Carbon fiber composite board for aviation and preparation process
By using carbon fiber, PBO fiber, bio-based epoxy resin and internal mold release agents, carbon fiber composite boards for aviation are prepared, which solves the problems of easy corrosion and high maintenance costs of traditional aviation boards, and realizes the high temperature and corrosion resistance of the materials. and chemical corrosion resistance, reducing costs and suitable for use in the aerospace field.
Patent Information
- Application Number
- CN202411436514.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional aviation boards are prone to corrosion, aging and high maintenance costs.
Using carbon fiber, PBO fiber, bio-based epoxy resin and internal mold release agent, carbon fiber composite boards for aviation are prepared through hot pressing tank process to ensure the high temperature, corrosion resistance and chemical corrosion resistance of the materials, and through specific preparation Process reduces raw material and maintenance costs.
It has achieved high temperature resistance, corrosion resistance and chemical corrosion resistance of carbon fiber composite sheets for aviation, reduced raw materials and maintenance costs, significantly improved the cost-effectiveness of the materials, and is suitable for use in the aerospace field.
Smart Images

Figure CN119019845A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of material science and engineering technology, and in particular to a carbon fiber composite plate for aviation and a preparation process thereof. Background Art
[0002] In the aerospace industry, the selection of materials is crucial because they directly affect the performance, safety and economy of the aircraft. Traditional aviation sheets mainly include materials such as aluminum alloys, high-strength steels and titanium alloys. These materials have a wide range of applications and an important position in the aviation field due to their excellent mechanical properties and relatively mature processing technology. With the continuous advancement of technology, the preparation process of these materials is also being continuously optimized. For example, the application of hydraulic forming process has significantly improved the manufacturing quality and efficiency of sheets. However, despite the many advantages of traditional materials, they also have some limitations, such as easy corrosion and aging, which leads to high maintenance costs and requires regular inspection and replacement.
[0003] In contrast, carbon fiber composites for aviation have gradually become the new favorite in the aerospace field due to their unique performance advantages, such as high temperature resistance, corrosion resistance, and chemical erosion resistance. Carbon fiber composites have low maintenance costs and longer service life, making them very suitable for high-end applications such as aerospace. In the future, with the continuous emergence of new materials, traditional aviation panels will continue to play an important role and promote the development of the aviation industry together with other new materials. At the same time, the application of carbon fiber composites will also be further expanded, bringing more innovations and breakthroughs to the aerospace industry. Summary of the invention
[0004] 1. Technical issues to be resolved In view of the shortcomings of the prior art, the present invention provides a carbon fiber composite sheet for aviation and a preparation process, which has the advantages of high temperature resistance, corrosion resistance, chemical erosion resistance and low maintenance cost, and solves the problems of easy corrosion, easy aging and high maintenance cost of traditional aviation sheets.
[0005] To achieve the above object, the present invention provides the following technical solutions: a carbon fiber composite sheet for aviation, wherein the raw materials of the composite sheet are composed of carbon fiber, high-performance fiber, resin matrix, high-performance polymer and fusion agent; The specific weight ratios of the raw materials are: asphalt-based carbon fiber 12%-15%; PE-based carbon fiber 7%-9%; PBO fiber 3%-6%; bismaleimide resin 11%-13%; bio-based epoxy resin 6%-8%; ultra-high molecular weight polyethylene 7%-12%; polyetheretherketone resin 4%-6%; low shrinkage additive 0.5%-1%; thickener 0.8%-1.1%; internal release agent 1%-1.3%; colorant 2%-2.5%; polyphenylene ether 3%-4%; polyetherimide 5%-6%.
[0006] Preferably, the carbon fiber is composed of asphalt-based carbon fiber and PE-based carbon fiber, and the high-performance fiber is PBO fiber.
[0007] Preferably, the resin matrix is composed of bismaleimide, bio-based epoxy resin, polyetheretherketone resin and ultra-high molecular weight polyethylene.
[0008] Preferably, the high-performance polymer consists of polyphenylene ether and polyetherimide, and the fusion agent consists of a low-shrinkage additive, a thickener, an internal mold release agent and a colorant.
[0009] Preferably, a preparation process of a carbon fiber composite sheet for aviation is prepared according to the weight ratio of raw materials of the above-mentioned carbon fiber composite sheet for aviation, and the preparation steps are: Step 1. Raw material preparation: Use a weighing instrument to weigh asphalt-based carbon fiber, PE-based carbon fiber, PBO fiber, bismaleimide resin, bio-based epoxy resin, ultra-high molecular weight polyethylene, polyetheretherketone resin, low shrinkage additive, thickener, internal release agent, colorant, polyphenylene ether and polyetherimide; Step 2: Preform preparation: the prepared raw materials are mixed evenly in a specific order to form a preform; Step 3: Laying the preform: Use an automatic tape laying machine to lay the preform on the mold; Step 4: Curing process: Select the autoclave process and set the curing conditions; Step 5: Post-processing of the board: After the curing is completed, the board is cut, ground and polished according to the manufacturer's design sample as a model; Step 6: Mechanical processing: Perform mechanical reprocessing as needed.
[0010] Preferably, the step 2 is to mix the raw materials in the following order: S1.1. Add bismaleimide resin, bio-based epoxy resin, low shrinkage additive and thickener into a high-precision mixer, set the temperature to 60°C, and stir at a stirring speed of 500 r / min for 15 min; S1.2, adding the asphalt-based carbon fiber, PE-based carbon fiber and PBO fiber into the mixture in S1.1 at a rate of 10 kg / min, and stirring at a temperature of 100°C and a stirring speed of 1000 r / min for 8 min; S1.3, adding ultra-high molecular weight polyethylene and polyetheretherketone resin to the mixture of S1.2, stirring at a temperature of 120°C and a stirring speed of 600 r / min for 10 min; S1.4, add colorant, polyphenylene ether and polyetherimide, lower the temperature to 50°C, stir at a stirring speed of 1000 r / min for 15 minutes to complete the entire mixing process to form a preform.
[0011] Preferably, the paving process of the preform in step 3 is: S2.1. Select the automatic tape laying machine as the mold laying equipment; S2.2, select a mold and apply a 1mm layer of inner release agent to the inner layer of the mold; S2.3, set the temperature of the automatic tape laying machine to 80°C; S2.4. Set the flow rate of the automatic tape laying machine to 20-30m / s, set the pressure of the automatic tape laying machine to 0.5-1MPa, start the automatic tape laying machine, and after preheating for 30 minutes, inject the preform from the mixing equipment into the automatic tape laying machine to start laying the preform.
[0012] Preferably, in the curing process of step 4, the preformed body covered in the mold is placed in an autoclave, the temperature is set to 120° C., the duration is 30 minutes, and the pressure of the autoclave is set to between 1-1.2 MPa.
[0013] Preferably, the post-processing process of the plate in step 5 is: S3.1. After curing is completed, cool the autoclave to room temperature and take out the composite sheet; S3.2. Finally, the composite board is cut to the same specifications as the sample designed by the manufacturer, and then polished.
[0014] Preferably, the mechanical processing in step six: mechanical reprocessing is performed according to the manufacturer's type requirements, including drilling and milling, to meet specific assembly and use requirements.
[0015] Compared with the prior art, the present invention provides a carbon fiber composite sheet for aviation and a preparation process, which has the following beneficial effects: 1. The aviation carbon fiber composite sheet of the present invention uses PBO fiber, bio-based epoxy resin and internal release agent. PBO fiber has excellent mechanical properties and heat resistance, and can be used to enhance the performance of composite materials. Bio-based epoxy resin is made of natural materials, has the characteristics of environmental protection and sustainability, and reduces the cost of raw materials while maintaining good bonding properties. The use of internal release agent helps the composite material to be more easily removed from the mold after molding, and reduces damage and defects on the surface of the product. The combination of the three raw materials makes the finished sheet have excellent high temperature resistance, corrosion resistance and chemical erosion resistance. After evaluation of finished product test data, the raw material cost and maintenance cost of the composite material are reduced by 5% and 3% respectively compared with the existing composite sheet, which effectively solves the problems of easy corrosion, easy aging and high maintenance cost of traditional aviation sheets. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a diagram of the preparation steps of the present invention. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] See also Figure 1 , a carbon fiber composite sheet for aviation, the raw materials of the composite sheet are composed of composite materials, carbon fibers, high-performance fibers, resin matrix, high-performance polymers and fusion agents, and the specific weight ratios of the raw materials and their functions are as follows: Asphalt-based carbon fiber: accounting for 12%-15%, with high strength, high modulus and excellent heat resistance, can be used to manufacture high-performance composite materials; PE-based carbon fiber: accounting for 7%-9%. PE-based carbon fiber has the characteristics of light weight and high strength and can be used in the aerospace field; PBO fiber: accounting for 3%-6%. PBO fiber has excellent mechanical properties and heat resistance and is used to enhance the performance of composite materials; Bismaleimide resin (BMI): accounting for 11%-13%. BMI resin is a high-performance thermosetting resin with excellent high temperature resistance and mechanical properties; Bio-based epoxy resin: 6%-8%. This resin is made from natural materials and is environmentally friendly and sustainable while maintaining good bonding properties. Ultra-high molecular weight polyethylene (UHMWPE): accounting for 7%-12%, with high wear resistance and self-lubrication, used in demanding working environments; Polyetheretherketone (PEEK) resin: accounting for 4%-6%. PEEK resin is a high-performance engineering plastic with excellent heat resistance, chemical resistance and mechanical properties; Low shrinkage additives: accounting for 0.5%-1%, used to reduce the volume shrinkage of composite materials during the curing process and improve the dimensional accuracy of the products; Thickener: 0.8%-1.1%, used to increase the viscosity of the resin to facilitate molding operation and control; Internal release agent: accounting for 1%-1.3%, helps the composite material to be more easily removed from the mold after molding, reducing damage and defects on the surface of the product; Colorants: 2%-2.5%, used to color composite materials to meet specific color requirements; Polyphenylene ether (PPO): accounting for 3%-4%. PPO is a high-performance polymer with good heat resistance, chemical resistance and electrical insulation. Polyetherimide (PEI): accounting for 5%-6%, PEI is an amorphous high-performance polymer with excellent heat resistance, chemical resistance and mechanical properties.
[0019] Specifically, the carbon fiber is composed of asphalt-based carbon fiber and PE-based carbon fiber, and the high-performance fiber is PBO fiber.
[0020] Specifically, the resin matrix consists of bismaleimide, bio-based epoxy resin, polyetheretherketone resin and ultra-high molecular weight polyethylene.
[0021] Specifically, the high-performance polymer consists of polyphenylene ether and polyetherimide, and the fusing agent consists of a low-shrinkage additive, a thickener, an internal mold release agent and a colorant.
[0022] Specifically, a preparation process of a carbon fiber composite sheet for aviation is prepared according to the weight ratio of raw materials of the above-mentioned carbon fiber composite sheet for aviation, and the preparation steps are: Step 1. Raw material preparation: Use a weighing instrument to weigh asphalt-based carbon fiber, PE-based carbon fiber, PBO fiber, bismaleimide resin, bio-based epoxy resin, ultra-high molecular weight polyethylene, polyetheretherketone resin, low shrinkage additive, thickener, internal release agent, colorant, polyphenylene ether and polyetherimide; Step 2: Preform production: Mix the prepared raw materials in a specific order to form a preform. This step helps with subsequent curing and molding, because the quality of the preform directly affects the performance of the final sheet. High-precision equipment and technology are used; Step 3: Preform laying: The preform is then laid on the mold using an automatic tape laying machine; these devices ensure uniform fiber distribution and precise lamination angles to optimize the mechanical properties of the composite material; Step 4: Curing process: Select the autoclave process and set the curing conditions to ensure that the resin is fully cured and forms a dense internal structure. At the same time, monitor the temperature and pressure field distribution during the curing process to avoid defects. Step 5: Post-processing of the board: After the curing is completed, the board is cut, ground and polished according to the manufacturer's design sample as a model to obtain the shape and size required by the manufacturer; Step 6: Mechanical processing: Perform mechanical reprocessing as needed, such as drilling, milling, etc., to meet specific assembly and use requirements. During the processing, pay attention to controlling the processing parameters and tool selection to avoid damage to the composite material.
[0023] Specifically, step 2 is to mix the raw materials in order: S1.1. Add bismaleimide resin, bio-based epoxy resin, low shrinkage additive and thickener into a high-precision mixer, set the temperature to 60°C, and stir at a stirring speed of 500 r / min for 15 minutes to ensure the uniformity and fluidity of the resin matrix; S1.2, adding the asphalt-based carbon fiber, PE-based carbon fiber and PBO fiber into the mixture in S1.1 at a rate of 10 kg / min, stirring at a temperature of 100°C and a stirring speed of 1000 r / min for 8 min to ensure that the fibers are evenly dispersed in the resin matrix; S1.3, adding ultra-high molecular weight polyethylene and polyetheretherketone resin to the mixture of S1.2, stirring at a temperature of 120°C and a stirring speed of 600 r / min for 10 min, and continuing stirring to maintain uniformity; S1.4, add colorant, polyphenylene ether and polyetherimide, lower the temperature to 50°C, stir at a stirring speed of 1000 r / min for 15 minutes to complete the entire mixing process to form a preform.
[0024] Specifically, the draping process of the preform in step 3: S2.1. Select the automatic tape laying machine as the mold laying equipment: the automatic tape laying machine can realize automatic and continuous production, improve production efficiency, and reduce the impact of human factors on the quality of the board. At the same time, the automatic tape laying machine has a high-precision control system that can accurately control the laying sequence, position and tension of the fiber material to ensure the uniformity and stability of the preform; S2.2. Select a mold and apply a 1mm layer of inner mold release agent to the inner layer of the mold: The inner mold release agent is applied to the inner surface of the mold to prevent the preform from sticking to the mold and facilitate the subsequent demoulding operation. The thickness of 1mm is usually enough to form an effective isolation layer, but the specific thickness needs to be adjusted according to the requirements of the plate and the actual situation; S2.3. Set the temperature of the automatic tape laying machine to 80°C. This temperature is within the recommended curing temperature range of the resin matrix, ensuring that the resin can be fully cured and achieve the expected performance. S2.4. Set the flow rate of the automatic tape laying machine to 20-30m / s, set the pressure of the automatic tape laying machine to 0.5-1MPa, start the automatic tape laying machine, and after preheating for 30 minutes, inject the preform from the mixing equipment into the automatic tape laying machine to start preform laying. Preheating before injecting the preform into the automatic tape laying machine can help the equipment reach a stable working state and reduce errors and unstable factors caused by temperature changes. At the same time, preheating also helps to improve the fluidity and wettability of the resin matrix, thereby improving the quality of the preform. When the preform is injected from the mixing equipment into the automatic tape laying machine, the flow rate and pressure within this range can avoid bubbles or unevenness.
[0025] Specifically, in the curing process of step 4: the preform covered in the mold is placed in an autoclave, the temperature is set to 120°C, and the duration is 30 minutes. This step is to fully cure the resin matrix to achieve the expected performance, and the pressure of the autoclave is set between 1-1.2MPa. This pressure can ensure that the resin matrix will not produce bubbles or unevenness during the curing process.
[0026] Specifically, the post-processing process of the plate in step 5: S3.1. After curing is completed, cool the autoclave to room temperature and take out the composite sheet. During the cooling process, the temperature needs to be gradually lowered to avoid deformation or cracking of the sheet due to rapid temperature changes; S3.2. Finally, the composite board is cut to the same specifications as the sample designed by the manufacturer, and then polished to meet the size and surface quality requirements of the board.
[0027] Specifically, in step six, mechanical processing: mechanical reprocessing is carried out according to the manufacturer's type requirements, including drilling and milling, to meet specific assembly and use requirements. During the processing, attention should be paid to controlling the processing parameters and tool selection to avoid damage to the composite material.
[0028] Example 1
[0029] A factory made carbon fiber composite panels for aviation based on the above raw materials and preparation steps, and conducted tests on high temperature resistance, corrosion resistance, and chemical erosion resistance. Finally, the raw materials and maintenance costs were evaluated. The test data and evaluation results are shown in Table 1 below.
[0030] Table 1 Test items Test conditions Test Data Evaluation results High temperature resistance Temperature range: room temperature to 250°C No noticeable deformation or performance degradation Meet the high temperature use standards of aviation materials Corrosion resistance Soak in 3.5% NaCl solution for 48 hours No corrosion Excellent corrosion resistance Chemical resistance Exposure to acidic (pH 3) and alkaline (pH 11) environments for 24 hours each No noticeable loss of quality or change in performance Shows good resistance to chemical attack Raw material cost 5% reduction compared with existing composite panels The decrease was 5% Cost-effectiveness analysis shows high cost-effectiveness Maintenance costs Compared with the existing composite panels, it is reduced by 3% The decline was 3% Low maintenance cost and significant economic benefits under long-term use Machining performance Drilling, milling High processing precision and good surface quality Easy to machine and meet the requirements of complex structural design Overall evaluation - - The aviation carbon fiber composite sheet has excellent comprehensive performance and is suitable for use in the aerospace field .
[0031] Comparative Example 1: A factory removed PBO fiber, bio-based epoxy resin and internal release agent from the above raw materials, and kept other raw materials unchanged. The factory also made aviation carbon fiber composite plates according to the preparation steps of the present invention, and conducted tests on high temperature resistance, corrosion resistance and chemical erosion resistance. Finally, the raw materials and maintenance costs were evaluated. The test data and evaluation results are shown in Table 2 below: Table 2 Test items Test conditions Test Data Evaluation results High temperature resistance Temperature range: room temperature to 250°C No noticeable deformation or performance degradation Meet the high temperature use standards of aviation materials Corrosion resistance Soak in 3.5% NaCl solution for 48 hours The corrosion area is 1% Poor corrosion resistance Chemical resistance Exposure to acidic (pH 3) and alkaline (pH 11) environments for 24 hours each Quality loss 2% Poor resistance to chemical corrosion Raw material cost Compared with the existing composite panels, it is reduced by 6% The decline was 6% Cost-effectiveness analysis shows high cost-effectiveness Maintenance costs Compared with the existing composite panels, it increased by 4% The decline was 4% High maintenance cost under long-term use Machining performance Drilling, milling The processing accuracy is average and the surface quality is rough Not easy to machine and cannot meet the requirements of complex structural design Overall evaluation - - The comprehensive performance of the aviation carbon fiber composite sheet is average and is not suitable for use in the aerospace field From the above Tables 1 and 2, we know that: Comparative Example 1 lacks PBO fiber, bio-based epoxy resin and internal release agent, resulting in insufficient corrosion resistance and chemical erosion resistance of the carbon fiber composite sheet for aviation. Since there is no internal release agent for the inner coating of the mold, the surface quality of the sheet is rough and the processing accuracy is general. Although the reduction in raw materials reduces the cost of raw materials for the sheet, the overall performance of the sheet decreases, resulting in an increase in maintenance costs. Therefore, it is not suitable for use in the aerospace field.
[0032] In Example 1, the aviation carbon fiber composite sheet of the present invention uses PBO fiber, bio-based epoxy resin and internal release agent, so that the finished sheet has excellent high temperature resistance, corrosion resistance and chemical erosion resistance, and the raw material cost and maintenance cost are reduced by 5% and 3% respectively compared with the existing composite sheet, and the comprehensive cost has high cost performance. At the same time, due to the special processing process, the sheet has good mechanical processing performance, is easy to drill and mill, and meets the manufacturer's complex structural design requirements. Therefore, the aviation carbon fiber composite sheet of the present invention has excellent comprehensive performance and is suitable for use in the aerospace field.
[0033] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A carbon fiber composite sheet for aviation, characterized in that: The raw materials of composite panels are composed of carbon fiber, high-performance fiber, resin matrix, high-performance polymer and fusion agent; The specific weight ratios of raw materials are: asphalt-based carbon fiber 12%-15%; PE-based carbon fiber 7%-9%; PBO fiber 3%-6%; bismaleimide resin 11%-13%; bio-based epoxy resin 6%-8%; ultra-high molecular weight polyethylene 7%-12%; polyetheretherketone resin 4%-6%; low shrinkage additive 0.5%-1%; thickener 0.8%-1.1%; internal release agent 1%-1.3%; colorant 2%-2.5%; polyphenylene ether 3%-4%; polyetherimide 5%-6%.
2. The carbon fiber composite sheet for aviation according to claim 1, characterized in that: The carbon fiber is composed of asphalt-based carbon fiber and PE-based carbon fiber, and the high-performance fiber is PBO fiber.
3. The carbon fiber composite sheet for aviation according to claim 1, characterized in that: The resin matrix consists of bismaleimide, bio-based epoxy resin, polyetheretherketone resin and ultra-high molecular weight polyethylene.
4. The carbon fiber composite sheet for aviation according to claim 1, characterized in that: The high-performance polymer consists of polyphenylene ether and polyetherimide, and the fusing agent consists of a low-shrinkage additive, a thickener, an internal mold release agent and a colorant.
5. A process for preparing a carbon fiber composite sheet for aviation, characterized in that: According to claim 1, the carbon fiber composite sheet for aviation is prepared by the weight ratio of raw materials, and the preparation steps are: Step 1. Raw material preparation: Use a weighing instrument to weigh asphalt-based carbon fiber, PE-based carbon fiber, PBO fiber, bismaleimide resin, bio-based epoxy resin, ultra-high molecular weight polyethylene, polyetheretherketone resin, low shrinkage additive, thickener, internal release agent, colorant, polyphenylene ether and polyetherimide; Step 2: Preform preparation: the prepared raw materials are mixed evenly in a specific order to form a preform; Step 3: Laying the preform: Use an automatic tape laying machine to lay the preform on the mold; Step 4: Curing process: Select the autoclave process and set the curing conditions; Step 5: Post-processing of the board: After the curing is completed, the board is cut, ground and polished according to the manufacturer's design sample as a model; Step 6: Mechanical processing: Perform mechanical reprocessing as needed.
6. The process for preparing a carbon fiber composite sheet for aviation according to claim 5, characterized in that: The second step is to mix the raw materials in order: S1.
1. Add bismaleimide resin, bio-based epoxy resin, low shrinkage additive and thickener into a high-precision mixer, set the temperature to 60°C, and stir at a stirring speed of 500 r / min for 15 min; S1.2, adding the asphalt-based carbon fiber, PE-based carbon fiber and PBO fiber into the mixture in S1.1 at a rate of 10 kg / min, and stirring at a temperature of 100°C and a stirring speed of 1000 r / min for 8 min; S1.3, adding ultra-high molecular weight polyethylene and polyetheretherketone resin to the mixture of S1.2, stirring at a temperature of 120°C and a stirring speed of 600 r / min for 10 min; S1.4, add colorant, polyphenylene ether and polyetherimide, lower the temperature to 50°C, stir at a stirring speed of 1000 r / min for 15 minutes to complete the entire mixing process to form a preform.
7. The process for preparing a carbon fiber composite sheet for aviation according to claim 5, characterized in that: The paving process of the preform in step 3: S2.
1. Select the automatic tape laying machine as the mold laying equipment; S2.2, select a mold and apply a 1mm layer of inner release agent to the inner layer of the mold; S2.3, set the temperature of the automatic tape laying machine to 80°C; S2.
4. Set the flow rate of the automatic tape laying machine to 20-30m / s, set the pressure of the automatic tape laying machine to 0.5-1MPa, start the automatic tape laying machine, and after preheating for 30 minutes, inject the preform from the mixing equipment into the automatic tape laying machine to start laying the preform.
8. The process for preparing a carbon fiber composite sheet for aviation according to claim 5, characterized in that: The curing process in step 4 is as follows: the preformed body covered in the mold is placed in an autoclave, the temperature is set to 120° C., the duration is 30 minutes, and the pressure of the autoclave is set between 1-1.2 MPa.
9. The process for preparing a carbon fiber composite sheet for aviation according to claim 5, characterized in that: Post-processing of the plate in step 5: S3.
1. After curing is completed, cool the autoclave to room temperature and take out the composite sheet; S3.
2. Finally, the composite board is cut to the same specifications as the sample designed by the manufacturer, and then polished.
10. The process for preparing a carbon fiber composite sheet for aviation according to claim 5, characterized in that: Mechanical processing in step six: mechanical reprocessing is performed according to the manufacturer's type requirements, including drilling and milling, to meet specific assembly and use requirements.
Citation Information
Patent Citations
Epoxy-based resin composition for composite materials
CN107108854A
Prepreg, method for producing same, and slit tape prepreg
CN110191915A
Prepreg and production method therefor, slit tape prepreg, carbon fiber-reinforced composite material
CN112292419A
Automatic dry fiber laying material as well as preparation method and application thereof
CN117621486A