Autocatalytic palm oil-based dynamic covalent polymer material and application thereof

Through the preparation of autocatalytic palm oil-based dynamic covalent polymer materials, the toxic catalyst and non-renewable problems in traditional polyurethane acrylate materials are solved, and a green and environmentally friendly high-performance steel anticorrosion coating is realized, with good mechanical properties and recyclability .

CN119019927APending Publication Date: 2024-11-26刘文地
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411149089.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional polyurethane acrylate materials use toxic catalysts during the preparation process and are non-renewable and recyclable, resulting in environmental pollution and limited resources.

Method used

The autocatalytic dynamic covalent polymer material is prepared using palm oil base material. The autocatalysis of palm oil diethanolamide is utilized by the combination of acrylate-capped palm oil-based polyurethane linear oligomer, hydroxyethyl acrylate and photoinitiator. , realize the preparation of organometallic catalysts without the need, and form self-healing and recyclable steel anticorrosion coatings through ultraviolet light curing.

Benefits of technology

It realizes the green and environmental protection of bio-based polymer materials, has good mechanical properties and self-repairability, reduces environmental pollution, is cheap and has large output, and solves the problems of non-renewable and recycling of traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019927A_ABST
    Figure CN119019927A_ABST
Patent Text Reader

Abstract

The invention discloses an autocatalytic palm oil-based dynamic covalent polymer material and application thereof, and belongs to the technical field of bio-based dynamic polymer materials. According to the invention, palm oil-based dihydric alcohol is used as a raw material and is subjected to polycondensation with diisocyanate and hydroxyethyl acrylate to obtain an acrylate-terminated palm oil-based polyurethane linear oligomer, and then the acrylate-terminated palm oil-based polyurethane linear oligomer and hydroxyethyl acrylate are prepared into the catalyst-free palm oil-based dynamic covalent polymer material under the action of a photoinitiator. The autocatalytic palm oil-based dynamic covalent polymer material prepared by the invention not only is environment-friendly in raw material source, but also does not need to use an organic metal catalyst in the preparation process, and has good mechanical properties, self-repairability and recoverability; the steel anticorrosive paint prepared by using the epoxy resin has good adhesive force, flexibility, impact resistance, solvent wiping resistance, water resistance and salt fog resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of bio-based dynamic polymer materials, and in particular relates to a self-catalytic palm oil-based dynamic covalent polymer material and an application thereof. Background Art

[0002] Polyurethane acrylate is a recognized high-performance photocurable resin that is highly favored in the coating field for its excellent mechanical strength, hardness and adhesion. However, the preparation process of polyurethane acrylate requires the use of catalysts such as highly toxic organotin compounds. Since the catalysts in the polymer are difficult to remove, the use of highly toxic catalysts leads to a series of production safety and environmental problems. At the same time, the preparation of traditional polyurethane acrylates usually relies on petroleum-based polyols. Considering the limited nature of petroleum resources, this dependence may limit its future application. In addition, the recycling difficulties associated with polyurethane acrylates have also triggered the generation of a large amount of waste plastics, causing immeasurable harm to the environment. Therefore, the development of repairable and recyclable polyurethane acrylate materials will help significantly alleviate these problems. Summary of the invention

[0003] The purpose of the present invention is to synthesize a dynamic covalent polymer material without the use of an organic metal catalyst using a palm oil-based material as a raw material. The dynamic polymer material has good mechanical strength and self-healing properties, and can reduce pollution to the environment. It can solve the problems of non-renewable raw materials of traditional polyurethane acrylates, the use of toxic catalysts in the preparation process, and the non-recyclability of thermosetting three-dimensional network structures. The material can be used to prepare a self-healing and recyclable steel anti-corrosion coating, and the resulting steel anti-corrosion coating has good corrosion resistance.

[0004] To achieve the above object, the present invention adopts the following technical solution: A self-catalytic palm oil-based dynamic covalent polymer material comprises the following raw materials by mass: 78 parts of acrylate-terminated palm oil-based polyurethane linear oligomers, 20 parts of hydroxyethyl acrylate and 2 parts of a photoinitiator.

[0005] Furthermore, the acrylate-terminated palm oil-based polyurethane linear oligomer is prepared from the following raw materials in parts by mass: 2.62-5.77 parts of palm oil diethanolamide, 0.29-1.46 parts of isosorbide, 1.01 parts of hexamethylene diisocyanate, 5.56 parts of isophorone diisocyanate, 2.32 parts of hydroxyethyl acrylate and 10 parts of butanone. The preparation method is to mix palm oil diethanolamide, hexamethylene diisocyanate and butanone in proportion and introduce N2, and stir magnetically in an oil bath at 75°C for 1 hour; then add isophorone diisocyanate, continue stirring for 1 hour, then add isosorbide, continue stirring for 4 hours, and finally add hydroxyethyl acrylate, and continue stirring for 2 hours.

[0006] Furthermore, the photoinitiator is 1-hydroxycyclohexyl phenyl ketone.

[0007] The preparation method of the self-catalytic palm oil-based dynamic covalent polymer material is to mix acrylate-terminated palm oil-based polyurethane linear oligomer, hydroxyethyl acrylate and a photoinitiator in proportion, stir them evenly with a magnetic stirrer at room temperature, pour them into a mold, irradiate the mold under a 360 W ultraviolet light source for 2 min (during the ultraviolet irradiation process, the distance between the ultraviolet light source and the mold is 15 cm), and then cure the mold to obtain the self-catalytic palm oil-based dynamic covalent polymer material.

[0008] The method for preparing steel anti-corrosion coating using the self-catalytic palm oil-based dynamic covalent polymer material is to uniformly coat the uncured self-catalytic palm oil-based dynamic covalent polymer material on the surface of the steel, then expose the coating on the surface of the steel to an ultraviolet light source for curing, and then obtain the steel anti-corrosion coating after tempering.

[0009] The specific steps are as follows: after wiping and drying Q215 steel with ethanol, use a 100 μm wet film preparation device to evenly coat an appropriate amount of acrylate-terminated palm oil-based polyurethane linear oligomer, hydroxyethyl acrylate and photoinitiator on the steel surface in proportion, expose the coating on the steel surface to a 360 W ultraviolet light source for 2 min (the distance between the ultraviolet light source and the steel surface is kept at 15 cm during the irradiation process), then place the coated steel in a 120 ℃ oven for 12 hours, and after cooling to room temperature, an anti-corrosion coating is formed on the steel surface.

[0010] The beneficial effects of the present invention are: (1) The self-catalytic palm oil-based dynamic covalent polymer material prepared by the present invention is a type of polyurethane acrylate with high bio-based content, no toxic catalyst, and environmental friendliness; it uses low-priced, high-yield, green and harmless palm oil-based materials as raw materials, providing a new idea for the preparation of photocurable resins from palm oil raw materials.

[0011] (2) The present invention utilizes the self-catalytic effect of the tertiary amine group in the palm oil diethanolamide structure to prepare a palm oil-based dynamic covalent network polymer material, so that no organic metal catalyst is required in its preparation, and its mechanical properties are comparable to those of traditional polymer materials prepared using organic tin catalysts. At the same time, it has excellent self-healing and recyclable properties.

[0012] (3) The present invention adopts an optimized combination of process parameters, namely, using palm oil-based diethanolamide and isosorbide in a mass ratio of 2.7:1 to prepare acrylate-terminated palm oil-based polyurethane linear oligomers, hydroxyethyl acrylate, and photoinitiator in a dosage ratio of 78 wt%, 20 wt% and 2 wt%, respectively, to prepare a dynamic covalent network with good scratch repair and recyclability, and its tensile properties, hardness, adhesion, flexibility, impact resistance and other properties are excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 This is a comparison diagram of the tensile stress and tensile strain of the self-catalytic palm oil-based dynamic covalent polymer materials prepared in Examples 1 to 5.

[0014] Figure 2 This is a comparison chart of the tensile stress and tensile strain of the self-catalytic palm oil-based dynamic covalent polymer material prepared in Example 2 and the organotin-catalyzed palm oil-based polymer material prepared in the comparative example.

[0015] Figure 3 This is the kinetic differential calorimetry scanning curve of the self-catalytic palm oil-based dynamic covalent polymer material prepared in Examples 1 to 5.

[0016] Figure 4 The lap shear strength between the self-catalytic palm oil-based dynamic covalent polymer material prepared in Example 2 and different materials.

[0017] Figure 5 This is the scratch repair condition of the self-catalytic palm oil-based dynamic covalent polymer material prepared in Example 2.

[0018] Figure 6 This is a comparison diagram of the tensile stress and tensile strain of the self-catalytic palm oil-based dynamic covalent polymer material prepared in Example 2 before and after recovery. DETAILED DESCRIPTION

[0019] A self-catalytic palm oil-based dynamic covalent polymer material is prepared by mixing 78 parts of acrylate-terminated palm oil-based polyurethane linear oligomer, 20 parts of hydroxyethyl acrylate and 2 parts of a photoinitiator by weight, stirring the mixture evenly under magnetic stirring (50 r / min) at room temperature, and then pouring the mixture into a polytetrafluoroethylene mold. The mold is irradiated under a 360 W ultraviolet light source for 2 min (during the ultraviolet irradiation process, the distance between the ultraviolet light source and the mold is 15 cm) to cure the mixture.

[0020] The acrylate-terminated palm oil-based polyurethane linear oligomer is prepared by mixing 2.62-5.77 parts of palm oil diethanolamide, 1.01 parts of hexamethylene diisocyanate and 10 parts of butanone by mass, introducing N2, and magnetically stirring in an oil bath at 75°C for 1 hour; then adding 5.56 parts of isophorone diisocyanate, continuing to stir for 1 hour, then adding 0.29-1.46 parts of isosorbide, continuing to stir for 4 hours, and finally adding 2.32 parts of hydroxyethyl acrylate, and continuing to stir for 2 hours.

[0021] The photoinitiator is 1-hydroxycyclohexyl phenyl ketone.

[0022] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0023] Raw materials: Palm oil (melting point: 18 °C; acid value: 0.16 mg KOH / g) was purchased from Shanghai Dingfen Chemical Technology Co., Ltd., China; isosorbide, hexamethylene diisocyanate, isophorone diisocyanate, hydroxyethyl acrylate and diethanolamine were purchased from Shanghai Jingchun (Aladdin) Industrial Co., Ltd.; sodium chloride, ethyl acetate and sodium methoxide were purchased from Shanghai Sinopharm Chemical Reagent Co., Ltd.; butanone was purchased from Tianjin Daqiu Zhuanghongda Co., Ltd.

[0024] The palm oil-based diethanolamide used was synthesized using palm oil and diethanolamine as raw materials and sodium methoxide as a catalyst. The synthesis method was as follows: a 1000 mL three-necked flask equipped with a mechanical stirrer was placed in an oil bath and N2 was introduced, followed by the addition of diethanolamine (124.9 g) and sodium methoxide (1.62 g). After stirring at 80 °C for 20 min, palm oil (200 g) was added and the oil bath was heated to 120 °C, mechanically stirred for 4 h, and the product was cooled to room temperature, mixed evenly with ethyl acetate, added with a saturated NaCl solution for repeated purification for 3 to 5 times, and then rotary evaporated for purification for 3 h to obtain palm oil diethanolamide.

[0025] Example 1 Palm oil diethanolamide (5.77 g), hexamethylene diisocyanate (1.01 g) and butanone (10 g) were added into a 250 ml three-necked flask, and N2 was introduced. The mixture was stirred magnetically (200 r / min) for 1 h in an oil bath at 75 °C. Isophorone diisocyanate (5.56 g) was added and the stirring was continued for 1 h. Isosorbide (0.29 g, the mass ratio of palm oil diethanolamide to isosorbide was 19.9:1) was added and the stirring was continued for 4 h. Hydroxyethyl acrylate (2.32 g) was added and the stirring was continued for 2 h to obtain acrylate-terminated palm oil-based polyurethane linear oligomers. Acrylate-terminated palm oil-based polyurethane linear oligomers (15.6 g), hydroxyethyl acrylate (4 g) and initiator 1-hydroxycyclohexyl phenyl ketone (0.4 g) were magnetically stirred (50 r / min) for 5 min at room temperature to make them uniform, and then 100 A wet film preparation device with a diameter of 1 μm was used to evenly coat it on the surface of the steel that had been wiped with ethanol and dried. The coating on the steel surface was exposed to a 360 W ultraviolet light source for 2 min (the distance between the ultraviolet light source and the steel surface was kept at 15 cm during the irradiation process). The coated steel was then placed in an oven at 120 ℃ for 12 h. After cooling to room temperature, the steel anti-corrosion coating was obtained, which was recorded as PUA1.

[0026] Example 2 Palm oil diethanolamide (4.24 g), hexamethylene diisocyanate (1.01 g) and butanone (10 g) were added into a 250 ml three-necked flask, and N2 was introduced. The mixture was stirred magnetically (200 r / min) for 1 h in an oil bath at 75 °C. Isophorone diisocyanate (5.56 g) was added and the stirring was continued for 1 h. Isosorbide (0.58 g, the mass ratio of palm oil diethanolamide to isosorbide is 7.3:1) was added and the stirring was continued for 4 h. Hydroxyethyl acrylate (2.32 g) was added and the stirring was continued for 2 h to obtain acrylate-terminated palm oil-based polyurethane linear oligomers. Acrylate-terminated palm oil-based polyurethane linear oligomers (15.6 g), hydroxyethyl acrylate (4 g) and initiator 1-hydroxycyclohexyl phenyl ketone (0.4 g) were magnetically stirred (50 r / min) for 5 min at room temperature to make them uniform, and then 100 A wet film preparation device with a diameter of 1 μm was used to evenly coat it on the surface of the steel that had been wiped with ethanol and dried. The coating on the steel surface was exposed to a 360 W ultraviolet light source for 2 min (the distance between the ultraviolet light source and the steel surface was kept at 15 cm during the irradiation process). The coated steel was then placed in an oven at 120 ℃ for 12 h. After cooling to room temperature, an anti-corrosion coating for steel was obtained, which was recorded as PUA2.

[0027] Example 3 Palm oil diethanolamide (3.71 g), hexamethylene diisocyanate (1.01 g) and butanone (10 g) were added into a 250 ml three-necked flask, and N2 was introduced. The mixture was stirred magnetically (200 r / min) for 1 h in an oil bath at 75 °C. Isophorone diisocyanate (5.56 g) was added and the stirring was continued for 1 h. Isosorbide (0.87 g, the mass ratio of palm oil diethanolamide to isosorbide was 4.2:1) was added and the stirring was continued for 4 h. Hydroxyethyl acrylate (2.32 g) was added and the stirring was continued for 2 h to obtain acrylate-terminated palm oil-based polyurethane linear oligomers. Acrylate-terminated palm oil-based polyurethane linear oligomers (15.6 g), hydroxyethyl acrylate (4 g) and initiator 1-hydroxycyclohexyl phenyl ketone (0.4 g) were magnetically stirred (50 r / min) for 5 min at room temperature to make them uniform, and then 100 A wet film preparation device with a diameter of 1 μm was used to evenly coat it on the surface of the steel that had been wiped with ethanol and dried. The coating on the steel surface was exposed to a 360 W ultraviolet light source for 2 min (the distance between the ultraviolet light source and the steel surface was kept at 15 cm during the irradiation process). The coated steel was then placed in an oven at 120 ℃ for 12 h. After cooling to room temperature, an anti-corrosion coating for steel was obtained, which was recorded as PUA3.

[0028] Example 4 Palm oil diethanolamide (3.18 g), hexamethylene diisocyanate (1.01 g) and butanone (10 g) were added into a 250 ml three-necked flask, and N2 was introduced. The mixture was stirred magnetically (200 r / min) for 1 h in an oil bath at 75 °C. Isophorone diisocyanate (5.56 g) was added and the stirring was continued for 1 h. Isosorbide (1.17 g, the mass ratio of palm oil diethanolamide to isosorbide was 2.7:1) was added and the stirring was continued for 4 h. Hydroxyethyl acrylate (2.32 g) was added and the stirring was continued for 2 h to obtain acrylate-terminated palm oil-based polyurethane linear oligomers. Acrylate-terminated palm oil-based polyurethane linear oligomers (15.6 g), hydroxyethyl acrylate (4 g) and initiator 1-hydroxycyclohexyl phenyl ketone (0.4 g) were magnetically stirred (50 r / min) for 5 min at room temperature to make them uniform, and then 100 A wet film preparation device with a diameter of 1 μm was used to evenly coat it on the surface of the steel that had been wiped with ethanol and dried. The coating on the steel surface was exposed to a 360 W ultraviolet light source for 2 min (the distance between the ultraviolet light source and the steel surface was kept at 15 cm during the irradiation process). The coated steel was then placed in an oven at 120 ℃ for 12 h. After cooling to room temperature, an anti-corrosion coating for steel was obtained, which was recorded as PUA4.

[0029] Example 5 Palm oil diethanolamide (2.65 g), hexamethylene diisocyanate (1.01 g) and butanone (10 g) were added into a 250 ml three-necked flask, and N2 was introduced. The mixture was stirred magnetically (200 r / min) for 1 h in an oil bath at 75 °C. Isophorone diisocyanate (5.56 g) was added and the stirring was continued for 1 h. Isosorbide (1.46 g, the mass ratio of palm oil diethanolamide to isosorbide was 1.8:1) was added and the stirring was continued for 4 h. Hydroxyethyl acrylate (2.32 g) was added and the stirring was continued for 2 h to obtain acrylate-terminated palm oil-based polyurethane linear oligomers. Acrylate-terminated palm oil-based polyurethane linear oligomers (15.6 g), hydroxyethyl acrylate (4 g) and initiator 1-hydroxycyclohexyl phenyl ketone (0.4 g) were magnetically stirred (50 r / min) for 5 min at room temperature to make them uniform, and then 100 The wet film preparation device with a diameter of 1 μm was evenly coated on the steel surface that had been wiped with ethanol and dried, and the coating on the steel surface was exposed to a UV light source with a power of 360 W for 2 min (the distance between the UV light source and the steel surface was kept at 15 cm during the irradiation process); the coated steel was then placed in an oven at 120 ℃ for 12 h, and after cooling to room temperature, an anti-corrosion coating for steel was obtained, which was recorded as PUA5.

[0030] Comparative Example Palm oil diethanolamide (3.18 g), hexamethylene diisocyanate (1.01 g), butanone (10 g) and dibutyltin dilaurate (0.05 g) were added into a 250 ml three-necked flask, and N2 was introduced. The mixture was stirred magnetically (200 r / min) for 1 h in an oil bath at 75 °C. Isophorone diisocyanate (5.56 g) was added and the stirring was continued for 1 h. Isosorbide (1.17 g, the mass ratio of palm oil diethanolamide to isosorbide was 2.7:1) was added and the stirring was continued for 4 h. Hydroxyethyl acrylate (2.32 g) was added and the stirring was continued for 2 h to obtain acrylate-terminated palm oil-based polyurethane linear oligomers. Acrylate-terminated palm oil-based polyurethane linear oligomers (15.6 g), hydroxyethyl acrylate (4 g) and initiator 1-hydroxycyclohexyl phenyl ketone (0.4 g) were magnetically stirred (50 r / min) for 5 min at room temperature to make them uniform, and then 100 A wet film preparation device with a diameter of 1 μm was used to evenly coat it on the surface of the steel that had been wiped with ethanol and dried. The coating on the steel surface was exposed to a 360 W ultraviolet light source for 2 min (the distance between the ultraviolet light source and the steel surface was kept at 15 cm during the irradiation process). The coated steel was then placed in an oven at 120 ℃ for 12 h. After cooling to room temperature, the steel anticorrosion coating was obtained, which was recorded as PUA4-DBTDL.

[0031] Performance Testing 1. Gel content test of autocatalytic palm oil-based dynamic covalent polymer materials: The gel content of the autocatalytic palm oil-based dynamic covalent polymer material obtained in Examples 1 to 5 was determined by the solvent extraction method in ASTM D2765-16. The specific operation is to remove no more than 0.300 g ( w 1) The dried sample was wrapped with filter paper and placed in a Soxhlet extractor; 250 mL of dichloromethane was added to a 500 mL round-bottom flask and heated under reflux at 60 °C for 12 h; after the extraction, the swollen sample was collected and weighed ( w g The swollen samples were then dried in a vacuum oven at 100 °C until a constant weight was reached ( w 2). Calculate the gel content according to the following formula: Gel content = ( w 1 / w 2)×100%.

[0032] 2. Differential scanning calorimetry analysis of autocatalytic palm oil-based dynamic covalent polymer materials: Differential scanning calorimetry analysis was performed on a DSC 25 device (TA Instruments, USA); the specific operation was to take about 10 mg of the powder sample of the self-catalytic palm oil-based dynamic covalent polymer material obtained in Examples 1 to 5 and put it in a standard aluminum crucible with a lid; the experimental temperature was -50 ~ 250 °C, the heating rate was 10 °C / min, and it was carried out in a N2 atmosphere (20 mL / min).

[0033] 3. Mechanical properties test of palm oil-based polyurethane linear oligomers and autocatalytic palm oil-based dynamic covalent polymer materials: The samples prepared in Examples 1 to 5 were made into dumbbell-shaped specimens (specifications: 75 mm long, 10 mm wide at both ends, 5 mm wide in the middle, and 3 mm thick) to test the tensile properties. The tensile properties test was carried out in accordance with ASTM D638-10 standard; the tensile properties were completed on a microcomputer-controlled electronic universal testing machine.

[0034] The pencil hardness of the samples prepared in Examples 1 to 5 was tested at room temperature using a pencil hardness tester (model QHQ-A, China) according to the Chinese standard GB / T6739-2006.

[0035] The palm oil-based dynamic covalent polymer material prepared in Example 2 was subjected to a lap shear strength test. The specific operation is to use the sample as an adhesive to bond two plates of the same material with a size of 125 mm × 20 mm together, then compress the prepared sample with a 500 g steel block, and then cure it in an oven at 120 ° C for 30 min; then cool the bonded sample to room temperature. The lap shear strength test was completed on a microcomputer-controlled electronic universal testing machine.

[0036] 4. Scratch repair test of autocatalytic palm oil-based dynamic covalent polymer material: A sharp knife was used to scratch the surface of the palm oil-based dynamic covalent polymer material sample prepared in Example 2 to create scratches; the sample was then placed at 100° C. and 120° C. for 1 h, respectively, and the scratch repair was observed using an optical microscope.

[0037] 5. Test of the recovery performance of autocatalytic palm oil-based dynamic covalent polymer materials: The palm oil-based dynamic covalent polymer material sample prepared in Example 2 was crushed and then pressed using a tablet press at 100° C. and 10 MPa for 1 h; finally, a square sheet with a thickness of 1 to 2 mm was obtained, which was then tested according to the mechanical properties test method.

[0038] 6. Performance test of steel anticorrosion coating prepared by autocatalytic palm oil-based dynamic covalent polymer materials: The anti-corrosion performance of the steel anti-corrosion coating prepared in Example 2 was tested, and the adhesion was tested with reference to GB / T9286-2021; the flexibility was tested with reference to GB / T 1731-2020; the impact resistance was tested with reference to GB / T1732-2020; the water resistance was tested with reference to GB / T1733-1993; the salt spray resistance was tested with reference to GB / T1771-2007; and the solvent wipe resistance was tested with reference to GB / T 23989-2009.

[0039] Table 1 Determination results of gel content and hardness of autocatalytic palm oil-based dynamic covalent polymer

[0040] It can be seen from Table 1 that the gel content of palm oil-based dynamic covalent polymer materials prepared with palm oil diethanolamide and isosorbide in different mass ratios is above 91%; at the same time, the pencil hardness of PUA1, PUA2, PUA3, PUA4 and PUA5 are 2H, 3H, 4H, 4H and 5H, respectively, indicating that the pencil hardness of the dynamic covalent polymer material increases with the increase of the amount of isosorbide.

[0041] Figure 1The tensile stress and tensile strain comparison diagram of the self-catalytic palm oil-based dynamic covalent polymer materials prepared by palm oil diethanolamide and isosorbide in different mass ratios in Examples 1 to 5. As can be seen from the figure, the tensile strengths of PUA1, PUA2, PUA3, PUA4 and PUA5 are 4.6 MPa, 5.7 MPa, 6.7 MPa, 9.0 MPa and 12.4 MPa, respectively; the elongation at break of PUA1, PUA2, PUA3, PUA4 and PUA5 are 169%, 159%, 140%, 128% and 94%, respectively. It can be seen that the elongation at break of the palm oil-based dynamic covalent polymer material decreases with the increase of the amount of isosorbide, while the tensile strength increases with the increase of the amount of isosorbide.

[0042] Figure 2 The tensile stress and tensile strain comparison diagram of the self-catalytic palm oil-based dynamic covalent polymer material prepared by palm oil diethanolamide and isosorbide at a mass ratio of 2.7:1 in Example 2 and the palm oil-based polymer material prepared by adding an organic tin catalyst in the comparative example. As can be seen from the figure, the palm oil-based polymer material PUA4-DBTDL prepared by adding dibutyltin dilaurate catalyst has a tensile strength of 9.4 MPa and an elongation at break of 98.8%; its tensile strength is slightly higher than PUA4's 9.0 MPa, and its elongation at break is lower than PUA4's 128%. It shows that the dynamic polymer material prepared by the catalyst-free method has an effect comparable to that of the material prepared by the organic tin catalyst.

[0043] Figure 3 The kinetic differential calorimetry scanning curves of the self-catalytic palm oil-based dynamic covalent polymer materials prepared in Examples 1 to 5. As can be seen from the figure, the glass transition temperatures of PUA1, PUA2, PUA3, PUA4 and PUA5 are 36.4°C, 37.4°C, 39.2°C, 43.3°C and 48.9°C, respectively, indicating that the thermal stability of the self-catalytic palm oil-based dynamic covalent polymer materials increases significantly with the increase of isosorbide content.

[0044] Figure 4 The lap shear strength of the self-catalytic palm oil-based dynamic covalent polymer material prepared in Example 2 and different materials. As can be seen from the figure, the lap shear strength of the palm oil-based dynamic covalent polymer material PUA4 on glass, nylon, aluminum, wood and steel are 9.6 MPa, 0.8 MPa, 2.1 MPa, 5.0 MPa and 8.5 MPa respectively.

[0045] Figure 5 The scratch repairing condition of the self-catalytic palm oil-based dynamic covalent polymer material prepared in Example 2. As can be seen from the figure, the scratches of the self-catalytic palm oil-based dynamic covalent polymer material PUA4 can be well repaired after being placed at 100°C and 120°C for 1 hour.

[0046] Figure 6 The figure is a comparison of the tensile stress and tensile strain before and after the recycling of the self-catalytic palm oil-based dynamic covalent polymer material prepared in Example 2. As can be seen from the figure, after the self-catalytic palm oil-based dynamic covalent polymer PUA4 is crushed and kept at 100°C and 10 MPa for 1 hour, a polyurethane resin with a tensile strength of 15.1 MPa and an elongation at break of 56% can be obtained, indicating that it has good recyclability.

[0047] Table 2 Performance test results of steel anticorrosion coatings prepared using autocatalytic palm oil-based dynamic covalent polymer materials

[0048] It can be seen from Table 2 that the steel anti-corrosion coating prepared by the self-catalytic palm oil-based dynamic covalent polymer material has excellent adhesion, flexibility, impact resistance, solvent abrasion resistance, water resistance and salt spray resistance.

[0049] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A self-catalytic palm oil-based dynamic covalent polymer material, characterized in that: The raw materials used include, by weight: 78 parts of acrylate-terminated palm oil-based polyurethane linear oligomer, 20 parts of hydroxyethyl acrylate and 2 parts of photoinitiator.

2. The autocatalytic palm oil-based dynamic covalent polymer material according to claim 1, characterized in that: The acrylate-terminated palm oil-based polyurethane linear oligomer is prepared from the following raw materials in parts by mass: 2.62-5.77 parts of palm oil diethanolamide, 0.29-1.46 parts of isosorbide, 1.01 parts of hexamethylene diisocyanate, 5.56 parts of isophorone diisocyanate, 2.32 parts of hydroxyethyl acrylate and 10 parts of butanone.

3. The autocatalytic palm oil-based dynamic covalent polymer material according to claim 2, characterized in that: The preparation method of the acrylate-terminated palm oil-based polyurethane linear oligomer is as follows: palm oil diethanolamide, hexamethylene diisocyanate and butanone are mixed in proportion and N2 is introduced, and magnetic stirring is performed in an oil bath at 75°C for 1 hour; then isophorone diisocyanate is added, stirring is continued for 1 hour, isosorbide is added, stirring is continued for 4 hours, and finally hydroxyethyl acrylate is added, and stirring is continued for 2 hours.

4. The autocatalytic palm oil-based dynamic covalent polymer material according to claim 1, characterized in that: The photoinitiator is 1-hydroxycyclohexyl phenyl ketone.

5. The autocatalytic palm oil-based dynamic covalent polymer material according to claim 1, characterized in that: The preparation method is: after mixing acrylate-terminated palm oil-based polyurethane linear oligomer, hydroxyethyl acrylate and a photoinitiator in proportion, magnetically stirring them evenly at room temperature, pouring them into a mold, irradiating the mold under a 360 W ultraviolet light source for 2 minutes to cure it, and obtaining the self-catalytic palm oil-based dynamic covalent polymer material.

6. The autocatalytic palm oil-based dynamic covalent polymer material according to claim 5, characterized in that: During the UV irradiation process, the distance between the UV light source and the mold was 15 cm.

7. A method for preparing steel anticorrosion coating using the autocatalytic palm oil-based dynamic covalent polymer material according to claim 1, characterized in that: An appropriate amount of uncured autocatalytic palm oil-based dynamic covalent polymer is uniformly coated on the surface of the steel, and then the coating on the surface of the steel is exposed to an ultraviolet light source for curing, and then tempered to obtain the steel anticorrosive coating.

8. The method for preparing steel anticorrosion coating using autocatalytic palm oil-based dynamic covalent polymer material according to claim 7, characterized in that: The curing is performed under a 360 W ultraviolet light source for 2 min, and the distance between the ultraviolet light source and the steel surface is maintained at 15 cm during the irradiation process.

9. The method for preparing steel anticorrosion coating using autocatalytic palm oil-based dynamic covalent polymer material according to claim 7, characterized in that: The tempering is carried out by baking in an oven at 120°C for 12 h.

Citation Information

Patent Citations

  • Vegetable oil based polyurethane acrylic ester, preparing process and use thereof

    CN101497684A

  • UV-cured self-repairing polyurethane acrylate coating and preparation method thereof

    CN113072874A

  • Fatty acid chain suspended palm oil based thermoplastic polyurethane elastomer and preparation method thereof

    CN114478976A

  • Catalyst-free recoverable vegetable oil-based self-repairing ultraviolet curing coating and preparation method thereof

    CN115948066A

  • Aqueous bio-based energy curable polyurethane compositions

    CN116568767A