A method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels
By constructing micro-nano composites on the surface of wooden bathroom cabinet boards and preparing superhydrophobic and corrosion-resistant functional fillers, the problem of wooden boards being susceptible to mold erosion in humid environments has been solved, achieving superhydrophobicity and mold-killing ability, and improving service life.
Patent Information
- Application Number
- CN202411372793.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-09-29
AI Technical Summary
Existing bathroom cabinet wooden panels are susceptible to mold in humid environments. Coating treatments are difficult to achieve superhydrophobicity and self-cleaning effects, and mold can easily damage the coating, reducing its service life.
By constructing micro-nano composites on the surface of wood-based panels, superhydrophobic and corrosion-resistant functional fillers were prepared by modifying them with aminosilane coupling agents and adding ethyl chloroacetate and long-chain imidazole. These fillers were then blended with epoxy resin and a curing agent to form a coating with superhydrophobicity and antifungal properties.
It achieves superhydrophobicity and excellent mold-killing ability on the surface of bathroom cabinet panels, improving corrosion resistance and service life.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface treatment technology, and specifically relates to a corrosion-resistant and self-cleaning surface treatment method for bathroom cabinet panels. Background Technology
[0002] Bathroom vanities are cabinets used to store items in the bathroom. They are made of various types of boards, which can be broadly categorized into wood, stone, metal, and plastic. Wood, with its practicality, aesthetics, and high strength, has gradually become the mainstream material for bathroom vanity boards. However, wood generally has the disadvantage of high water absorption, making it prone to moisture absorption during actual use. This leads to extensive mold and corrosion, significantly reducing its lifespan and practicality. Therefore, many existing technologies involve surface treatments on bathroom vanity wood boards, such as lamination, to give them hydrophobic properties. However, these technologies still have certain drawbacks limiting their effectiveness. On the one hand, simple lamination treatments cannot achieve superhydrophobic properties and lack self-cleaning capabilities. On the other hand, the bathroom itself is an environment where mold thrives. Under the long-term combined action of moisture and humidity, the coating formed after lamination is also susceptible to mold erosion and damage, ultimately failing to achieve its intended effect. Summary of the Invention
[0003] To address the problems existing in the prior art, the purpose of this invention is to provide a corrosion-resistant and self-cleaning surface treatment method for bathroom cabinet panels. This invention uses silica as a micron-scale structure and constructs nano-scale titanium dioxide on its surface via a hydrothermal method to obtain a micro-nano composite. Then, an aminosilane coupling agent is used as a modifier to modify the surface with amino groups. Next, an ionic liquid containing carboxyl / long-chain alkanes, obtained by acidification of ethyl chloroacetate and long-chain imidazole through the action of halogen atoms and nitrogen, and a compounded dehydrorosin acid are added. Both react with the amino groups through dehydration condensation, thereby preparing a superhydrophobic and corrosion-resistant functional filler. When this filler is physically blended with epoxy resin and a curing agent in a small amount, the resulting coating, when applied to the surface of wooden or alloy panels of bathroom cabinets, not only possesses superhydrophobic properties and a self-cleaning effect, but also exhibits excellent mold-killing ability and very good resistance to mold corrosion.
[0004] The objective of this invention can be achieved through the following technical solutions:
[0005] A method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels, the method comprising the following steps:
[0006] (1) Coating is applied to the surface of the bathroom cabinet board, and dried to form a coating with a thickness of 0.2-0.25mm, which completes the treatment; the material of the bathroom cabinet board is wood or alloy; the coating includes epoxy resin, curing agent and superhydrophobic corrosion-resistant functional filler; the mass ratio of epoxy resin, curing agent and superhydrophobic corrosion-resistant functional filler is 40-42:10-12:1.
[0007] As a preferred embodiment of the present invention, the preparation method of the coating in step (1) includes the following steps:
[0008] Step X: Add the curing agent and the superhydrophobic and corrosion-resistant functional filler to the epoxy resin, and then mix them at room temperature for 10-15 minutes to complete the preparation.
[0009] As a preferred technical solution of the present invention, the drying in step (1) refers to drying at a temperature of 60-70℃ for 8-10 hours.
[0010] As a preferred technical solution of the present invention, the curing agent in step (1) is diethylenetriamine.
[0011] As a preferred technical solution of the present invention, the superhydrophobic and corrosion-resistant functional filler in step (1) is prepared by the following steps:
[0012] Step A: Add glacial acetic acid to 40-50 parts by weight of an aqueous ethanol solution until the pH is adjusted to 2.5-3 to obtain the first solution; add 0.1-0.15 parts by weight of silicon dioxide and 0.5-0.7 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stir at room temperature for 10-15 minutes to mix to obtain the second solution; add the second solution dropwise to the first solution while stirring, and after the addition is complete, carry out a hydrothermal reaction, filter, take the filter residue, wash with deionized water, then vacuum dry at 50-70℃ until constant weight, and finally heat to 500-520℃ at a heating rate of 4-6℃ / min and calcine for 2 hours to obtain the micro-nano composite;
[0013] Step B: Add 0.1-0.2 parts by weight of deionized water, 1 part by weight of micro-nano composite and 0.2-0.25 parts by weight of aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stir at 70-75℃ for 10-12 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 50-70℃ until constant weight to obtain amino-modified micro-nano composite.
[0014] Step C: Add 5-6 parts by weight of long-chain imidazole to 6-7 parts by weight of ethyl chloroacetate, stir at 60-65℃ for 24-26 hours, cool naturally to room temperature, filter, remove the filtrate, wash with ether, then add 45-50 parts by weight of deionized water and 8-10 parts by weight of concentrated hydrochloric acid with a mass fraction of 35-38%, and finally stir at 30-35℃ for 20-24 hours to remove impurities and obtain an ionic liquid;
[0015] Step D: Add 1-2 parts by weight of amino-modified micro / nano complex, 0.3-0.4 parts by weight of ionic liquid and 0.1-0.2 parts by weight of dehydrorosin acid to 60-80 parts by weight of anhydrous ethanol. Mix at room temperature for 5-10 minutes, adjust the pH to 3-3.5 with hydrochloric acid solution, stir at 65-70℃ for 6-8 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 50-70℃ until constant weight. The preparation is complete.
[0016] Furthermore, the ethanol-water solution in step A has a mass fraction of 45-50%.
[0017] Furthermore, the particle size of the silica in step A is 2-3 micrometers.
[0018] Furthermore, the dripping rate described in step A is controlled at 1-2 drops / s.
[0019] Furthermore, the hydrothermal reaction described in step A refers to heating the reactor to 190-200°C at a heating rate of 3-5°C / min and then holding the temperature at that temperature for 24 hours.
[0020] Further, the aminosilane coupling agent in step B is γ-aminopropyltrimethoxysilane.
[0021] Further, the long-chain imidazole in step C is at least one of 1-pentylimidazolium, N-hexylimidazolium, and N-decylimidazolium.
[0022] Further, step C, which involves removing impurities, refers to distilling at 50°C under a vacuum of -0.08 MPa until all volatiles are removed, followed by washing with ether, and finally vacuum drying at 40-45°C until constant weight.
[0023] Furthermore, the hydrochloric acid solution in step D has a mass fraction of 15-20%.
[0024] The beneficial effects of this invention are:
[0025] (1) This invention uses silicon dioxide as a micron-scale structure and constructs nano-scale titanium dioxide on its surface by hydrothermal method to obtain a micro-nano composite. Then, an aminosilane coupling agent is used as a modifier to modify the amino groups. Next, an ionic liquid containing carboxyl / long-chain alkanes, obtained by acidification of ethyl chloroacetate and long-chain imidazole through the action of halogen atoms and nitrogen, and dehydroabrasive acid are added. The two react together with the amino groups to undergo dehydration condensation, thereby preparing a superhydrophobic and corrosion-resistant functional filler. When the coating obtained by physical blending it with epoxy resin and curing agent with a small amount is applied to the surface coating of wooden or alloy boards of bathroom cabinets, the resulting coating not only has superhydrophobic properties and a self-cleaning effect, but also has excellent fungicidal ability and very good resistance to fungal corrosion.
[0026] (2) This invention creatively combines micron-sized silica and nano-sized titanium dioxide through a hydrothermal method to construct a micro-nano structure. Based on this, amino modification of silane coupling agent and co-grafting of ionic liquid / dehydrorosin acid are carried out sequentially to finally prepare a superhydrophobic and corrosion-resistant functional filler. It can achieve superhydrophobic properties and excellent bactericidal ability with only a small amount of addition. As an imidazole salt compound, the ionic liquid not only has a good bactericidal effect, but its long-chain alkane structure can also endow it with low surface energy. Dehydrorosin acid itself has many biological activities, such as antibacterial properties. At the same time, from a structural point of view, one of its end groups is also isopropyl, which has strong hydrophobicity. Therefore, after co-grafting with ionic liquid, it can produce a certain synergistic effect and play an excellent role together.
[0027] (3) The surface treatment method provided by the present invention is universal. Even for other materials such as alloy plates, it has the same excellent technical effect, that is, it can give the surface superhydrophobic properties and antibacterial properties. Detailed Implementation
[0028] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with embodiments, is provided below.
[0029] The epoxy resin used in all embodiments and comparative examples of this invention was purchased directly from the market, specifically from Hansoh, model EPIKOTE 6520-WH-53A; the wood used was oak.
[0030] Example 1
[0031] A method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels, the method comprising the following steps:
[0032] (1) Coating is applied to the surface of the bathroom cabinet board, and dried to form a coating with a thickness of 0.2mm, thus completing the treatment; the material of the bathroom cabinet board is wood; the coating includes epoxy resin, curing agent and superhydrophobic corrosion-resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the superhydrophobic corrosion-resistant functional filler is 40:10:1.
[0033] The preparation method of the coating in step (1) includes the following steps:
[0034] Step X: Add the curing agent and the superhydrophobic and corrosion-resistant functional filler to the epoxy resin, and then stir at room temperature for 10 minutes to mix, thus completing the preparation.
[0035] The drying in step (1) refers to drying at a temperature of 60°C for 8 hours.
[0036] The curing agent in step (1) is diethylenetriamine.
[0037] The superhydrophobic and corrosion-resistant functional filler described in step (1) is prepared through the following steps:
[0038] Step A: Add glacial acetic acid to 40 parts by weight of an aqueous ethanol solution until the pH is adjusted to 2.5 to obtain the first solution; add 0.1 parts by weight of silicon dioxide and 0.5 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stir at room temperature for 10 min to mix to obtain the second solution; add the second solution dropwise to the first solution while stirring, and after the addition is complete, carry out a hydrothermal reaction, filter, take the filter residue, wash with deionized water, then vacuum dry at 50℃ until constant weight, and finally heat to 500℃ at a heating rate of 4℃ / min and calcine for 2 h to obtain the micro-nano composite.
[0039] Step B: Add 0.1 parts by weight of deionized water, 1 part by weight of micro-nano composite and 0.2 parts by weight of aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stir at 70°C for 10 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 50°C until constant weight to obtain amino-modified micro-nano composite.
[0040] Step C: Add 5 parts by weight of long-chain imidazole to 6 parts by weight of ethyl chloroacetate, stir at 60°C for 24 hours, cool naturally to room temperature, filter, remove the filtrate, wash with ether, then add 45 parts by weight of deionized water and 8 parts by weight of 35% concentrated hydrochloric acid, and finally stir at 30°C for 20 hours to remove impurities and obtain ionic liquid.
[0041] Step D: Add 1 part by weight of amino-modified micro / nano complex, 0.3 parts by weight of ionic liquid and 0.1 parts by weight of dehydrorosin acid to 60 parts by weight of anhydrous ethanol. Mix at room temperature for 5 minutes, adjust the pH to 3 with hydrochloric acid solution, stir at 65°C for 6 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 50°C until constant weight. The preparation is complete.
[0042] The ethanol-water solution in step A has a mass fraction of 45%.
[0043] The silica particles in step A have a particle size of 2 micrometers.
[0044] The dropping rate in step A is controlled at 1 drop / s.
[0045] The hydrothermal reaction mentioned in step A refers to heating the reactor to 190°C at a heating rate of 3°C / min and then holding the temperature for 24 hours.
[0046] The aminosilane coupling agent mentioned in step B is γ-aminopropyltrimethoxysilane.
[0047] The long-chain imidazole mentioned in step C is N-n-decylimidazol.
[0048] The removal of impurities in step C refers to distillation at 50°C under a vacuum of -0.08 MPa until all volatiles are removed, followed by washing with ether and finally vacuum drying at 40°C until constant weight.
[0049] The hydrochloric acid solution in step D has a mass fraction of 15%.
[0050] Example 2
[0051] A method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels, the method comprising the following steps:
[0052] (1) Coating is applied to the surface of the bathroom cabinet board, and dried to form a coating with a thickness of 0.25mm, thus completing the treatment; the material of the bathroom cabinet board is wood; the coating includes epoxy resin, curing agent and superhydrophobic corrosion-resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the superhydrophobic corrosion-resistant functional filler is 42:12:1.
[0053] The preparation method of the coating in step (1) includes the following steps:
[0054] Step X: Add the curing agent and the superhydrophobic and corrosion-resistant functional filler to the epoxy resin, and then stir at room temperature for 15 minutes to mix, thus completing the preparation.
[0055] The drying in step (1) refers to drying at a temperature of 70°C for 10 hours.
[0056] The curing agent in step (1) is diethylenetriamine.
[0057] The superhydrophobic and corrosion-resistant functional filler described in step (1) is prepared through the following steps:
[0058] Step A: Add glacial acetic acid to 50 parts by weight of an aqueous ethanol solution until the pH is adjusted to 3 to obtain the first solution; add 0.15 parts by weight of silica and 0.7 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stir at room temperature for 15 min to mix to obtain the second solution; add the second solution dropwise to the first solution while stirring, and after the addition is complete, carry out a hydrothermal reaction, filter, take the filter residue, wash with deionized water, then vacuum dry at 70℃ until constant weight, and finally heat to 520℃ at a heating rate of 6℃ / min and calcine for 2 h to obtain the micro-nano composite;
[0059] Step B: Add 0.2 parts by weight of deionized water, 1 part by weight of micro-nano composite and 0.25 parts by weight of aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stir at 75°C for 12 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 70°C until constant weight to obtain amino-modified micro-nano composite.
[0060] Step C: Add 6 parts by weight of long-chain imidazole to 7 parts by weight of ethyl chloroacetate, stir at 65°C for 26 hours, cool naturally to room temperature, filter, remove the filtrate, wash with ether, then add 50 parts by weight of deionized water and 10 parts by weight of concentrated hydrochloric acid with a mass fraction of 38%, and finally stir at 35°C for 24 hours to remove impurities and obtain ionic liquid.
[0061] Step D: Add 2 parts by weight of amino-modified micro / nano complex, 0.4 parts by weight of ionic liquid and 0.2 parts by weight of dehydrorosin acid to 80 parts by weight of anhydrous ethanol. Mix at room temperature for 10 minutes, adjust the pH to 3.5 with hydrochloric acid solution, stir at 70°C for 8 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 70°C until constant weight is achieved. The preparation is now complete.
[0062] The ethanol-water solution in step A has a mass fraction of 50%.
[0063] The silica particles in step A have a diameter of 3 micrometers.
[0064] The dripping rate in step A is controlled at 2 drops / s.
[0065] The hydrothermal reaction mentioned in step A refers to heating the reactor to 200°C at a heating rate of 5°C / min and then holding the temperature for 24 hours.
[0066] The aminosilane coupling agent mentioned in step B is γ-aminopropyltrimethoxysilane.
[0067] The long-chain imidazole mentioned in step C is N-n-decylimidazol.
[0068] The removal of impurities in step C refers to distillation at 50°C under a vacuum of -0.08 MPa until all volatiles are removed, followed by washing with ether and finally vacuum drying at 45°C until constant weight.
[0069] The hydrochloric acid solution in step D has a mass fraction of 20%.
[0070] Example 3
[0071] A method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels, the method comprising the following steps:
[0072] (1) Coating is applied to the surface of the bathroom cabinet board, and dried to form a coating with a thickness of 0.23mm, thus completing the treatment; the material of the bathroom cabinet board is wood; the coating includes epoxy resin, curing agent and superhydrophobic corrosion-resistant functional filler; the mass ratio of the epoxy resin, the curing agent and the superhydrophobic corrosion-resistant functional filler is 41:11:1.
[0073] The preparation method of the coating in step (1) includes the following steps:
[0074] Step X: Add the curing agent and the superhydrophobic and corrosion-resistant functional filler to the epoxy resin, and then stir at room temperature for 13 minutes to mix, thus completing the preparation.
[0075] The drying in step (1) refers to drying at a temperature of 65°C for 9 hours.
[0076] The curing agent in step (1) is diethylenetriamine.
[0077] The superhydrophobic and corrosion-resistant functional filler described in step (1) is prepared through the following steps:
[0078] Step A: Add glacial acetic acid to 45 parts by weight of an aqueous ethanol solution until the pH is adjusted to 2.8 to obtain the first solution; add 0.13 parts by weight of silica and 0.6 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stir at room temperature for 13 min to mix to obtain the second solution; add the second solution dropwise to the first solution while stirring, and after the addition is complete, carry out a hydrothermal reaction, filter, take the filter residue, wash with deionized water, then vacuum dry at 60℃ until constant weight, and finally heat to 510℃ at a heating rate of 5℃ / min and calcine for 2 h to obtain the micro-nano composite;
[0079] Step B: Add 0.15 parts by weight of deionized water, 1 part by weight of micro-nano composite and 0.23 parts by weight of aminosilane coupling agent to 60 parts by weight of anhydrous ethanol, stir at 73°C for 11 hours, filter, take the filter residue, wash with deionized water, and finally vacuum dry at 60°C until constant weight to obtain amino-modified micro-nano composite.
[0080] Step C: Add 5.5 parts by weight of long-chain imidazole to 6.5 parts by weight of ethyl chloroacetate, stir at 63°C for 25 hours, cool naturally to room temperature, filter, remove the filtrate, wash with ether, then add 48 parts by weight of deionized water and 9 parts by weight of concentrated hydrochloric acid with a mass fraction of 36%, and finally stir at 33°C for 22 hours to remove impurities and obtain an ionic liquid;
[0081] Step D: Add 1.5 parts by weight of amino-modified micro / nano composite, 0.35 parts by weight of ionic liquid and 0.15 parts by weight of dehydrorosin acid to 70 parts by weight of anhydrous ethanol. Mix at room temperature for 8 minutes, adjust the pH to 3.3 with hydrochloric acid solution, stir at 68°C for 7 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 60°C until constant weight. The preparation is complete.
[0082] The ethanol-water solution in step A has a mass fraction of 48%.
[0083] The silica particles in step A have a diameter of 3 micrometers.
[0084] The dripping rate in step A is controlled at 1.5 drops / s.
[0085] The hydrothermal reaction described in step A refers to heating the reactor to 195°C at a heating rate of 4°C / min and then holding the temperature at that temperature for 24 hours.
[0086] The aminosilane coupling agent mentioned in step B is γ-aminopropyltrimethoxysilane.
[0087] The long-chain imidazole mentioned in step C is N-n-decylimidazol.
[0088] The removal of impurities in step C refers to distillation at 50°C under a vacuum of -0.08 MPa until all volatiles are removed, followed by washing with ether and finally vacuum drying at 43°C until constant weight.
[0089] The hydrochloric acid solution in step D has a mass fraction of 18%.
[0090] Comparative Example 1
[0091] Based on Example 1, in step A, tetrabutyl titanate was replaced with an equal weight of deionized water, while all other steps remained unchanged.
[0092] Comparative Example 2
[0093] Based on Example 1, the ionic liquid in step D is replaced with an equal weight of dehydrorosin acid, while the rest remain unchanged.
[0094] Comparative Example 3
[0095] Based on Example 1, in step D, dehydrorosin acid was replaced with an ionic liquid of equal weight, while all other steps remained unchanged.
[0096] Test Example 1
[0097] Hydrophobicity test:
[0098] Static contact angle and rolling contact angle tests were conducted on the bathroom cabinet panels with the surface treatment completed in Examples 1-3 and Comparative Examples 1-3, respectively.
[0099] Table 1. Hydrophobicity test results
[0100] Static contact angle / ° Rolling contact angle / ° Example 1 156.2 6.0 Example 2 158.1 5.7 Example 3 156.4 5.9 Comparative Example 1 134.3 30.7 Comparative Example 2 144.4 16.9 Comparative Example 3 146.2 16.3
[0101] Test Example 2
[0102] Antibacterial performance test:
[0103] The bathroom cabinet boards with surface treatment completed in Examples 1-3 and Comparative Examples 1-3 were subjected to antibacterial performance testing (film application method) according to standard GB / T 21510-2008. The tested bacteria was Aspergillus flavus.
[0104] Table 1. Results of antibacterial performance test
[0105] Antibacterial rate / % Example 1 99.89 Example 2 99.90 Example 3 99.90 Comparative Example 1 99.87 Comparative Example 2 82.11 Comparative Example 3 87.52
[0106] As can be seen from the comparison of Example 1 and Comparative Examples 1-3 in Test Examples 1-2, the bathroom cabinet board obtained after the surface treatment of the present invention not only has superhydrophobic properties and a self-cleaning effect, but also has excellent anti-mold killing ability and very good resistance to mold corrosion.
[0107] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels, characterized in that, Includes the following steps: (1) Coating is applied to the surface of the bathroom cabinet board, and dried to form a coating with a thickness of 0.2-0.25mm, thus completing the treatment; the material of the bathroom cabinet board is wood or alloy; the coating includes epoxy resin, curing agent and superhydrophobic corrosion-resistant functional filler; the mass ratio of epoxy resin, curing agent and superhydrophobic corrosion-resistant functional filler is 40-42:10-12:1; The superhydrophobic and corrosion-resistant functional filler is prepared through the following steps: Step A: Add glacial acetic acid to 40-50 parts by weight of an aqueous ethanol solution until the pH is adjusted to 2.5-3 to obtain the first solution; add 0.1-0.15 parts by weight of silicon dioxide and 0.5-0.7 parts by weight of tetrabutyl titanate to 20 parts by weight of anhydrous ethanol, and then stir at room temperature for 10-15 minutes to mix to obtain the second solution; add the second solution dropwise to the first solution while stirring, and after the addition is complete, carry out a hydrothermal reaction, filter, take the filter residue, wash with deionized water, then vacuum dry at 50-70℃ until constant weight, and finally heat to 500-520℃ at a heating rate of 4-6℃ / min and calcine for 2 hours to obtain the micro-nano composite; Step B: Add 0.1-0.2 parts by weight of deionized water, 1 part by weight of the micro / nano composite, and 0.2-0.25 parts by weight of aminosilane coupling agent to 60 parts by weight of anhydrous ethanol. Then stir at 70-75℃ for 10-12 hours, filter, collect the filter residue, wash with deionized water, and finally vacuum dry at 50-70℃ until constant weight to obtain the amino-modified micro / nano composite; the aminosilane coupling agent is γ-aminopropyltrimethoxysilane. Step C: Add 5-6 parts by weight of long-chain imidazole to 6-7 parts by weight of ethyl chloroacetate, stir at 60-65°C for 24-26 hours, cool naturally to room temperature, filter, remove the filtrate, wash with diethyl ether, then add 45-50 parts by weight of deionized water and 8-10 parts by weight of concentrated hydrochloric acid with a mass fraction of 35-38%, and finally stir at 30-35°C for 20-24 hours to remove impurities and obtain an ionic liquid; the long-chain imidazole is at least one of 1-pentylimidazolium, N-hexylimidazolium, and N-decylimidazolium; the removal of impurities refers to distillation at 50°C under a vacuum of -0.08 MPa until all volatiles are removed, then washing with diethyl ether, and finally vacuum drying at 40-45°C until constant weight; Step D: Add 1-2 parts by weight of amino-modified micro / nano complex, 0.3-0.4 parts by weight of ionic liquid and 0.1-0.2 parts by weight of dehydrorosin acid to 60-80 parts by weight of anhydrous ethanol. Mix at room temperature for 5-10 minutes, adjust the pH to 3-3.5 with hydrochloric acid solution, stir at 65-70℃ for 6-8 hours, filter, take the filter residue, wash with anhydrous ethanol, and finally vacuum dry at 50-70℃ until constant weight. The preparation is complete.
2. The method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The preparation method of the coating in step (1) includes the following steps: adding the curing agent and the superhydrophobic and corrosion-resistant functional filler to the epoxy resin, and then mixing them at room temperature for 10-15 minutes to complete the preparation.
3. The method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The drying in step (1) refers to drying at a temperature of 60-70℃ for 8-10 hours.
4. The method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The curing agent in step (1) is diethylenetriamine.
5. The method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The silica particles in step A have a particle size of 2-3 micrometers.
6. The method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The hydrothermal reaction described in step A refers to heating the reactor to 190-200℃ at a heating rate of 3-5℃ / min and then holding the temperature at that temperature for 24 hours.
7. The method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The ethanol aqueous solution in step A has a mass fraction of 45-50%.
8. The method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The dripping rate in step A is controlled at 1-2 drops / s.
9. A method for corrosion-resistant and self-cleaning surface treatment of bathroom cabinet panels according to claim 1, characterized in that, The hydrochloric acid solution in step D has a mass fraction of 15-20%.
Citation Information
Patent Citations
Method for preparing nano silicon dioxide coated by nano titanium dioxide
CN101613537A
Method for preparing nanometer titanium dioxide coated nanometer silicon dioxide film
CN102416314A