Method for regulating and controlling chromophore arrangement mode and room-temperature phosphorescence performance through covalent bonds based on carrier structure change

Through the microstructure changes of inorganic carriers and the covalent bonding, the microarrangement of phosphorescent molecules is regulated, the problem of competitive covalent reaction is solved, and the construction and regulation of multi-color dynamic phosphorescent materials are realized, which is suitable for high-level anti-counterfeiting and information storage. .

CN119020014APending Publication Date: 2024-11-26BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410905920.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When constructing multicolor dynamic room temperature phosphorescent materials, competitive covalent reactions often occur during the covalent bond construction process, resulting in unwanted fragments coexisting with the target product, hindering the regulation of phosphorescence emission, and lacking fine and controllable strategies. Regulates competitive covalent response.

Method used

By synthesizing the tunable inorganic carrier with hydroxyl groups on the surface, a covalent cross-linking network is constructed, and the microarrangement of the phosphorescent molecules is regulated by the microstructure changes of the inorganic carrier to achieve dynamically adjustable phosphorescent colors and Time-dependent emission.

Benefits of technology

It realizes stable and efficient regulation of phosphorescent molecules, improves phosphorescence efficiency, and builds a multi-color dynamic room temperature phosphorescent material with time-dependent variable emission, which is suitable for high-level anti-counterfeiting and information storage fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004932091180000011
    Figure HDA0004932091180000011
  • Figure HDA0004932091180000012
    Figure HDA0004932091180000012
  • Figure HDA0004932091180000021
    Figure HDA0004932091180000021
Patent Text Reader

Abstract

The invention discloses a method for regulating and controlling a chromophore arrangement mode and room-temperature phosphorescence performance through covalent bonds based on carrier structure change, and belongs to the technical field of room-temperature phosphorescence material preparation. The preparation method comprises the following steps: synthesizing an inorganic carrier with hydroxyl on the surface and adjustable structural composition, preparing a suspension, preparing a phosphorescent molecule solution, carrying out covalent reaction on phosphorescent molecules and the inorganic carrier, and removing a solvent to obtain the organic-inorganic composite room-temperature phosphorescent material with a covalent structure. The microstructure of an inorganic carrier is changed, and organic-inorganic composite phosphorescent materials with different carrier structures are synthesized; through fine regulation and control of a microstructure of an inorganic substance and a covalent bond effect between the inorganic substance and a phosphorescent chromophore, regulation and control of microcosmic arrangement of the chromophore and dynamic room-temperature phosphorescence performance are realized, and multicolor dynamic phosphorescence is constructed; the dynamic adjustable afterglow of the composite phosphorescent material is used for designing multi-stage encryption application of Morse passwords and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of room temperature phosphorescent material preparation, and specifically relates to a method for regulating the microscopic arrangement of phosphorescent molecules based on the change of the inorganic carrier structure through covalent cross-linking to regulate the room temperature phosphorescent properties and construct a dynamic room temperature phosphorescent material with time dependence. Background Art

[0002] Room temperature phosphorescent (RTP) materials have a wide range of applications in anti-counterfeiting, data storage and encryption due to their long luminescence lifetime. Among them, time-dependent multicolor dynamic room temperature phosphorescent materials have a wide range of applications in high-level anti-counterfeiting because they can display multiple phosphorescent colors at different times.

[0003] In order to construct multicolor dynamic room temperature phosphorescent materials, it is often necessary to optimize the microscopic arrangement of chromophores and adjust them to be in an aggregated or isolated state. Due to the high energy and stability of covalent bonds, they have been used to regulate the microscopic arrangement of chromophores in dynamic RTP materials. However, when constructing multicolor dynamic RTP materials through covalent bonds, some competitive covalent reactions will inevitably occur, resulting in the coexistence of some unwanted fragments with the target product, hindering the regulation of phosphorescence emission. Therefore, a more sophisticated and controllable strategy is urgently needed to regulate competitive covalent reactions to achieve ideal chromophore molecular arrangement and dynamic phosphorescence emission.

[0004] The method of the present invention is based on the fine regulation of the microstructure of the inorganic carrier and the covalent bond between the inorganic carrier and the phosphorescent chromophore to achieve the regulation of the microscopic arrangement of the chromophore. On the one hand, the phosphorescent chromophore can be stabilized by inorganic substances to limit its non-radiative transition and improve the phosphorescence efficiency; on the other hand, the microscopic arrangement of the phosphorescent chromophore is affected by the change of the microscopic molecular structure of the inorganic carrier to construct multicolor dynamic phosphorescence. This method achieves the regulation of the microstructure of the phosphorescent chromophore through covalent bonds based on the change of the carrier structure, thereby constructing a room temperature phosphorescent material with time-dependent variable emission, providing a new method for constructing and regulating multifunctional room temperature phosphorescent materials, and providing application prospects for high-level anti-counterfeiting and information storage. Summary of the invention

[0005] In order to meet the demand for constructing multicolor, time-dependent room temperature phosphorescent materials, the present invention provides a method for regulating the microscopic arrangement and phosphorescent properties of phosphorescent chromophores based on the microscopic structural changes of inorganic carriers through covalent reactions.

[0006] The technical scheme of the present invention is: synthesize an inorganic carrier with hydroxyl groups on the surface and adjustable structural composition and configure it into a suspension, configure a phosphorescent molecule solution, make the phosphorescent molecules and the inorganic carrier undergo a covalent reaction, and construct a composite material with a covalent cross-linked network. The solvent is removed by a solvent evaporation method to obtain an organic-inorganic composite material, which not only has a time-dependent phosphorescent afterglow, but also has a dynamically adjustable phosphorescent color related to the inorganic structure. By regulating the microstructure of the inorganic carrier, the phosphorescence of the composite material can be effectively regulated to achieve different dynamic / static colors. The dynamically adjustable afterglow of the phosphorescent material is used to realize multi-level encryption applications such as Morse code encryption technology. The method is suitable for mass production of composite materials, and the constructed organic-inorganic composite material has excellent adjustable performance, which greatly expands the application of advanced anti-counterfeiting encryption and dynamic storage.

[0007] The present invention provides a method for regulating the arrangement of chromophores and room temperature phosphorescence performance based on changes in carrier structure and through covalent bonds. The method is simple, has mild conditions, and can be finely regulated. The constructed composite material has good phosphorescence performance, adjustable color, and a wide range of applications, providing a new method for achieving advanced anti-counterfeiting encryption.

[0008] A method for regulating the arrangement of chromophores and room temperature phosphorescence performance through covalent bonds based on changes in carrier structure, characterized in that it comprises the following steps:

[0009] (1) synthesizing an inorganic carrier with hydroxyl groups on the surface and adjustable structural composition and preparing it into a suspension;

[0010] (2) dissolving the phosphorescent molecule modified with boronic acid groups at both ends and adding an alkaline buffer solution to hydrolyze the boronic acid groups;

[0011] (3) Weigh a certain amount of the inorganic carrier suspension of step (1) and the phosphorescent molecule solution containing boric acid groups at both ends of step (2), respectively, and stir for 1 hour to allow them to be fully dispersed and react.

[0012] (4) Pour the fully reacted solution into a watch glass, place it in a 60°C oven, and dry it for 4 hours.

[0013] (5) changing the microstructure of the inorganic carrier in step (1), repeating steps 2-(4) to synthesize organic-inorganic composite phosphorescent materials with different carrier structures;

[0014] (6) Using the adjustable afterglow of composite phosphorescent materials constructed from different inorganic carriers to design multi-level encryption applications such as Morse code.

[0015] The method is suitable for constructing a composite material in which an inorganic carrier with adjustable structural composition and phosphorescent molecules can form a covalent bond.

[0016] In step (1), in step (1), the hydroxyl-rich inorganic substance is selected from montmorillonite (MMT), layered double metal hydroxides (LDHs), and silicon dioxide; preferably layered double metal hydroxides (LDHs). The divalent metal in LDHs is selected from Mg, Zn, Ca, etc., and the trivalent metal is selected from Al, Ga, etc., preferably magnesium aluminum hydrotalcite (MgAl-LDHs). The present invention can further introduce formamide and the like in the preparation process to obtain peeled thin LDHs, thereby further optimizing the performance of the composite material.

[0017] In step (2), the phosphorescent molecule modified with boronic acid groups at both ends is an aromatic boronic acid molecule, the number of boronic acid groups in a single molecule is 2 or 3, and the middle luminescent part can be selected from biphenyl, phenyl, tetraphenylethylene, etc.; 1,3-phenylenediboronic acid molecule (BBA) is preferred.

[0018] The alkaline buffer solution is a K2CO3 / KHCO3 buffer solution with a pH of 10.5, and the solvent for preparing the phosphorescent molecule solution is a mixed solvent of dimethyl sulfoxide:buffer solution=4:1 (volume ratio).

[0019] In step (3), the amount of the inorganic carrier and the phosphorescent molecules used to construct the composite material is in the following relationship: the phosphorescent molecules account for 5%-80% of the mass of the inorganic carrier.

[0020] The stirring reaction in step (4) is carried out at room temperature for 10 min-4 h. To increase the reaction speed and degree, the temperature may be appropriately heated to 20-60°C.

[0021] The specific method for changing the microstructure of the inorganic carrier in step (5) is: by adjusting the feed ratio, the ratio of divalent and trivalent metals on the LDHs layer is adjusted, and the adjustment range is divalent: trivalent molar ratio = 2:1, 3:1, 4:1 and 5:1. The synthesis method of organic-inorganic composite phosphorescent materials with different carrier structures is the same as step (3) and step (4).

[0022] The specific design scheme of the Morse code in step (6) is as follows: LDH-17% BBA composite powder with different divalent: trivalent molar ratios, especially Mg: Al, is made into a "dot" pattern, excited with an ultraviolet lamp with a wavelength of 280nm for 3s, and then the ultraviolet lamp is turned off, and the phosphorescence change of the anti-counterfeiting pattern is observed and photographed. The cyan "dot" phosphorescent pattern represents "-", and the dark blue "dot" phosphorescent pattern represents "·", and the Morse code table is referred to for decryption.

[0023] The constructed composite material can be prepared in large quantities and appears as fine white powder under visible light.

[0024] The composite phosphorescent material of the present invention exhibits dynamically adjustable phosphorescent emission. Composite materials prepared from LDHs with different divalent:trivalent molar ratios, especially Mg:Al ratio, exhibit completely different phosphorescence after removing 280nm ultraviolet light. Taking the composite material LDH-17%BBA constructed with 17% BBA as an example, when Mg / Al=5:1, it exhibits pure cyan phosphorescent emission for 2s. When Mg / Al=4:1, a dynamic phosphorescent color gradually changes from cyan to dark blue is observed. When Mg / Al=2:1, the phosphorescence of LDH-17%BBA is mainly dark blue. This dynamically adjustable phosphorescent color can be used for multi-level anti-counterfeiting encryption applications.

[0025] The room temperature phosphorescent material constructed by the present invention is a powder material, which is pure white under visible light, has fine particles, and can be prepared in large quantities. Under the covalent action of the phosphorescent molecules with the inorganic matrix, the room temperature phosphorescent performance is significantly enhanced, and the phosphorescent life span of the second level can be obtained. Under the regulation of the inorganic carrier on the microscopic arrangement of the phosphorescent molecules, the dynamically adjustable phosphorescent color can be achieved.

[0026] The present invention is based on the change of the structure of the inorganic carrier and the regulation of the microscopic arrangement of the phosphorescent molecules through covalent cross-linking to regulate the room temperature phosphorescence performance. On the one hand, the rigid covalent cross-linking network inhibits the non-radiative transition of the phosphorescent molecules, greatly improving the phosphorescence performance; on the other hand, by changing the structure of the inorganic carrier, the influence on the microscopic arrangement of the chromophore molecules is achieved, and a dynamically adjustable multi-color phosphorescence is constructed. Therefore, this method successfully constructs an adjustable room temperature phosphorescent material with time-dependent variable emission. The room temperature phosphorescent material constructed by this method has a long phosphorescence life, rich colors, can be prepared in large quantities, and the phosphorescence color is dynamically adjustable, which can provide a new method for applications in the fields of advanced anti-counterfeiting, dynamic encryption and information storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 XRD spectra of LDHs with different magnesium-aluminum ratios (Mg / Al=5:1, 4:1, 3:1, 2:1).

[0028] Figure 2 This is the low-temperature phosphorescence emission spectrum of the phosphorescent molecule BBA in DMSO solution and in solid powder state.

[0029] Figure 3 Fourier transform infrared spectra of LDHs, phosphorescent molecule BBA and composite material LDHs-17%BBA.

[0030] Figure 4 Time-resolved spectrum of LDHs-17%BBA.

[0031] Figure 5A is the phosphorescence lifetime of LDHs-17% BBA at 400nm emission under 280nm excitation, and B is the phosphorescence lifetime of LDHs-17% BBA at 465nm emission under 280nm excitation.

[0032] Figure 6 Phosphorescence emission spectra of LDHs-17% BBA with different magnesium-aluminum ratios (Mg / Al=5:1, 4:1, 3:1, 2:1).

[0033] Figure 7 Zeta potential diagrams of LDHs with different magnesium-aluminum ratios (Mg / Al=5:1, 4:1, 3:1, 2:1).

[0034] Figure 8 This is the Morse code encryption process made of LDHs-17% BBA with different magnesium-aluminum ratios (Mg / Al=4:1, 2:1). DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with examples, but the present invention is not limited to the following examples.

[0036] Embodiment 1:

[0037] (1) Synthesis of monolayer Mg-Al LDHs

[0038] Using formamide as an inhibitor, thin-layer LDHs nanosheets were prepared by a one-step method. Specifically, 10mL of a mixed salt solution consisting of Mg(NO3)2·6H2O and Al(NO3)3·9H2O was added dropwise to a NaNO3 solution (0.01mol / L, 10mL) containing 23% formamide under stirring at 80°C. At the same time, NaOH solution (0.25mol / L) was added to the mixture to keep the pH value at 10. After the addition was completed, the mixture was centrifuged and washed three times with deionized water to obtain LDHs nanosheet colloid for later use. The above method was used to synthesize single-layer MgAl-LDHs nanosheets with different Mg:Al ratios (2:1~5:1). As Figure 1 As shown, the characteristic diffraction peaks of (003), (006) and (009) planes of LDHs at 11.9°, 23.5° and 34.8°, indicating that LDHs with different Mg / Al ratios were successfully synthesized.

[0039] (2) Preparation of phosphorescent molecule BBA solution

[0040] A K2CO3 / KHCO3 buffer solution with a pH of 10.5 was prepared, and 40 mg of BBA was dissolved in a mixture of 40 mL of DMSO and the buffer solution to obtain a phosphorescent molecular solution (1 mg / mL). The room temperature phosphorescence properties of BBA itself were studied, and the low temperature spectrum of BBA in a dimethyl sulfoxide solution cooled by liquid nitrogen was shown in FIG. Figure 2 As shown in the figure, under excitation at 280 nm, pure deep blue emission at 400 nm can be observed from the DMSO solution of BBA, while the phosphorescence emission wavelength of BBA powder at low temperature is about 500 nm. This phenomenon can be attributed to the isolation-aggregation mechanism of the chromophore: the emission peak at 400 nm is related to the isolated molecules of BBA, while the emission peak at 465 nm is caused by the molecular aggregation of BBA.

[0041] (3) Construction of LDHs-17% BBA composites

[0042] The monolayer LDH nanosheets were dispersed in deionized water to obtain a 2 g / L suspension. Then, 9 mg of LDHs suspension was added to 3 mL of BBA solution and stirred at room temperature for 1 h. The reaction mixture was poured into a petri dish and dried at 60 ° C for 6 h. The resulting composite material was labeled LDH-17% BBA.

[0043] (4) Structural study of LDH-17% BBA composites

[0044] like Figure 3 As shown, the original components of the composite material were tested by Fourier transform infrared spectroscopy, and LDH-17%BBA showed characteristic peaks of LDHs and BBA, indicating that the composite material was successfully constructed. -1 The absorption peak at 1390 cm-1 is attributed to the stretching vibration of OH, which is significantly broadened in the LDH-17% BBA composite. -1 The absorption peak at 40° is broader and stronger than that of LDHs. These changes indicate that LDH-17%BBA forms BO bonds and hydrogen bonds.

[0045] (5) Study on the phosphorescence properties of LDH-17% BBA composites

[0046] Figure 4Figure 2 is the phosphorescence emission spectrum of LDH-17%BBA. It can be seen that the composite material has two emission peaks at 400nm and 465nm. The time-resolved spectrum shows the time-varying phosphorescence behavior of LDH-17%BBA. Under excitation at 280nm, a stronger cyan phosphorescence can be observed at 465nm and a weaker dark blue phosphorescence can be observed at 400nm. It is worth noting that the cyan phosphorescence (465nm) decays faster than the dark blue phosphorescence (400nm), resulting in a dynamic phosphorescence emission change from cyan to dark blue. Figure 5 The phosphorescence lifetime of the LDH-17% BBA composite material under 280nm excitation was demonstrated. A longer phosphorescence lifetime of 1.032s was observed at 400nm, while a faster phosphorescence decay was observed at 465nm, showing a shorter phosphorescence lifetime of 367.1ms. This is because the effect of LDH effectively regulates the microscopic arrangement of BBA molecules, making it have both isolated and aggregated states, thus showing different room temperature phosphorescence emission colors.

[0047] (6) Regulation of dynamic phosphorescence of LDH-17% BBA composite materials.

[0048] LDHs with Mg / Al ratios ranging from 2:1 to 5:1 were reacted with BBA respectively. Figure 6 It was shown that these LDH-17%BBA composites prepared from LDHs with different Mg:Al ratios exhibited completely different phosphorescence after the removal of UV light. LDH-17%BBA exhibited a completely cyan phosphorescence emission for 2s at Mg / Al=5:1. When the Mg / Al of LDH-17%BBA was 4:1, a dynamic phosphorescence color was observed to gradually change from cyan to dark blue. When Mg / Al=2:1, the phosphorescence of LDH-17%BBA was dominated by dark blue emission. To verify the mechanism, we tested the zeta potential of BBA and LDHs with different Mg:Al ratios (see Figure 7 ). BBA is negatively charged and LDHs are positively charged, resulting in a certain electrostatic attraction between BBA and LDHs. It is worth noting that the zeta potential of LDHs increases from 17.2mV at Mg / Al=5:1 to 38.5mV at Mg / Al=2:1. In other words, the higher the proportion of Al in LDHs, the stronger the positive charge of LDHs to attract negatively charged BBA. BBA molecules on LDHs with Mg / Al=5:1 tend to aggregate and emit cyan phosphorescence, while BBA on LDHs with Mg / Al=2:1 is in an isolated state and emits deep blue phosphorescence. Therefore, by regulating the metal ratio and charge distribution of the inorganic LDHs layer, the covalent interaction between LDHs and BBA molecules is effectively regulated, affecting the isolated / aggregated state of BBA molecules, and achieving effective regulation of their dynamic room temperature phosphorescence.

[0049] (7) Multi-level anti-counterfeiting encryption of LDH-17% BBA composite materials

[0050] Morse code encryption technology was realized using the afterglow of LDH-17%BBA composites with different Mg:Al ratios ( Figure 8 ). In the Morse code, cyan phosphorescence is encrypted as "lines" and dark blue phosphorescence is encrypted as "dots". (Mg:Al=4:1)LDH-17%BBA (marked as "a") and (Mg:Al=2:1)LDH-17%BBA (marked as "b") were made into anti-counterfeiting patterns, as shown in the figure. It should be noted that (Mg:Al=4:1)LDH-17%BBA (marked as "a") exhibits a time-varying phosphorescence emission from cyan to dark blue, while (Mg:Al=2:1)LDH-17%BBA (marked as "b") exhibits a continuous dark blue phosphorescence emission. For this reason, we can decipher the Morse code displayed by the sample. After turning off the ultraviolet light (280nm) excitation, the Morse code can be deciphered as "-", "·", "·-", "--", and decrypted as "TEAM", but this is deceptive information. The real message can be obtained after 2 seconds. At this time, the Morse code is deciphered as "·", "·", "·", "·", and decrypted as "EEII". Therefore, compared with the single-level encrypted phosphorescent system, the multi-level encryption process with time dimension has significant advantages.

Claims

1. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on changes in carrier structure, characterized in that: The following steps are involved: (1) synthesizing an inorganic carrier with hydroxyl groups on the surface and adjustable structural composition and preparing it into a suspension; (2) dissolving the phosphorescent molecule modified with boronic acid groups at both ends and adding an alkaline buffer solution to hydrolyze the boronic acid groups; (3) Weigh a certain amount of the inorganic carrier suspension of step (1) and the phosphorescent molecule solution containing boric acid groups at both ends of step (2), respectively, and stir for 1 hour to allow them to be fully dispersed and react. (4) Pour the fully reacted solution into a watch glass, place it in a 60°C oven, and dry it for 4 hours. (5) changing the microstructure of the inorganic carrier in step (1), repeating steps 2-(4) to synthesize organic-inorganic composite phosphorescent materials with different carrier structures; (6) Using the adjustable afterglow of composite phosphorescent materials constructed from different inorganic carriers to design multi-level encryption applications such as Morse code.

2. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on changes in carrier structure according to claim 1, characterized in that: In step (1), the hydroxyl-rich inorganic material is selected from montmorillonite (MMT), layered double hydroxides (LDHs), and silicon dioxide; preferably, hydrotalcite (LDHs); the divalent metal can be Mg, Zn, Ca, etc., and the trivalent metal can be Al, Ga, etc., and different methods can be regulated to synthesize different layer metal elements or different sizes of hydrotalcite; formamide and the like can be further introduced during the preparation process to obtain exfoliated thin-sheet LDHs, thereby further optimizing the performance of the composite material.

3. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on changes in carrier structure according to claim 1, characterized in that: In step (2), the phosphorescent molecule is an aromatic boronic acid molecule, the number of boronic acid groups in the molecule is 2 or 3, and the middle luminescent part can be selected from biphenyl, phenyl, tetraphenylethylene, etc.; the purpose of preparing the alkaline buffer solution is to hydrolyze the boronic acid molecules, and a K2CO3 / KHCO3 buffer system is selected.

4. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on carrier structure changes according to claim 1, characterized in that: In step (3), the amount of the inorganic substance and the phosphorescent molecule used to construct the composite material is in the following relationship: the phosphorescent molecule accounts for 5%-80% of the amount of the inorganic substance.

5. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on carrier structure changes according to claim 1, characterized in that: In step (4), the stirring time is 10 min-4 h, and the stirring temperature is room temperature; heating is performed appropriately to increase the degree of reaction, and the temperature range is 20-60°C.

6. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on carrier structure changes according to claim 1, characterized in that: The specific method for changing the microstructure of the inorganic carrier in step (5) is: by adjusting the feed ratio, the ratio of divalent and trivalent metals on the LDHs layer is adjusted, and the adjustment range is divalent: trivalent molar ratio = 2:1, 3:1, 4:1 and 5:

1.

7. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on carrier structure changes according to claim 1, characterized in that: The LDH-17% BBA composite powder with different divalent: trivalent molar ratios of Mg:Al was made into a "dot" pattern, and the UV light with a wavelength of 280nm was used to excite for 3s and then turned off to observe the phosphorescence changes of the anti-counterfeiting pattern and take photos. The cyan "dot" phosphorescent pattern represents "-", and the dark blue "dot" phosphorescent pattern represents "·", which is decrypted by referring to the Morse code table.

8. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on carrier structure changes according to claim 1, characterized in that: The constructed composite material exhibits multicolor and dynamic room temperature phosphorescence emission. Taking LDH-17% BBA as an example, it exhibits room temperature phosphorescence emission at 400nm and 465nm, respectively, and its phosphorescence lifetime is different. By regulating the molecular structure of inorganic substances, the luminescence intensity and lifetime at different wavelengths can be effectively adjusted.

9. A method for regulating the arrangement of chromophores and room temperature phosphorescence properties through covalent bonds based on changes in carrier structure according to claim 1, characterized in that: Used for anti-counterfeiting encryption or dynamic storage.