Preparation method and application of high-strength environment-friendly epoxy grouting material

By optimizing the ratio of epoxy grouting materials, high-strength and environmentally friendly epoxy grouting materials were developed, which solved the problem of insufficient fluidity and consolidation performance of epoxy grouting materials in the steel-mixed tower in the existing technology, and achieved high strength Repair and prove its human and environmentally friendly safety.

CN119019967APending Publication Date: 2024-11-26CHINA INST OF WATER RESOURCES & HYDROPOWER RES +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411172117.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing epoxy grouting materials have good fluidity in concrete crack repair in steel-concrete towers, but the mechanical properties of the consolidation body are insufficient, and the volatile components are harmful to workers and the environment, and cannot meet the repair needs of high-strength concrete sections.

Method used

Develop a high-strength environmentally friendly epoxy grouting material. By optimizing the material ratio, including epoxy resin, diluent, defoaming agent, reinforcement particles, toughening agent and curing agent, it ensures good fluidity and compressive strength after consolidation. It reaches more than 90MPa and is proven to be safe by acute toxicity test in rats.

Benefits of technology

It has achieved good fluidity of epoxy grouting material, has high consolidation mechanical properties, and has compressive strength of more than 90MPa after 28 days. It has been proved that it is non-toxic to the human body through the rat acute toxicity test, which satisfies the steel-concrete tower. High-strength restoration requirements for concrete sections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a high-strength environment-friendly epoxy grouting material. The high-strength environment-friendly epoxy grouting material comprises 40-50 parts of epoxy resin, 10-30 parts of a diluent, 0.1-0.2 part of a defoaming agent, 0.3-0.5 part of reinforcing particles, 0.5-0.7 part of a toughening agent and 20-35 parts of a curing agent. The preparation method comprises the following steps: fully mixing epoxy resin, a diluent, a defoaming agent, reinforcing particles and a flexibilizer according to a ratio, and uniformly stirring to form a component A; and mixing and stirring the component A and the curing agent. The prepared high-strength environment-friendly epoxy grouting material is good for human bodies and the environment and good in fluidity, the mechanical strength of a consolidated body after consolidation is high, and the compressive strength is 90 MPa or above after the age of 28 days. The material effectively solves the problem that the prestress of an anchor bolt of an existing fan foundation is unqualified. The problem of a fan foundation can be solved, and after treatment, the percent of pass of anchor bolt prestress detection can reach 90% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of grouting materials, and in particular to a method for preparing a high-strength and environmentally friendly epoxy grouting material and application of the high-strength and environmentally friendly epoxy grouting material prepared by the preparation method in repairing concrete cracks of a steel-concrete tower type wind turbine. Background Art

[0002] The development of the wind power industry is one of the major measures to promote the clean and low-carbon transformation of energy. At present, the development of the wind power industry has gradually shifted from the "Three North Regions" to the central and eastern regions and low wind speed areas. In order to increase the return on investment in low wind speed wind farms, increasing the height of wind towers and utilizing high-altitude wind energy is one of the main means. To this end, the structure of wind power towers has undergone fundamental changes, and the towers have also been transformed from pure steel towers to steel-concrete composite towers. However, cracks will inevitably occur in the concrete sections of steel-concrete composite towers during construction, transportation, and installation. The reasons for the formation of these concrete cracks vary, and the impact on the tower is also different. In most cases, when concrete cracks are detected, the cracks should be evaluated and handled in a timely manner to prevent the wind turbine from causing greater defects due to reciprocating cyclic dynamic loads during operation, thereby affecting the safety of the entire wind turbine.

[0003] In the past, epoxy grouting materials were one of the main reinforcement materials for repairing concrete cracks. Since epoxy grouting materials have good fluidity and excellent mechanical properties of the consolidated body after consolidation, epoxy grouting materials are also used to repair concrete sections in steel-concrete towers. In order to ensure the low viscosity and good fluidity of epoxy grouting materials, the previous method was to use furfural and acetone system diluents in epoxy grouting materials, or to use low-viscosity curing agents such as ethylenediamine. However, the above-mentioned components are highly volatile and easily produce irritating odors, which are not only harmful to production workers, but also unfriendly to high-altitude workers, which will greatly increase the risk of construction workers in aerial construction. In addition, the strength of concrete in steel-concrete towers is much greater than that of conventional concrete. Previously, the strength of concrete was generally around C40, while the strength of concrete in concrete towers was generally C80 or higher. Therefore, epoxy grouting materials above C40 can meet the requirements for concrete crack repair, but cannot meet the strength requirements of C80. Therefore, there are few epoxy grouting materials on the market that meet the needs of concrete section repair, and they cannot meet the needs of a large number of concrete tower repairs.

[0004] In view of the above-mentioned deficiencies, the present invention aims to study an environmentally friendly epoxy grouting material with good fluidity and high strength, so as to meet the needs of repairing cracks in concrete sections of steel-concrete towers. Summary of the invention

[0005] At present, there are epoxy grouting materials for repairing concrete cracks, but there are few epoxy grouting materials for repairing cracks in concrete sections of steel-concrete towers. Materials in this area are still in the research and development stage. Based on a long-term study of epoxy grouting materials, the present invention studies the material ratio and develops an environmentally friendly epoxy grouting material that is good for the human body and the environment, has good fluidity, and has high mechanical strength of the consolidated body after consolidation. Under the premise of satisfying good fluidity, the material has excellent mechanical properties of the consolidated body, among which the compressive strength is above 90MPa after the age of 28d.

[0006] The present invention is achieved by the following technical means:

[0007] The present invention firstly discloses a high-strength environmentally friendly epoxy grouting material, comprising the following raw materials in proportion by weight:

[0008] 40-50 parts of epoxy resin, 10-30 parts of diluent, 0.1-0.2 parts of defoaming agent, 0.3-0.5 parts of reinforcing particles, 0.5-0.7 parts of toughening agent, and 20-35 parts of curing agent.

[0009] Furthermore, the epoxy resin is selected from one or more of bisphenol A epoxy resin E51, E44, and bisphenol F epoxy resin.

[0010] Furthermore, the diluent includes, but is not limited to, glycidyl ether diluents, acetone, butanone, methyl ethyl ketone, cyclohexanone, and n-butanol.

[0011] Furthermore, the glycidyl ether diluent includes but is not limited to: butyl glycidyl ether, octyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, and ethylene glycol diglycidyl ether.

[0012] Furthermore, the defoaming agent is organic silicone.

[0013] Furthermore, the reinforcing particles include but are not limited to: steel fibers and graphite particles.

[0014] Furthermore, the toughening agent includes but is not limited to: nano silicon dioxide particles.

[0015] Furthermore, the curing agent includes, but is not limited to: polyamide curing agent, aromatic amine curing agent, phenolic amine curing agent, and aliphatic curing agent.

[0016] Furthermore, the polyamide curing agent includes but is not limited to: 651, 650;

[0017] The aromatic amines include, but are not limited to: m-toluenediamine;

[0018] The phenolic amine curing agent includes but is not limited to: T31;

[0019] The aliphatic curing agent includes but is not limited to: triethylenetetramine and diethylenetetramine.

[0020] The present invention also discloses a method for preparing a high-strength environmentally friendly epoxy grouting material, comprising the following steps:

[0021] (1) preparing component A: fully mixing epoxy resin, diluent, defoamer, reinforcing particles and toughening agent according to proportions, stirring evenly to form component A;

[0022] (2) Preparation of high-strength and environmentally friendly epoxy grouting material: Mix component A with the curing agent and stir to obtain the product.

[0023] Furthermore, in step (1), the stirring speed is 1000 r / min and the stirring time is 5 min.

[0024] Furthermore, in step (2), the stirring speed is 1000 r / min and the stirring time is 3 min.

[0025] The invention also discloses a high-strength and environment-friendly epoxy grouting material prepared according to any one of the above preparation methods.

[0026] The present invention also discloses an application of any of the above-mentioned high-strength environmentally friendly epoxy grouting materials in repairing concrete cracks of a steel-concrete tower type fan.

[0027] The beneficial effects of the present invention are:

[0028] 1. The present invention is based on a long-term study of epoxy grouting materials. By studying the material ratio, an environmentally friendly epoxy grouting material is developed that is good for the human body and the environment, has good fluidity, and has high mechanical strength of the consolidated body after consolidation. The material has excellent mechanical properties of the consolidated body while meeting the requirement of good fluidity. Among them, the compressive strength is above 90MPa after the age of 28d.

[0029] 2. The repair of concrete cracks in steel-concrete tower wind turbines is different from the previous concrete crack repair. Previously, concrete crack repairs mostly used pressure pumps to inject epoxy grouting materials, while fan concrete crack repairs mostly used syringes to manually inject epoxy grouting materials. The viscosity of the material is considered to be below 500mPa·s, and the compressive strength of the consolidated body of the epoxy grouting material after consolidation is greater than 90MPa. The epoxy grouting material applied in the present invention is an environmentally friendly material, which has passed the rat acute toxicity test, LD 50 The values ​​are all greater than 5000 mg / kg, which is practically non-toxic and therefore harmless to the human body.

[0030] 3. The present invention proposes a comprehensive grouting material and construction method for strengthening the wind turbine foundation, which solves the problem of unqualified prestressing of anchor bolts in the current wind turbine foundation. DETAILED DESCRIPTION

[0031] The embodiments of the present invention will be described in detail below in conjunction with examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer.

[0032] Embodiment 1:

[0033] A high-strength environmentally friendly epoxy grouting material and preparation method thereof

[0034] (1) 40 parts of epoxy resin (E51), 20 parts of diluent, 0.15 parts of defoaming agent, 0.3 parts of reinforcing particles, and 0.6 parts of toughening agent were mixed to form component A;

[0035] (2) Select polyamide 650, T31, and triethylenetetramine to form a curing agent, and the curing agent is 30 parts;

[0036] (3) Component A is uniformly mixed with the curing agent to form a high-strength and environmentally friendly epoxy grouting material.

[0037] Embodiment 2:

[0038] A high-strength environmentally friendly epoxy grouting material and preparation method thereof

[0039] (1) 40 parts of epoxy resin (E51), 20 parts of diluent, 0.15 parts of defoaming agent, 0.35 parts of reinforcing particles, and 0.6 parts of toughening agent were mixed to form component A;

[0040] (2) Select polyamide 650, T31, and triethylenetetramine to form a curing agent, and the curing agent is 30 parts;

[0041] (3) Component A is uniformly mixed with the curing agent to form a high-strength and environmentally friendly epoxy grouting material.

[0042] Embodiment 3:

[0043] A high-strength environmentally friendly epoxy grouting material and preparation method thereof

[0044] (1) 40 parts of epoxy resin (E51), 20 parts of diluent, 0.15 parts of defoaming agent, 0.4 parts of reinforcing particles, and 0.6 parts of toughening agent were mixed to form component A;

[0045] (2) Select polyamide 650, T31, and triethylenetetramine to form a curing agent, and the curing agent is 30 parts;

[0046] (3) Component A is uniformly mixed with the curing agent to form a high-strength and environmentally friendly epoxy grouting material.

[0047] Embodiment 4:

[0048] A high-strength environmentally friendly epoxy grouting material and preparation method thereof

[0049] (1) 45 parts of epoxy resin (E51), 20 parts of diluent, 0.15 parts of defoaming agent, 0.4 parts of reinforcing particles, and 0.6 parts of toughening agent were mixed to form component A;

[0050] (2) Select polyamide 650, T31, and triethylenetetramine to form a curing agent, and the curing agent is 30 parts;

[0051] (3) Component A is uniformly mixed with the curing agent to form a high-strength and environmentally friendly epoxy grouting material.

[0052] Embodiment 5:

[0053] A high-strength environmentally friendly epoxy grouting material and preparation method thereof

[0054] (1) 50 parts of epoxy resin (E51), 20 parts of diluent, 0.15 parts of defoaming agent, 0.4 parts of reinforcing particles, and 0.6 parts of toughening agent were mixed to form component A;

[0055] (2) Select polyamide 650, T31, and triethylenetetramine to form a curing agent, and the curing agent is 30 parts;

[0056] (3) Component A is uniformly mixed with the curing agent to form a high-strength and environmentally friendly epoxy grouting material.

[0057] Embodiment 6:

[0058] A high-strength environmentally friendly epoxy grouting material and preparation method thereof

[0059] (1) 50 parts of epoxy resin (E51), 20 parts of diluent, 0.15 parts of defoaming agent, 0.4 parts of reinforcing particles, and 0.6 parts of toughening agent were mixed to form component A;

[0060] (2) Select polyamide 650, T31, and triethylenetetramine to form a curing agent, and the curing agent is 35 parts;

[0061] (3) Component A is uniformly mixed with the curing agent to form a high-strength and environmentally friendly epoxy grouting material.

[0062] Test Example 1

[0063] The epoxy grouting materials prepared in each group of Examples 1 to 6 were tested and molded, and finally formed into a solid body, and then the performance was tested. The results are shown in Table 1:

[0064] Table 1 Performance indicators of high-strength environmentally friendly epoxy grouting materials

[0065]

[0066] According to the results in Table 1, the high-strength environmentally friendly epoxy grouting material has a low initial viscosity, a 28-day compressive strength of more than 90 MPa, and high dry and wet bonding strength, which can meet the repair requirements of the steel-mixed fan tower section.

[0067] Test Example 2

[0068] The acute toxicity test in rats was conducted with reference to GB / T 21757-2008. Healthy male and female rats were provided by a laboratory animal technology company (Beijing, China). The rats were placed in clean polypropylene cages and subjected to a 12-hour light / dark cycle in a temperature-controlled animal room (23±2°C, relative humidity 50-70%). Three male or female rats were placed in each cage, and the rats were checked every day. The animals were fed with standard commercial rat pellet feed (a laboratory animal technology company, Beijing, China) and ultrapure water. The daily feeding mass content of the sample was 5000 mg / kg, which met the quality requirements for experimental animals. The test period was 14 days according to GB / T 21757-2008.

[0069] Grouping Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 <![CDATA[LD 50 Value]]> >5000 >5000 >5000 >5000 >5000 >5000

[0070] According to the above table, the epoxy grouting material applied in the present invention is an environmentally friendly material and has passed the rat acute toxicity test. 50 The values ​​are all greater than 5000 mg / kg, which is practically non-toxic and therefore harmless to the human body.

[0071] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.

Claims

1. A high-strength environmentally friendly epoxy grouting material, comprising the following raw materials in proportion by weight: 40-50 parts of epoxy resin, 10-30 parts of diluent, 0.1-0.2 parts of defoaming agent, 0.3-0.5 parts of reinforcing particles, 0.5-0.7 parts of toughening agent, and 20-35 parts of curing agent.

2. The high-strength environmentally friendly epoxy grouting material according to claim 1, wherein: The epoxy resin is selected from one or more of bisphenol A epoxy resin E51, E44 and bisphenol F epoxy resin.

3. The high-strength environmentally friendly epoxy grouting material according to claim 1, wherein: The diluent includes: glycidyl ether diluent, acetone, butanone, methyl ethyl ketone, cyclohexanone, and n-butanol.

4. The high-strength environmentally friendly epoxy grouting material according to claim 3, wherein: The glycidyl ether diluents include: butyl glycidyl ether, octyl glycidyl ether, phenyl glycidyl ether, benzyl glycidyl ether, and ethylene glycol diglycidyl ether.

5. The high-strength environmentally friendly epoxy grouting material according to claim 1, wherein: The defoaming agent is organic silicone; The reinforcing particles include: steel fibers and graphite particles; The toughening agent includes: nano silicon dioxide particles; The curing agent includes: polyamide curing agent, aromatic amine curing agent, phenolic amine curing agent, and aliphatic curing agent.

6. The high-strength environmentally friendly epoxy grouting material according to claim 5, wherein: The polyamide curing agent includes: 651, 650; The aromatic amines include: m-toluenediamine; The phenolic amine curing agent includes: T31; The aliphatic curing agent includes triethylenetetramine and diethylenetetramine.

7. A method for preparing any high-strength environmentally friendly epoxy grouting material according to any one of claims 1 to 6, comprising the following steps: (1) preparing component A: fully mixing epoxy resin, diluent, defoamer, reinforcing particles and toughening agent according to proportions, stirring evenly to form component A; (2) Preparation of high-strength and environmentally friendly epoxy grouting material: Mix component A with the curing agent and stir to obtain the product.

8. The preparation method according to claim 7, wherein: The stirring speed in step (1) is 1000 r / min and the stirring time is 5 min; The stirring speed in step (2) is 1000 r / min and the stirring time is 3 min.

9. A high-strength and environmentally friendly epoxy grouting material prepared according to the preparation method of claim 7 or 8.

10. Use of the high-strength environmentally friendly epoxy grouting material according to claim 1 to 6 or 9 in repairing concrete cracks in a steel-concrete tower type wind turbine.

Citation Information

Cited By

  • Epoxy grouting material as well as preparation method and application thereof

    CN122037468A