 did not prepare temporary plugging particles during the preparation process because the first composite material was not heat-resistant and could not be processed to obtain the second composite material. According to the raw materials used and the preparation process, the copolymerization molar ratio of glycolide and lactide in the first ethylene-lactide copolymer used in Comparative Example 2 was different from those in Examples 1 to 10; no ammonium polyphosphate was added to the first composite material prepared in Comparative Example 5, and the first composite material was not prepared according to the preparation method provided by the present invention. The inventors believe that the first composite material prepared in Comparative Example 5 may not reach a crystalline state and affect its heat resistance. Comparative Examples 2 and 5 show that ammonium polyphosphate is beneficial to enhancing the heat resistance of the first composite material, the copolymerization molar ratio of glycolide and lactide in the first ethylene-lactide copolymer and the preparation steps will affect the performance of the first composite material, thereby affecting the preparation of the second composite material with the first composite material as the core material, and ultimately affecting the preparation of the temporary plugging particles.

[0228] 2. Determination of dissolution rate of temporary blocking particles

[0229] The standard dissolution rate and water-deficiency dissolution rate of the temporary plugging particles prepared in Examples 1 to 10 and Comparative Examples 1 to 8 at different temperatures were measured. The experimental steps are as follows:

[0230] A. Determination of standard dissolution rate of temporary plugging particles at different temperatures

[0231] (1) Set the constant temperature drying oven to 105°C and dry the filter paper to a constant weight, recorded as m1 (accurate to 0.0001 g);

[0232] (2) Weigh 2 g (accurate to 0.0001 g) of temporary plugging particles using an electronic balance, recorded as m2; add the weighed temporary plugging particles into a wide-mouth bottle containing 200 mL of distilled water and stir evenly; put the wide-mouth bottle containing the temporary plugging particles and distilled water into an oven set to the experimental temperature, keep the temperature constant for 72 hours, and then stop heating;

[0233] (3) Open the wide-mouth bottle, filter the mixture in the wide-mouth bottle with a quick qualitative filter paper, rinse the filter residue with 100 mL of distilled water, and then place the filter paper and the filter residue in an oven at a temperature of 105°C to dry to a constant weight, which is recorded as m3;

[0234] (4) Calculate the standard dissolution rate of temporary blocking particles;

[0235] The experimental temperatures in step (2) are 60°C and 90°C.

[0236] According to the order of steps (1), (2), (3), and (4), the standard dissolution rate of the temporary plugging particles prepared in Examples 1 to 10 and Comparative Examples 1 to 8 was measured. During the determination of the standard dissolution rate of each temporary plugging particle, the oven temperature in step (2) was set to 60° C. and 90° C., and the standard dissolution rate of each temporary plugging agent at 60° C. and 90° C. was obtained. The specific results are shown in Table 2.

[0237] B. Determination of water-deficient dissolution rate of temporary plugging particles at different temperatures

[0238] ① Set the constant temperature drying oven to 105℃, and dry the experimental filter paper to constant weight, recorded as m1' (accurate to 0.0001g);

[0239] ② Use an electronic balance to weigh 20g (accurate to 0.0001g) of temporary plugging particles, counted as m2', add the weighed temporary plugging particles into a wide-mouth bottle filled with 20mL of distilled water, and stir evenly; put the wide-mouth bottle filled with temporary plugging particles and distilled water into an oven set to the experimental temperature, keep the temperature constant for 72h, and then stop heating;

[0240] ③Open the wide-mouth bottle, filter the mixture in the wide-mouth bottle with rapid qualitative filter paper, rinse the filter residue with 100mL of distilled water, and then place the filter paper and filter residue in an oven at 105℃ and dry them to constant weight, recorded as m3'.

[0241] ④According to Calculate the water-deficient dissolution rate of the temporary plugging particles; the experimental temperature in step ② is 60℃ and 90℃.

[0242] According to the order of steps ①, ②, ③, and ④, the water-deficient dissolution rate of the temporary plugging particles prepared in Examples 1 to 10 and Comparative Examples 1 to 8 was measured. In the process of measuring the water-deficient dissolution rate of each temporary plugging particle, the oven temperature in step ② was set to 60°C and 90°C, and the water-deficient dissolution rate of each temporary plugging agent at 60°C and 90°C was obtained. The specific results are shown in Table 2, where " / " indicates that the temporary plugging particles cannot be measured or are not prepared for measurement.

[0243] Table 2. Standard dissolution rate and water-deficient dissolution rate of temporary plugging particles at different temperatures

[0244]

[0245] The data in Table 2 show that the standard dissolution rate and water-deficient dissolution rate of the temporary plugging particles of the second composite material prepared in Examples 1 to 10 at 60°C are 80.3% to 96.5% and 71.5% to 90.7%, respectively; the standard dissolution rate and water-deficient dissolution rate at 90°C are 96.4% to 99.6% and 91.3% to 99.2%, respectively, indicating that the temporary plugging agents prepared in Examples 1 to 10 have excellent solubility at 60 to 90°C and can maintain a high dissolution rate even in the absence of water. The copolymerization molar ratio of glycolide and lactide in the first ethylene-lactide copolymer used in the temporary plugging particles prepared in Comparative Example 1 is different from that used in Examples 1 to 10, as shown by the standard dissolution rate and water-deficient dissolution rate of the temporary plugging particles prepared in Comparative Example 1 at 60°C are 65.8% and 52.2%, respectively; the standard dissolution rate and water-deficient dissolution rate at 90°C are 89.3% and 81.7%, respectively, and the solubility performance is inferior to that of the temporary plugging particles of the second composite material prepared in Examples 1 to 10. The temporary plugging particles prepared in Comparative Example 3 contain a first composite material prepared by using a commercially available nucleating agent and a first ethylene-lactide copolymer, without adding ammonium polyphosphate. Both the standard dissolution rate and the water-deficient dissolution rate are lower than those of the temporary plugging particles made of the second composite material prepared in Examples 1 to 10, indicating that ammonium polyphosphate is beneficial to enhancing the dissolution performance of the temporary plugging particles of the second composite material. Comparative Example 6 directly physically mixes the first ethylene-lactide copolymer and the second ethylene-lactide copolymer to prepare temporary plugging particles. At the same temperature, its standard dissolution rate and water-deficient dissolution rate are lower than those of the temporary plugging particles prepared in Examples 1 to 10. Comparative Example 7 uses Although the temporary plugging particles prepared by simply physically mixing soluble acrylic resin irregular particles and copolymer-grade polyacrylamide irregular particles have a high standard dissolution rate at 90°C, their standard dissolution rate at 60°C is only 20.4%, and they only swell but do not dissolve in the absence of water. The water-absence dissolution rates at 60°C and 90°C are both 0, which cannot meet the complex formation conditions in practical applications. The temporary plugging particles in Comparative Example 8 are polylactic acid irregular particles, which do not dissolve at 60°C, and their standard dissolution rate and water-absence dissolution rate at 90°C are only 37.5% and 26.8%, respectively, and their solubility is obviously poor.

[0246] According to the plugging strength data shown in Table 1 and the dissolution rate data shown in Table 2, the temporary plugging particles of the second composite material prepared in Examples 1 to 10 have good plugging pressure bearing capacity, high solubility and excellent solubility in water shortage conditions, and can effectively plug cracks with a width of 1mm to 2mm. They have strong adaptability to cracks, low requirements for underground water bodies, and no pollution to the environment, and can meet the requirements of the current temporary plugging and fracturing technology for temporary plugging agents. Although the temporary plugging particles prepared in Comparative Examples 1 and 3 have high plugging strength for 1mm and 2mm cracks, they have poor solubility and high requirements for underground water bodies in practical applications; although the temporary plugging particles prepared in Comparative Examples 4 and 6 have good solubility, they have poor plugging pressure bearing capacity and cannot effectively plug cracks; the plugging pressure bearing capacity and solubility of the temporary plugging agents in Comparative Examples 7 and 8 are not good, and cannot meet the requirements of the temporary plugging and fracturing technology for temporary plugging agents; the processes in Comparative Examples 2 and 5 cannot prepare the second composite material and temporary plugging particles. It is shown that the copolymerization molar ratio of glycolide and lactide in the first glycolide-lactide copolymer, ammonium polyphosphate and its polymerization degree, and the method steps for preparing the first composite material and the second composite material will affect the performance of the final temporary plugging particles and whether temporary plugging particles made of the second composite material can be prepared.

[0247] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.

Claims

1. A first composite material comprising a first ethylene-lactide copolymer and ammonium polyphosphate.

2. The first composite material according to claim 1, characterized in that: The mass ratio of the first lactide-ethylene glycol copolymer to ammonium polyphosphate is (2 to 4):

1.

3. The first composite material according to claim 1 or 2, characterized in that: The first glycolide-lactide copolymer is obtained by copolymerizing glycolide and lactide in a molar ratio of 85:15; and / or The weight average molecular weight of the first ethylene-lactide copolymer is greater than 50,000; Preferably, the weight average molecular weight of the first ethylene-lactide copolymer is 50,000 to 100,000.

4. The first composite material according to any one of claims 1 to 3, characterized in that: The degree of polymerization of the ammonium polyphosphate is 1000 to 1200.

5. A method for preparing the first composite material according to any one of claims 1 to 4, comprising the following steps: 1) mixing the first lactide-ethylene glycol copolymer and ammonium polyphosphate and granulating the mixture to obtain an intermediate material; 2) Extruding the intermediate material into a strip, and rolling it up after cooling to obtain the first composite material.

6. The method according to claim 5, characterized in that In step 1), the granulation is performed by a twin-screw granulator; Preferably, the granulation condition is melt extrusion granulation at 170°C to 190°C.

7. The method according to claim 5 or 6, characterized in that: In step 2), the extrusion drawing is performed by a 3D printing wire machine; Preferably, the intermediate material is extruded into a strand at 175°C to 190°C.

8. A second composite material having a skin-core structure; the material of the core layer of the skin-core structure is the first composite material; the material of the skin layer of the skin-core structure is the second ethylene-lactide copolymer; The first composite material is the first composite material according to any one of claims 1 to 4 or the first composite material prepared by the method according to any one of claims 5 to 7.

9. The second composite material according to claim 8, characterized in that: The second glycolide-lactide copolymer is obtained by copolymerizing glycolide and lactide in a molar ratio of (30 to 70):(70 to 30); and / or The weight average molecular weight of the second ethylene-lactide copolymer is 30,000 to 50,000; Preferably, the second glycolide-lactide copolymer is obtained by copolymerizing glycolide and lactide in a molar ratio of 50:

50.

10. The second composite material according to claim 8 or 9, characterized in that: The second composite material is a cylindrical composite material having the skin-core structure; Preferably, the core layer in the skin-core structure is a cylinder with a diameter of 1 mm to 2 mm; and / or The thickness of the skin layer in the skin-core structure is 0.5 mm to 1 mm.

11. A method for preparing the second composite material according to any one of claims 8 to 10, comprising the following steps: The second ethylene-lactide copolymer is coated on the surface of the core layer, pulled, and cooled to obtain the second composite material.

12. The method according to claim 11, characterized in that The coating and drawing are achieved by a wire extruder; Preferably, the temperature of the wire extruder hopper is 110° C. to 130° C.; and / or The cooling temperature is cooling to room temperature.

13. The method according to claim 11 or 12, characterized in that: Cutting the second composite material into particles along a direction perpendicular to the axial direction of the cylinder to obtain temporary plugging particles; Preferably, the temporary plugging particles are cylindrical, with a diameter of 2 mm to 4 mm; and / or a height of 3 mm to 5 mm; Preferably, the temporary plugging particles have a diameter of 2.5 mm to 4 mm.

14. Use of any one of the first composite material according to any one of claims 1 to 4, the first composite material prepared by the method according to any one of claims 5 to 7, the second composite material according to any one of claims 8 to 10, and the second composite material prepared by the method according to any one of claims 11 to 13 in the field of natural gas production enhancement technology, especially in temporary plugging and diversion fracturing.

Citation Information

Patent Citations

  • Novel flame retardant and anti-static biodegradable material and preparation method thereof

    CN103881338A

  • Temporary plugging agent for temporary plugging diversion for overcoming high stress difference in shale gas fracturing, and preparation method thereof

    CN108300442A

  • Plugging agent for drilling fluid and preparation method thereof

    CN111607366A

  • Preparation method of water-soluble composite material temporary plugging agent for diversion fracturing

    CN113249101A

  • Novel glycolide-rich copolymers

    WO2009016194A1