White light quantum dot, preparation method and light emitting diode

By using single-component white light quantum dots in WQLED, using halogen doping ZnSe quantum dots and covering the ZnS shell, the self-absorption and color drift problems in existing WQLEDs are solved, and efficient white light emission and stability are achieved, improving Device performance.

CN119020015APending Publication Date: 2024-11-26SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974146.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Due to the lack of efficient white light emitting layer, existing white light quantum dot light emitting diodes (WQLEDs) have lower electroluminescent performance than white organic light emitting diodes (WOLEDs), and there is a self-absorbing effect and Foster resonance energy transfer in hybrid QDs or series devices. , color drift and other problems affect device stability and application prospects.

Method used

Using single-component white light quantum dots, halogen doped ZnSe quantum dots are synthesized in an inert gas environment and coated with ZnS shell to form a Cl:ZnSe/ZnS structure, and the halogen ion doping amount and ZnS are synthesized and regulated by thermal implantation method. The thickness of the shell enables efficient white light emission and avoids self-absorption and color drift.

Benefits of technology

The excellent stability and efficient luminescence of white light quantum dots are achieved. The WQLED brightness of single-component white light QDs reaches 16610cd m-2, the maximum value of external quantum efficiency (EQE) is 7.96%, and the spectral stability is maintained under different operating voltages. Avoid color drift.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020015A_ABST
    Figure CN119020015A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of light-emitting materials, in particular to a white light quantum dot, a preparation method and a light-emitting diode. Selenium powder and octadecene are mixed to obtain a first precursor solution; mixing a zinc source, oleic acid and paraffin to obtain a second precursor solution; mixing a halogen source with octadecene to obtain a third precursor solution; mixing the first precursor solution and octyl mercaptan in an inert gas environment to obtain a fourth precursor solution; at 280-330 DEG C, the first precursor solution is injected into a mixed reaction of anhydrous zinc acetate, paraffin and oleic acid, then the third precursor solution is injected, then the fourth precursor solution is added, the white light quantum dots are obtained, the white light quantum dots comprise X: ZnSe / ZnS, and X comprises one or more than two of Cl, Br and I. The quantum dot provided by the invention is a single component emitting white light, and improves color drift and reabsorption effect. The patent of the invention is subsidized by the national key research and development plan 2022YFE0200200.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of luminescent materials, and in particular to a white light quantum dot, a preparation method and a light emitting diode. Background Art

[0002] Colloidal quantum dots (QDs) have attracted much attention due to their high photoluminescence quantum yield (PLQY), size-dependent tunable emission spectrum, narrow half-width, and low-cost solution processability, and are considered to be the next generation of display lighting materials. The performance of monochrome QDs-based light-emitting diodes (QLEDs) has approached the requirements of commercial applications, but the research on white QDs-based light-emitting diodes (WQLEDs), which are extremely important in practical applications, has lagged far behind. Due to the lack of efficient white light QDs emitting layers, the electroluminescent performance of current WQLEDs lags far behind that of the most advanced white organic light-emitting diodes (WOLEDs).

[0003] At present, the white light emitting layer of most WQLEDs is realized by mixing QDs of different colors or connecting red / green / blue (R / G / B) devices in series to achieve white light emission. However, the self-absorption effect and Förster resonance energy transfer (FRET) of the mixed QDs emitting layer lead to low efficiency of white light devices. The structure of the series device is complex and has a high turn-on voltage. In the process of device preparation, the upper solvent will corrode the lower material, causing the device structure to be damaged. When working for a long time, the aging degree of different QDs is inconsistent, resulting in serious color drift in both mixed QDs and series structure devices.

[0004] Therefore, designing and developing a method to prepare a stable and efficient white light QDs luminescent layer is of great significance for improving the application prospects of WQLED. Summary of the invention

[0005] In order to overcome the existing technical problems, the purpose of the present invention is to provide a white light quantum dot, a preparation method and a light-emitting diode. The white light quantum dot is a single component and has excellent stability.

[0006] Technical solution: In order to achieve the above objectives, the present invention provides the following technical solution: a method for preparing white light quantum dots, comprising:

[0007] Mixing selenium powder and octadecene, heating and stirring in an inert gas environment to obtain a first precursor solution;

[0008] Mixing a zinc source, oleic acid and paraffin, and heating and stirring under an inert gas environment to obtain a second precursor solution, wherein the zinc source includes zinc oxide and / or anhydrous zinc acetate;

[0009] Mixing a halogen source and octadecene, heating and dissolving, and obtaining a third precursor solution, wherein the halogen source comprises one or more of oleylamine chloride, oleylamine bromide, oleylamine iodine, phenethylamine chloride, phenethylamine bromide, and phenethylamine iodine;

[0010] mixing the first precursor solution and octanethiol under an inert gas environment to obtain a fourth precursor solution;

[0011] At 280-330° C., a first precursor solution is first injected into a reaction mixture of anhydrous zinc acetate, paraffin wax, and oleic acid, and then a third precursor solution is injected, wherein the volume ratio of the first precursor solution to the second precursor solution is 1.7-2.3:0.8-1.2; subsequently, the first precursor solution and the second precursor solution are alternately supplemented, and then the fourth precursor solution is added to react to obtain a quantum dot stock solution, and after purification treatment, white light quantum dots are obtained, wherein the white light quantum dots include X:ZnSe / ZnS, wherein X includes one or more of Cl, Br, and I.

[0012] The heating temperature for obtaining the first precursor solution is 240° C.-260° C., and the heating and stirring time is 1 h-7 h; optionally, the heating temperature is 240° C., and the heating and stirring time is 4 h.

[0013] The heating temperature for obtaining the second precursor solution is 240° C.-280° C., and the heating and stirring time is 15-30 min; optionally, the heating temperature is 240° C., and the heating and stirring time is 15 min.

[0014] The first precursor solution is first injected into a reaction mixture of anhydrous zinc acetate, paraffin and oleic acid at 280-330° C., wherein the molar concentration of zinc ions in the mixed solution after the reaction is 0.04-0.055 mol / L.

[0015] Wherein, the molar concentration of the first precursor solution is 0.15-0.25 mol / L, optionally 0.2 mol / L; or / and,

[0016] The molar concentration of the second precursor solution is 0.2-0.4 mol / L, optionally 0.3 mol / L; or / and,

[0017] The molar concentration of the third precursor solution is 0.01-0.02 mol / L.

[0018] The molar ratio of selenium to octanethiol in the first precursor solution in the fourth precursor solution is 1:1.4.

[0019] The volume ratio of the total amount of the first precursor solution, the second precursor solution, the third precursor solution and the fourth precursor solution added is 5:3:1:7.

[0020] The purification process includes adding anhydrous ethanol to the quantum dot stock solution to wash it until it becomes turbid, and then dispersing it in n-hexane after centrifugation.

[0021] The method comprises injecting a first precursor solution into a reaction mixture of anhydrous zinc acetate, paraffin wax and oleic acid at 280-330° C., and then injecting a third precursor solution; then alternately replenishing the first precursor solution and the second precursor solution, and then adding the fourth precursor solution to react and obtain a quantum dot stock solution, including:

[0022] Heat a mixture of 0.14-0.15 g of anhydrous zinc acetate, 13-16 ml of paraffin wax, and 0.9-1.1 ml of oleic acid to 280-330°C, inject 1.7-2.3 ml of the first precursor solution, and then inject 0.8-1.2 ml of the third precursor solution after 5s-15s, and then keep warm for 20-40 minutes;

[0023] Then, 2-3 ml of the first precursor solution and the second precursor solution are alternately added at an injection rate of 0.1 ml / min. Each time 0.5 ml of the first precursor solution or the second precursor solution is added, it is added again after an interval of 3-6 minutes to obtain a first intermediate solution; so that the reaction is sufficient.

[0024] The first intermediate solution was cooled to 240°C, and then 6-8 ml of the fourth precursor solution was added at an injection rate of 5 ml / h, and the temperature was raised to 290-310°C and kept at this temperature for 8-12 minutes to allow the reaction to be fully completed.

[0025] As a preferred method, the reaction system is purified, and the specific steps are as follows: the quantum dot stock solution is washed with anhydrous ethanol until it becomes turbid, and dispersed in n-hexane after centrifugation. The above steps are repeated 3 times, and the liquid concentration is adjusted to 10-15 g / L.

[0026] The present application also includes a second technical solution, a white light quantum dot, prepared by the above method, wherein the white light quantum dot comprises X:ZnSe / ZnS, where X comprises one or more of Cl, Br and I.

[0027] The white light quantum dots include a halogen-doped ZnSe core, the halogen includes one or more of Cl, Br and I, and a ZnS coating layer arranged outside the core.

[0028] The present application also includes a third technical solution, a light-emitting diode, including a light-emitting layer, and the light-emitting layer includes the above-mentioned white light quantum dots.

[0029] The EQE of the photodiode is 7.96% and the brightness reaches 16610cd m -2 .

[0030] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: (1) The single-component white light QDs prepared by halogen ion doping ZnSe QDs have excellent stability after being coated with a ZnS shell layer; (2) The maximum brightness of the WQLED prepared by the single-component white light QDs is 16610 cd m -2 , the maximum EQE is 7.96%; (3) The preparation method of the WQLED is simple and efficient. The single-component white light quantum dots act as the light-emitting layer to avoid or improve the color drift caused by the reabsorption effect between different quantum dots and the inconsistent aging degree of different color quantum dots during operation. (4) By adjusting the addition amount, it is convenient to adjust the addition amount of halogen ions, size control and ZnS shell coating. The single-component white light QDs have excellent stability as the light-emitting layer of WQLED. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic diagram of photoluminescence (PL) intensity-wavelength of different halogen-doped ZnSe quantum dot cores of the present application;

[0032] Figure 2 Schematic diagram of photoluminescence (PL) intensity-wavelength of ZnSe quantum dot cores with different third precursor doping amounts in the present application;

[0033] Figure 3 is a photoluminescence (PL) intensity-wavelength diagram of the quantum dots of Example 1 of the present application;

[0034] Figure 4 This is a schematic diagram of the diffraction intensity-angle of the core and core-shell white light quantum dots of the present application;

[0035] Figure 5 Transmission electron microscopy (TEM) of the core and core-shell quantum dots of the present application and the corresponding high-resolution images;

[0036] Figure 6 A schematic diagram of photoluminescence (PL) intensity-wavelength of the white light quantum dots of the present application and the ZnSe quantum dots of Comparative Example 1;

[0037] Figure 7 A schematic diagram of the structure of the light emitting diode of the present application;

[0038] Figure 8 The electroluminescence spectra of the light emitting diode under different voltages of Example 1 of the present application;

[0039] Fig. 9 A color coordinate diagram of the light emitting diode of Example 1 of the present application;

[0040] Fig.10 This is a graph of external quantum efficiency (EQE)-brightness of the light-emitting diode of the present application. DETAILED DESCRIPTION

[0041] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.

[0042] The present application provides a method for preparing white light quantum dots, comprising: mixing selenium powder and octadecene, heating and stirring in an inert gas environment to obtain a first precursor solution;

[0043] Mixing a zinc source, oleic acid and paraffin, heating and stirring under an inert gas environment to obtain a second precursor solution, wherein the zinc source includes zinc oxide and / or anhydrous zinc acetate;

[0044] Mixing a halogen source and octadecene, heating and dissolving, and obtaining a third precursor solution, wherein the halogen source comprises one or more of oleylamine chloride, oleylamine bromide, oleylamine iodine, phenethylamine chloride, phenethylamine bromide, and phenethylamine iodine;

[0045] mixing the first precursor solution and octanethiol under an inert gas environment to obtain a fourth precursor solution;

[0046] At 280-330° C., a first precursor solution is first injected into a reaction mixture of anhydrous zinc acetate, paraffin wax, and oleic acid, and then a third precursor solution is injected, wherein the volume ratio of the first precursor solution to the second precursor solution is 1.7-2.3:0.8-1.2; subsequently, the first precursor solution and the second precursor solution are alternately supplemented, and then the fourth precursor solution is added to react to obtain a quantum dot stock solution, and after purification treatment, white light quantum dots are obtained, wherein the white light quantum dots include X:ZnSe / ZnS, wherein X includes one or more of Cl, Br, and I.

[0047] In the embodiment of the present application, the quantum dots obtained are white light quantum dots. At 280-330°C, the first precursor solution is first injected into the reaction mixture of anhydrous zinc acetate, paraffin, and oleic acid, and then the third precursor solution is injected to facilitate the control of nucleation and allow the halogen to be doped in ZnSe to nucleate; by alternately supplementing the first precursor solution and the second precursor solution, it is convenient to control the growth of the nucleus, and by controlling the amount of the first precursor solution and the second precursor solution, it is convenient to control the size of the nucleus growth, and it is convenient to increase the size of the nucleus to 12-14nm. After alternately adding the first precursor solution and the second precursor solution, the fourth precursor solution is added to facilitate the control of the coating on the outside of X:ZnSe to form ZnS.

[0048] In the embodiment of the present application, the molar concentration of anhydrous zinc acetate in the reaction of mixing anhydrous zinc acetate, paraffin wax and oleic acid is less than the molar concentration of the second precursor solution, which facilitates the uniformity of conditional nucleation.

[0049] The heating temperature for obtaining the first precursor solution is 240° C.-260° C., and the heating and stirring time is 1 h-7 h; optionally, the heating temperature is 240° C., and the heating and stirring time is 4 h.

[0050] The heating temperature for obtaining the second precursor solution is 240° C.-280° C., and the heating and stirring time is 15-30 min; optionally, the heating temperature is 240° C., and the heating and stirring time is 15 min.

[0051] The first precursor solution is first injected into a reaction mixture of anhydrous zinc acetate, paraffin and oleic acid at 280-330° C., wherein the molar concentration of zinc ions in the mixed solution after the reaction is 0.04-0.055 mol / L.

[0052] Wherein, the molar concentration of the first precursor solution is 0.15-0.25 mol / L, optionally 0.2 mol / L; or / and,

[0053] The molar concentration of the second precursor solution is 0.2-0.4 mol / L, optionally 0.3 mol / L; or / and,

[0054] The molar concentration of the third precursor solution is 0.01-0.02 mol / L.

[0055] The molar ratio of selenium to octanethiol in the first precursor solution in the fourth precursor solution is 1:1.4.

[0056] The volume ratio of the total amount of the first precursor solution, the second precursor solution, the third precursor solution and the fourth precursor solution added is 5:3:1:7.

[0057] The purification process includes adding anhydrous ethanol to the quantum dot stock solution to wash it until it becomes turbid, and then dispersing it in n-hexane after centrifugation.

[0058] The method comprises injecting a first precursor solution into a reaction mixture of anhydrous zinc acetate, paraffin wax and oleic acid at 280-330° C., and then injecting a third precursor solution; then alternately replenishing the first precursor solution and the second precursor solution, and then adding the fourth precursor solution to react and obtain a quantum dot stock solution, including:

[0059] Heat a mixture of 0.14-0.15 g of anhydrous zinc acetate, 13-16 ml of paraffin wax, and 0.9-1.1 ml of oleic acid to 280-330°C, inject 1.7-2.3 ml of the first precursor solution, and then inject 0.8-1.2 ml of the third precursor solution after 5s-15s, and then keep warm for 20-40 minutes;

[0060] Then, 2-3 ml of the first precursor solution and the second precursor solution are alternately added at an injection rate of 0.1 ml / min. Each time 0.5 ml of the first precursor solution or the second precursor solution is added, it is added again after an interval of 3-6 minutes to obtain a first intermediate solution, so that the reaction is sufficient;

[0061] The first intermediate solution was cooled to 240°C, and then 6-8 ml of the fourth precursor solution was added at an injection rate of 5 ml / h, and the temperature was raised to 290-310°C and kept at this temperature for 8-12 minutes to allow the reaction to be fully completed.

[0062] As a preferred embodiment, when the temperature of the reaction mixture of anhydrous zinc acetate, paraffin and oleic acid is raised to 300° C., 1.7-2.3 ml of the first precursor solution is first injected, and 0.8-1.2 ml of the third precursor solution is injected after 10 seconds, followed by keeping the temperature for 30 minutes.

[0063] As a preferred method, the reaction system is purified, and the specific steps are as follows: the quantum dot stock solution is washed with anhydrous ethanol until it becomes turbid, and dispersed in n-hexane after centrifugation. The above steps are repeated 3 times, and the liquid concentration is adjusted to 10-15 g / L.

[0064] The present application also includes a second technical solution, a white light quantum dot, prepared by the above method, wherein the white light quantum dot comprises X:ZnSe / ZnS, where X comprises one or more of Cl, Br and I.

[0065] The white light quantum dots include a halogen-doped ZnSe core, the halogen includes one or more of Cl, Br and I, and a ZnS coating layer arranged outside the core.

[0066] The present application also includes a third technical solution, a light-emitting diode, including a light-emitting layer, and the light-emitting layer includes the above-mentioned white light quantum dots.

[0067] The EQE of the photodiode is 7.96% and the brightness reaches 16610cd m -2 .

[0068] The principle of the present invention is: in the present invention, a trace amount of halogen ions are doped during the synthesis of ZnSe QDs by hot injection, and self-trapped exciton emission (STE) in the broadband yellow-green light band is induced during the nucleation process of ZnSe QDs. By adjusting the doping amount of halogen ions, the size of ZnSe QDs and the thickness of the ZnS shell, the controllable synthesis of core / shell structure Cl:ZnSe / ZnS QDs with high efficiency white light emission (PLQY>80%) is successfully achieved. Compared with the white light emission of mixed QDs or tandem monochrome devices, this method effectively avoids the occurrence of self-absorption and color drift. In addition, the spectral shape of the WQLED prepared based on the single-component QDs is almost unchanged at different operating voltages, showing the excellent stability of the WQLED.

[0069] In order to illustrate the present invention, a method for synthesizing a single-component white light QDs provided by the present invention is described in detail below in conjunction with the figures and embodiments, but this should not be construed as a definition of the protection scope of the present invention.

[0070] Embodiment 1:

[0071] (1) First precursor solution (0.2 mol / L): 0.79 g of selenium powder was mixed with 50 ml of octadecene and heated and stirred at 240 °C for 4 h under nitrogen atmosphere;

[0072] (2) Second precursor solution (0.3 mol / L): 2.44 g zinc oxide, 40 ml oleic acid and 60 ml paraffin were mixed and heated and stirred at 240 °C for 15 min under nitrogen atmosphere;

[0073] (3) Third precursor solution (0.1 mol / L): Mix 0.03 g of oleylamine chloride and 1 ml of octadecene and heat until dissolved;

[0074] (4) Fourth precursor solution: 14 ml of the first precursor solution and 1 ml of octanethiol were mixed at 100 °C under nitrogen environment;

[0075] (5) 0.148 g of anhydrous zinc acetate, 1 ml of oleic acid and 15 ml of paraffin were placed in a three-necked flask, heated to 120°C to remove water vapor for 20 min, then vacuumed for 1 h, filled with nitrogen and heated to 300°C, 2 ml of the first precursor solution was injected first, and 10 s later, 1 ml of the third precursor solution was injected, and the temperature was kept for 30 min to obtain the first intermediate solution. The quantum dot core, i.e., Cl:ZnSe core, can be obtained.

[0076] (6) The first precursor solution and the second precursor solution are added at an injection rate of 0.1 ml / min, and each 0.5 ml of the precursor is added after an interval of 5 minutes. After alternately adding 3 ml of the first precursor solution and the second precursor solution (grown Cl:ZnSe nuclei can be obtained), the temperature is lowered to 240°C, and finally the fourth precursor solution is added at an injection rate of 5 ml / h. At the same time, the temperature is raised to 300°C, 7 ml of the fourth precursor solution is added, and the temperature is kept for 10 minutes and then lowered to obtain a quantum dot stock solution.

[0077] (7) The quantum dot stock solution was washed with anhydrous ethanol until turbid, and dispersed in n-hexane after centrifugation. The above steps were repeated 3 times, and the liquid concentration was adjusted to 15 g / L to obtain Cl:ZnSe / ZnS quantum dots, that is, quantum dots with a chlorine-doped ZnSe core and a ZnSs coating on the outside.

[0078] Preparation of light-emitting diodes (upright structure)

[0079] From bottom to top, a conductive substrate layer is first used, on which an ITO anode is arranged; a hole injection layer, a hole transport layer, a white light quantum dot luminescent layer, an electron transport layer and a metal aluminum electrode are arranged in sequence on top of the ITO anode, and a light-emitting unit is formed in this way to obtain a light-emitting diode device, see Figure 7 , the steps for preparing a light emitting diode are as follows:

[0080] (1) Cleaning of the glass substrate containing the ITO transparent electrode (i.e., anode): First, the ITO glass substrate was wiped with a dust-free cloth moistened with detergent, and then continuously ultrasonically cleaned with deionized water, acetone, and isopropanol for 15 minutes each. After that, the glass substrate was dried and its surface was treated with oxygen plasma gas for 15 minutes.

[0081] (2) Preparation of hole injection layer: PEDOT:PSS was spin-coated on the ITO glass at a speed of 4000 rpm for 40 s. After spin coating, the glass was annealed at 150°C for 15 min.

[0082] (3) Preparation of hole transport layer: TFB solution dissolved in chlorobenzene (CB) was spin-coated on the PEDOT:PSS film at a concentration of 8 mg / ml, a rotation speed of 4000 rpm, and a spin coating time of 40 s. After spin coating, the film was annealed at 120°C for 20 min.

[0083] (4) Preparation of white light quantum dot luminescent layer: A white light quantum dot solution dissolved in n-hexane was spin-coated on the TFB film at a concentration of 15 mg / ml, a rotation speed of 4000 rpm, and a spin coating time of 40 s. After spin coating, the film was annealed at 80°C for 5 min.

[0084] (5) Preparation of electron transport layer: The spin-coated device was transferred to a vacuum evaporation chamber and the vacuum degree was reduced to 10 -4 After Pa, Al electrode was evaporated at a speed of 100 nm in thickness.

[0085] Example 2

[0086] The difference from Example 1 is that in the preparation of white light quantum dots, step (5) is to place 0.148g of anhydrous zinc acetate, 1ml of oleic acid and 15ml of paraffin in a three-necked flask, heat to 120°C to remove water vapor for 15min, then evacuate for 1h, fill with nitrogen and heat to 310°C, first inject 2ml of the first precursor solution, inject 1ml of the second precursor solution after 10s, and keep warm for 30min. The first precursor solution and the second precursor solution are supplemented at an injection rate of 0.1ml / min, and each 0.5ml of the precursor is supplemented after an interval of 5min, and the first precursor solution and the second precursor solution are supplemented alternately after 3ml each, and then the temperature is lowered to 240°C, and finally the fourth precursor solution is supplemented at an injection rate of 5ml / h, and the temperature is raised to 300°C at the same time. After adding 3ml of the fourth precursor solution, it is kept warm for 10min and then cooled, and the quantum dot stock solution is obtained by reaction.

[0087] Example 3

[0088] The difference from Example 1 is that: the third precursor solution (0.1 mol / L): 0.016 g of phenethylammonium chloride and 1 ml of octadecene are mixed and heated until dissolved. The rest is similar to Example 1 and will not be explained in detail here.

[0089] Example 4

[0090] The difference from Example 1 is that: the third precursor solution (0.1 mol / L): 0.03484 g of oleylamine bromide and 1 ml of octadecene are mixed and heated until dissolved. The final product is Br:ZnSe / ZnS quantum dots, that is, quantum dots with Br-doped ZnSe core and ZnSs coated on the outside. The rest is similar to Example 1 and will not be explained in detail here.

[0091] Example 5

[0092] The difference from Example 1 is that: the third precursor solution (0.1 mol / L): 0.0395 g of oleylamine iodide and 1 ml of octadecene are mixed and heated until dissolved. The final product is I:ZnSe / ZnS quantum dots, that is, quantum dots with I-doped ZnSe core and ZnSs coated on the outside. The rest is similar to Example 1 and will not be explained in detail here.

[0093] Comparative Example 1:

[0094] 0.147g of anhydrous zinc acetate, 1ml of oleic acid and 15ml of paraffin are placed in a three-necked flask, the temperature is raised to 120℃ to remove water vapor for 15min, then vacuum is evacuated for 1h, the temperature is raised to 300℃ after nitrogen filling, 2ml of the first precursor solution is injected, and the temperature is kept warm for 30min to obtain a comparative intermediate product; then the first precursor and the second precursor are supplemented at an injection rate of 0.1ml / min, and each 0.5ml of the precursor is supplemented after an interval of 3min, and the first precursor solution and the second precursor solution are supplemented alternately by 3ml each, and finally the fourth precursor solution is supplemented at an injection rate of 5ml / h, and 7ml of the fourth precursor solution is added and kept warm for 10min before cooling; after cooling, the QDs stock solution is washed with anhydrous ethanol until it becomes turbid, and dispersed in n-hexane after centrifugation, the above steps are repeated 3 times, and the liquid concentration is adjusted to 15g / L.

[0095] Preparation of QDs light-emitting devices (upright structure)

[0096] From bottom to top, a conductive substrate layer is first used, on which an ITO anode is arranged; a hole injection layer, a hole transport layer, a QDs light-emitting layer, an electron transport layer and a metal aluminum electrode are arranged in sequence on top of the ITO anode, and a light-emitting unit is formed in this way to obtain a single-component white light QDs light-emitting diode device, see Figure 4 , the steps for preparing a single-component white light QDs light-emitting device are as follows:

[0097] (1) Cleaning of the glass substrate containing the ITO transparent electrode (i.e., anode): First, the ITO glass substrate was wiped with a dust-free cloth moistened with detergent, and then continuously ultrasonically cleaned with deionized water, acetone, and isopropanol for 15 minutes each. After that, the glass substrate was dried and its surface was treated with oxygen plasma gas for 15 minutes.

[0098] (2) Preparation of hole injection layer: PEDOT:PSS was spin-coated on the ITO glass at a speed of 4000 rpm for 40 s. After spin coating, the glass was annealed at 150°C for 15 min.

[0099] (3) Preparation of hole transport layer: TFB solution dissolved in chlorobenzene (CB) was spin-coated on the PEDOT:PSS film at a concentration of 8 mg / ml, a rotation speed of 4000 rpm, and a spin coating time of 40 s. After spin coating, the film was annealed at 120°C for 20 min.

[0100] (4) Preparation of QDs light-emitting layer: A QDs solution dissolved in n-hexane was spin-coated on the TFB film at a concentration of 15 mg / ml, a rotation speed of 4000 rpm, and a spin-coating time of 40 s. After spin-coating, the film was annealed at 80°C for 5 min.

[0101] (5) Preparation of electron transport layer: The spin-coated device was transferred to a vacuum evaporation chamber and the vacuum degree was reduced to 10 -4 After Pa, Al electrode was evaporated at a speed of 100 nm in thickness.

[0102] The difference between Comparative Example 2 and Example 1 is that in step (5), "first inject 2 ml of the first precursor solution, and then inject 1 ml of the third precursor solution after 10 seconds" is replaced by "first inject 2 ml of the first precursor solution, and then inject 0.5 ml of the third precursor solution after 10 seconds", and step (6) is not included. The rest is similar to Example 1 and will not be explained in detail here.

[0103] Comparative Example 3

[0104] The difference from Example 1 is that in step 5, "first inject 2 ml of the first precursor solution, and then inject 1 ml of the third precursor solution after 10 seconds" is replaced by "first inject 2 ml of the first precursor solution, and then inject 2 ml of the third precursor solution after 10 seconds", and step (6) is not included. The rest is similar to Example 1 and will not be explained in detail here.

[0105] Experimental test analysis

[0106] When halogen ions are doped during the nucleation process of ZnSe QDs, it is found that in addition to the intrinsic luminescence peak, an additional luminescence peak is formed at a long wavelength. The intensity of photoluminescence of ZnSe QDs doped with different halogen ions is tested, and the absorption intensity-wavelength diagram is obtained, as shown in the figure. Figure 1 As shown. Due to the introduction of halogen ions, a new luminescence peak appears at a long wavelength, forming a double-peak emission.

[0107] The "Cl:ZnSe core" prepared in the process of Example 1, the "comparative intermediate product" prepared in the process of Comparative Example 1, and the products of Comparative Example 2 and Comparative Example 3 were subjected to photoluminescence test. Figure 2 As shown, during the synthesis of Cl: ZnSe QDs cores, different amounts of the third precursor doping amount of QDs cores were added, wherein the doping amount of the third precursor was 0.5 ml (Comparative Example 2), 1 ml (Example 1) and 2 ml (Comparative Example 3), respectively. Figure 2In the figure, the curve of 0ml represents the "Cl:ZnSe core" prepared in the process of comparative example 1, and the photoluminescence intensity is tested to obtain an absorption intensity-wavelength graph. Due to the introduction of halogen ions, a new luminescence peak appears in the yellow-green band. When the halogen ion doping amount changes, the spectrum of the QDs core also changes. When the third precursor is 0.5ml, the small doping amount causes the long wavelength peak intensity to be too weak to form white light emission, and when the third precursor doping amount is 2ml, the large doping amount causes the long wavelength peak to be too strong and also cannot form white light emission; the doping amount of the third precursor in Example 1 of the present application is 1ml, which can emit better light.

[0108] The "Cl:ZnSe core", "grown Cl:ZnSe core" and "Cl:ZnSe / ZnS quantum dots" obtained in the preparation process of Example 1 were subjected to photoluminescence tests to obtain photoluminescence (PL) intensity-wavelength graphs, wherein the grown Cl:ZnSe core was not coated with a ZnS shell; while the Cl:ZnSe / ZnS quantum dots were grown Cl:ZnSe cores coated with a shell, and the short-wavelength peak of the spectrum was significantly increased. Because of the coating of the shell, the exposed surface defects of the QDs core were covered by the ZnS shell, reducing the occurrence of non-radiative recombination, thereby increasing the intensity of the intrinsic luminescence peak (short-wavelength peak) of the QDs. Single-component white light QDs can be prepared using the scheme of Example 1.

[0109] like Figure 4 As shown in the figure, "Example 1" represents the XRD spectrum of "Cl:ZnSe / ZnS quantum dots", and "quantum dot core" represents the "grown Cl:ZnSe core" obtained in the process. With the coating of the ZnS shell, the diffraction peak of Example 1 relative to the Cl:ZnSe QDs core moves toward the large angle direction, close to the peak position of the ZnS card standard, indicating that the ZnS shell grows on the quantum dot core. It should be noted that the diffraction peak position of Example 1 is somewhat different from that of the ZnS standard card. This is because the core-shell structure of Example 1 contains a large amount of ZnSe components, and the thickness of the ZnS shell is relatively thin, so that the diffraction peak of Example 1 is between ZnSe and ZnS.

[0110] like Figure 5 As shown, Figure a shows the transmission electron microscopy image and high-resolution transmission electron microscopy image (inset) of the "grown Cl:ZnSe core" obtained in the preparation process of Example 1, and it can be obtained that the average size of the Cl:ZnSe QDs core is 0.35nm, and the corresponding high-resolution image can show obvious lattice fringes, and the lattice spacing is 0.32nm, corresponding to the (111) surface of ZnSe; Figure 5b shows the transmission electron microscopy image and high-resolution transmission electron microscopy image (inset) of the "Cl:ZnSe / ZnS quantum dots" of Example 1. It can be seen that the average size of Cl:ZnSe / ZnS QDs is 12nm. Obvious lattice fringes are also found in the high-resolution transmission electron microscopy image. The lattice spacing is 0.31nm, corresponding to the (002) crystal plane of ZnS, proving the growth of the ZnS shell.

[0111] By testing the photoluminescence intensity of Example 1 and Comparative Example 1, an absorption intensity-wavelength graph was obtained, as shown in FIG. Figure 6 It can be clearly seen that the doped core-shell QDs can generate white light emission, while the undoped comparative example 1 only emits deep blue light; therefore, the single-component white light QDs prepared in Example 1 are used as the light-emitting layer of the LED device.

[0112] The single-component WQLED (light-emitting diode) prepared in Example 1 was characterized by electroluminescence spectrum, and the electroluminescence spectrum of the single-component WQLED was obtained. Figure 8 As shown, under the continuous action of bias voltage (5-8V), the spectrum hardly changes, indicating the stability under different operating voltages.

[0113] The single-component WQLED (light-emitting diode) prepared in Example 1 is characterized by color coordinates (CIE), and the CIE coordinates of the single-component WQLED are obtained, as shown in FIG. Fig. 9 As shown, the CIE coordinates are (0.28, 0.32), which are in the white light range, indicating that the prepared light-emitting diode exhibits white light emission.

[0114] The single-component WQLED (light-emitting diode) of Example 1 was tested for device performance, and the EQE of the single-component WQLED was obtained. Fig.10 As shown in Figure 2, the EQE of the device reaches 7.96% and the brightness reaches 16610 cd m -2 , which shows that the WQLED prepared based on single-component white light QDs has better device performance.

[0115] The present invention implements a Cl - The method of preparing single-component white light QDs by doping ZnSe QDs is to introduce Cl into the nucleation process of ZnSe QDs. - Produce a yellow-green luminescence peak, then by adjusting the Cl - By adjusting the doping amount, size of QDs and thickness of ZnS shell, single-component white light QDs were successfully prepared. Subsequently, WQLEDs were prepared based on the single-component white light QDs, showing stable white light emission.

[0116] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention of the present invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods. As long as they meet the purpose of the invention, as long as the QLED prepared by halogen ion-doped ZnSe QDs falls within the protection scope of the present invention.

Claims

1. A method for preparing white light quantum dots, characterized in that: include: Mixing selenium powder and octadecene, heating and stirring in an inert gas environment to obtain a first precursor solution; Mixing a zinc source, oleic acid and paraffin, and heating and stirring under an inert gas environment to obtain a second precursor solution, wherein the zinc source includes zinc oxide and / or anhydrous zinc acetate; Mixing a halogen source and octadecene, heating and dissolving, and obtaining a third precursor solution, wherein the halogen source comprises one or more of oleylamine chloride, oleylamine bromide, oleylamine iodine, phenethylamine chloride, phenethylamine bromide, and phenethylamine iodine; mixing the first precursor solution and octanethiol under an inert gas environment to obtain a fourth precursor solution; At 280-330° C., a first precursor solution is first injected into a reaction mixture of anhydrous zinc acetate, paraffin wax, and oleic acid, and then a third precursor solution is injected, wherein the volume ratio of the first precursor solution to the third precursor solution is 1.7-2.3:0.8-1.2; then the first precursor solution and the second precursor solution are alternately supplemented, and then the fourth precursor solution is added to react to obtain a quantum dot stock solution, and after purification treatment, white light quantum dots are obtained, wherein the white light quantum dots include X:ZnSe / ZnS, wherein X includes one or more of Cl, Br, and I.

2. The method according to claim 1, characterized in that The heating temperature for obtaining the first precursor solution is 240-260° C., and the heating and stirring time is 1 h-7 h; optionally, the heating temperature is 240° C., and the heating and stirring time is 4 h.

3. The method according to claim 1, characterized in that The heating temperature for obtaining the second precursor solution is 240° C.-280° C., and the heating and stirring time is 15-30 min; optionally, the heating temperature is 240° C., and the heating and stirring time is 15 min.

4. The method according to claim 1, characterized in that The first precursor solution is first injected into the reaction mixture of anhydrous zinc acetate, paraffin and oleic acid at 280-330° C., wherein the molar concentration of zinc ions in the mixed reaction solution is 0.04-0.055 mol / L; and / or, The molar concentration of the first precursor solution is 0.15-0.25 mol / L, optionally 0.2 mol / L; or / and, The molar concentration of the second precursor solution is 0.2-0.4 mol / L, optionally 0.3 mol / L; or / and, The molar concentration of the third precursor solution is 0.01-0.02 mol / L; and / or, The molar ratio of selenium to octanethiol in the first precursor solution in the fourth precursor solution is 1:1.

4.

5. The method according to claim 1, characterized in that The volume ratio of the total amount of the first precursor solution, the second precursor solution, the third precursor solution and the fourth precursor solution added is 5:3:1:

7.

6. The method according to claim 1, characterized in that The first precursor solution is first injected into the reaction mixture of anhydrous zinc acetate, paraffin wax and oleic acid at 280-330° C., and then the third precursor solution is injected; Subsequently, the first precursor solution and the second precursor solution are alternately added, and then the fourth precursor solution is added to react to obtain a quantum dot stock solution, including: Heat a mixture of 0.14-0.15 g of anhydrous zinc acetate, 13-16 ml of paraffin wax, and 0.9-1.1 ml of oleic acid to 280-330°C, inject 1.7-2.3 ml of the first precursor solution, and then inject 0.8-1.2 ml of the third precursor solution after 5-15 seconds, and then keep warm for 20-40 minutes; Then, 2-3 ml of the first precursor solution and the second precursor solution are alternately added at an injection rate of 0.1 ml / min. Each time 0.5 ml of the first precursor solution or the second precursor solution is added, it is added again after an interval of 3-6 minutes to obtain a first intermediate solution; The first intermediate solution was cooled to 240°C, and then 6-8 ml of the fourth precursor solution was added at an injection rate of 5 ml / h, and the temperature was raised to 290-310°C, and kept warm for 8-12 minutes.

7. The method according to claim 1, characterized in that The purification process includes adding anhydrous ethanol to the quantum dot stock solution to wash it until it becomes turbid, and dispersing it in n-hexane after centrifugation.

8. A white light quantum dot, characterized in that: White light quantum dots prepared by the method described in any one of claims 1 to 7, wherein the white light quantum dots include X:ZnSe / ZnS, and X includes one or more of Cl, Br and I.

9. The white light quantum dot according to claim 8, characterized in that: The white light quantum dot comprises a halogen-doped ZnSe core, wherein the halogen comprises one or more of Cl, Br and I, and a ZnS coating layer arranged outside the core.

10. A light emitting diode, characterized in that: It comprises a light-emitting layer, wherein the light-emitting layer comprises the white light quantum dots according to claim 8 or 9.