Ln-Yb co-doped efficient quantum shear luminescent material and preparation method thereof
Through the Ln-Yb co-doped tungstate material, the energy level difference of Yb ions is used to achieve near-infrared emission, which solves the problems of low luminous efficiency and unstable matrix of existing quantum shear materials, and improves the photoelectric conversion efficiency of solar cells And improves the stability of the material.
Patent Information
- Application Number
- CN202411109816.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
Existing quantum shear materials use single ion doping luminescence efficiency, and doped substrates such as fluoride and chloride are unstable, making it difficult to effectively improve the photoelectric conversion efficiency of solar cells in practical applications.
Using Ln-Yb co-doped tungstate material, the near-infrared emission is achieved through the energy level difference of Yb ions, matching the band gap width of silicon, improving the photoelectric conversion efficiency of solar cells, and producing NaYbxLn1yLn2z (WO4) through a specific preparation method. )2 materials.
The absorption of ultraviolet to visible light and the shear of high-energy photons are achieved, the photoelectric conversion efficiency of silicon-based solar cells is improved, and the stability and mechanical strength of the material are improved.
Smart Images

Figure CN119020032A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of luminescent materials, and in particular, relates to a Ln-Yb co-doped high-efficiency quantum shear luminescent material and a preparation method thereof. Background Art
[0002] Energy demand and green sustainable development strategies are major issues faced by all mankind. Solar energy has become one of the important clean energy sources due to its large resources, wide distribution range and environmental protection. Solar cells are the core components of photovoltaic power generation systems, and improving their photoelectric conversion efficiency has been a long-term concern and research issue for researchers.
[0003] The maximum theoretical photoelectric conversion efficiency of solar cells is 30.9%, but the actual conversion efficiency is relatively low, and spectral mismatch is one of the important reasons. At present, there are two common solutions: one is to introduce new solar cell materials or through structural design such as focusing and stacking, so that the spectral response of solar cells matches the solar spectrum to improve the photoelectric conversion efficiency; the other is to adapt the spectral response of solar cells by converting the solar spectrum to improve the photoelectric conversion efficiency. The former is costly and the process is complicated. The latter does not change the main structure of the battery, and the photoelectric efficiency can be improved only through spectral conversion. An effective way to solve the spectral conversion problem is quantum shearing, that is, rare earth ions convert a high-energy ultraviolet-visible photon into two near-infrared photons and are fully absorbed by the battery, so that two low-energy tubes are emitted for each high-energy photon absorbed, thereby obtaining a quantum efficiency greater than 100%, and ultimately achieving the purpose of improving the photoelectric conversion efficiency of the battery.
[0004] The existing quantum shearing materials have the following problems: (1) The luminescence efficiency of quantum shearing is very low when single ion doping is used. At the same time, the energies of the two photons released in this way are not necessarily equal and the emission wavelength is not easily controllable; (2) Most of the current quantum shearing materials use fluorides, chlorides and oxyfluorides as doping matrices, but the physical and chemical properties of fluorides and chlorides are unstable, they are easily deliquescent and corroded, and they have poor mechanical strength and temperature resistance, which limits their practical applications.
[0005] In view of this, this invention is proposed, which selects tungstate as the doping matrix and Ln-Yb ion co-doped quantum shearing material to fully utilize sunlight, thereby improving the conversion efficiency of crystalline silicon cells. Summary of the invention
[0006] The purpose of the present invention is to provide a Ln-Yb co-doped high-efficiency quantum shearing luminescent material and a preparation method thereof. The Ln-Yb co-doped high-efficiency quantum shearing luminescent material provided by the present invention can realize the absorption of ultraviolet to visible light, and then through the near-infrared emission of Yb, the high-energy photon is sheared into a photon that matches the bandgap width of crystalline silicon, thereby modifying the spectral distribution of sunlight and improving the effective utilization of sunlight by silicon-based solar cells.
[0007] To achieve the purpose of the present invention, the present invention adopts the following technical solution:
[0008] A Ln-Yb co-doped high-efficiency quantum shear luminescent material, wherein the chemical formula of the high-efficiency quantum shear luminescent material is: NaYb x Ln1 y Ln2 z (WO4)2;
[0009] Among them, 0.1≤x≤0.5, 0.5≤y+z≤0.9, y≥0, z≥0, x+y+z=1, y and z are not 0 at the same time.
[0010] Yb 3+ The luminescent wavelength (1000nm) corresponding to the energy level difference of the ions just matches the bandgap width of silicon, so Yb-doped luminescent materials are very suitable for improving the efficiency of silicon-based solar cells. After being excited by light, Ln-based element ions absorb high-energy ultraviolet or visible photons and excite adjacent Yb through cooperative energy transfer. 3+ ions, thereby causing energy level transitions and emitting infrared photons with a wavelength of about 1000nm. The Ln-Yb co-doped high-efficiency quantum shearing luminescent material provided by the present invention can achieve absorption of ultraviolet to visible light, and then through the near-infrared emission of Yb, high-energy photons are sheared into a photon that matches the bandgap width of crystalline silicon, modifying the spectral distribution of sunlight and improving the effective use of sunlight by silicon-based solar cells.
[0011] The present invention also provides a method for preparing the high-efficiency quantum shear luminescent material, wherein the preparation method comprises the following steps:
[0012] Step 1, weigh Na2CO3, WO3, Yb2O3, Ln1 oxide and Ln2 oxide according to the molar ratio of Na, W, Yb, Ln1 and Ln2 in the above chemical formula, mix them evenly, grind them to obtain raw material powder;
[0013] Step 2, calcining the raw material powder obtained in step 1 at a certain temperature for a certain time, and then cooling to room temperature;
[0014] Step 3: Grind the cooled solid into powder to obtain the high-efficiency quantum shear luminescent material.
[0015] Furthermore, in step 1, the oxide of Ln1 and the oxide of Ln2 are both Er2O3, Pr6O 11 , CeO2, Tb4O7, Nb2O3, Eu2O3 or Nd2O3, and the oxide of Ln1 is different from the oxide of Ln2.
[0016] Furthermore, in step 2, the calcination temperature is 800-1400°C, preferably 1000°C.
[0017] Furthermore, in step 2, the calcination time is 2 to 10 hours, preferably 4 hours.
[0018] Furthermore, in step 3, the particle size of the powder is 1 to 20 μm, preferably 5 μm.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] The Ln-Yb co-doped high-efficiency quantum shearing luminescent material provided by the present invention can realize the absorption of ultraviolet to visible light, and then shear the high-energy photon into a photon that matches the bandgap width of crystalline silicon through the near-infrared emission of Yb, thereby modifying the spectral distribution of sunlight and improving the effective utilization of sunlight by silicon-based solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The NaYb prepared in Example 1 0.5 Nd 0.45 Er 0.05 XRD pattern of (WO4)2 luminescent material;
[0022] Figure 2 The NaYb prepared in Example 1 0.5 Nd 0.45 Er 0.05 Photoluminescence spectrum of (WO4)2 luminescent material. DETAILED DESCRIPTION
[0023] The following are specific embodiments of the present invention, and the embodiments are intended to further describe the present invention rather than to limit the present invention.
[0024] Example 1
[0025] The chemical formula of the Ln-Yb co-doped high-efficiency quantum shear luminescent material provided in this embodiment is: NaYb 0.5 Nd 0.45 Er 0.05 (WO4)2.
[0026] Its preparation method is:
[0027] Step 1, weighing Na2CO3, WO3, Yb2O3, Nd2O3 and Er2O3 according to the molar ratio of Na, W, Yb, Nd and Er in the above chemical formula, mixing them evenly, grinding them, and obtaining raw material powder;
[0028] Step 2, calcining the raw material powder obtained in step 1 at 1000° C. for 4 hours and then cooling to room temperature;
[0029] Step 3: Grind the cooled solid into powder to obtain a high-efficiency quantum shear luminescent material with a particle size of 5 μm.
[0030] The phase and crystal structure of the obtained material were analyzed by X-ray diffraction. Figure 1 As shown, it is proved that the luminescent material NaYb 0.5 Nd 0.45 Er 0.05 (WO4)2, and the material is a tetragonal polycrystalline powder, which is consistent with the diffraction pattern of the standard card JCPDS48-0886. Figure 2 As shown in the figure, it was determined that the material underwent quantum shearing under the excitation of ultraviolet light with a wavelength of 365nm and emitted light of 980nm in the near-infrared region.
[0031] Example 2
[0032] The chemical formula of the Ln-Yb co-doped high-efficiency quantum shear luminescent material provided in this embodiment is: NaYb 0.5 Pr 0.45 Tb 0.05 (WO4)2.
[0033] Its preparation method is:
[0034] Step 1: Na2CO3, WO3, Yb2O3, Pr6O 11 and Tb4O7 according to the molar ratio of Na, W, Yb, Pr and Tb in the above chemical formula, weigh them, mix them evenly, grind them, and obtain raw material powder;
[0035] Step 2, calcining the raw material powder obtained in step 1 at 1000° C. for 4 hours and then cooling to room temperature;
[0036] Step 3: Grind the cooled solid into powder to obtain a high-efficiency quantum shear luminescent material with a particle size of 5 μm.
[0037] X-ray diffraction was used to analyze the phase and crystal structure of the obtained material, proving that the luminescent material NaYb was obtained by this method. 0.5 Pr 0.45 Tb 0.05 (WO4)2.
[0038] Example 3
[0039] The chemical formula of the Ln-Yb co-doped high-efficiency quantum shear luminescent material provided in this embodiment is: NaYb 0.3 Er 0.4 Tb 0.3 (WO4)2.
[0040] Its preparation method is:
[0041] Step 1, weighing Na2CO3, WO3, Yb2O3, Er2O3 and Tb4O7 according to the molar ratio of Na, W, Yb, Er and Tb in the above chemical formula, mixing them evenly, grinding them to obtain raw material powder;
[0042] Step 2, calcining the raw material powder obtained in step 1 at 1000° C. for 6 hours and then cooling to room temperature;
[0043] Step 3: Grind the cooled solid into powder to obtain a high-efficiency quantum shear luminescent material with a particle size of 3 μm.
[0044] X-ray diffraction was used to analyze the phase and crystal structure of the obtained material, proving that the luminescent material NaYb was obtained by this method. 0.3 Er 0.4 Tb 0.3 (WO4)2.
[0045] Example 4
[0046] The chemical formula of the Ln-Yb co-doped high-efficiency quantum shear luminescent material provided in this embodiment is: NaYb 0.1 Eu 0.5 Ce 0.4 (WO4)2.
[0047] Its preparation method is:
[0048] Step 1, weighing Na2CO3, WO3, Yb2O3, Eu2O3 and CeO2 according to the molar ratio of Na, W, Yb, Eu and Ce in the above chemical formula, mixing them evenly, grinding them, and obtaining raw material powder;
[0049] Step 2, calcining the raw material powder obtained in step 1 at 1000° C. for 10 hours and then cooling to room temperature;
[0050] Step 3: Grind the cooled solid into powder to obtain a high-efficiency quantum shear luminescent material with a particle size of 2 μm.
[0051] X-ray diffraction was used to analyze the phase and crystal structure of the obtained material, proving that the luminescent material NaYb was obtained by this method.0.1 Eu 0.5 Ce 0.4 (WO4)2.
[0052] Example 5
[0053] The chemical formula of the Ln-Yb co-doped high-efficiency quantum shear luminescent material provided in this embodiment is: NaYb 0.1 Er 0.3 Ce 0.6 (WO4)2.
[0054] Its preparation method is:
[0055] Step 1, weigh Na2CO3, WO3, Yb2O3, Er2O3 and CeO2 according to the molar ratio of Na, W, Yb, Er and Ce in the above chemical formula, mix them evenly, grind them to obtain raw material powder;
[0056] Step 2, calcining the raw material powder obtained in step 1 at 1000° C. for 10 hours and then cooling to room temperature;
[0057] Step 3: Grind the cooled solid into powder to obtain a high-efficiency quantum shear luminescent material with a particle size of 2 μm.
[0058] X-ray diffraction was used to analyze the phase and crystal structure of the obtained material, proving that the luminescent material NaYb was obtained by this method. 0.1 Er 0.3 Ce 0.6 (WO4)2.
[0059] Example 6
[0060] The chemical formula of the Ln-Yb co-doped high-efficiency quantum shear luminescent material provided in this embodiment is: NaYb 0.1 Nb 0.9 (WO4)2.
[0061] Its preparation method is:
[0062] Step 1, weigh Na2CO3, WO3, Yb2O3 and Nb2O3 according to the molar ratio of Na, W, Yb and Nb in the above chemical formula, mix them evenly, grind them to obtain raw material powder;
[0063] Step 2, calcining the raw material powder obtained in step 1 at 1400° C. for 2 hours, and then cooling to room temperature;
[0064] Step 3: Grind the cooled solid into powder to obtain a high-efficiency quantum shear luminescent material with a particle size of 1 μm.
[0065] X-ray diffraction was used to analyze the phase and crystal structure of the obtained material, proving that the luminescent material NaYb was obtained by this method. 0.1 Nb 0.9 (WO4)2.
[0066] Example 7
[0067] The chemical formula of the Ln-Yb co-doped high-efficiency quantum shear luminescent material provided in this embodiment is: NaYb 0.5 Er 0.5 (WO4)2.
[0068] Its preparation method is:
[0069] Step 1, weigh Na2CO3, WO3, Yb2O3 and Er2O3 according to the molar ratio of Na, W, Yb and Er in the above chemical formula, mix them evenly, grind them to obtain raw material powder;
[0070] Step 2, calcining the raw material powder obtained in step 1 at 800° C. for 6 hours and then cooling to room temperature;
[0071] Step 3: Grind the cooled solid into powder to obtain a high-efficiency quantum shear luminescent material with a particle size of 20 μm.
[0072] X-ray diffraction was used to analyze the phase and crystal structure of the obtained material, proving that the luminescent material NaYb was obtained by this method. 0.5 Er 0.5 (WO4)2.
[0073] Comparative Example 1
[0074] This comparative example is the same as Example 1, except that Yb2O3 is not added in step 1 to prepare NaNd 0.5 Er 0.5 (WO4)2.
[0075] Comparative Example 2
[0076] This comparative example is the same as Example 1, except that more Yb2O3 is added in step 1 to prepare NaYb 0.8 Nd 0.1 Er 0.1 (WO4)2.
[0077] Test Example 1
[0078] This test example tests the performance of the luminescent materials prepared in each embodiment.
[0079] Detection method: A Hitachi F-4600 fluorescence spectrometer equipped with a 150W xenon lamp was used to collect visible luminescence spectra, and an Edinburgh FLS1000 fluorescence spectrometer was used to measure infrared luminescence spectra.
[0080] The test results are shown in Table 1:
[0081] Table 1
[0082] Chemical composition Quantum yield (%) Example 1 <![CDATA[NaYb 0.5 Nd 0.45 Is 0.05 (WO4)2]]> 173 Example 2 <![CDATA[NaYb 0.5 Pr 0.45 Tb 0.05 (WO4)2]]> 162 Example 3 <![CDATA[NaYb 0.3 Is 0.4 Tb 0.3 (WO4)2]]> 144 Example 4 <![CDATA[NaYb 0.1 I 0.5 What 0.4 (WO4)2]]> 127 Example 5 <![CDATA[NaYb 0.1 Is 0.3 Ce 0.6 (WO4)2]]> 122 Example 6 <![CDATA[NaYb 0.1 Nb 0.9 (WO4)2]]> 101 Example 7 <![CDATA[NaYb 0.5 Is 0.5 (WO4)2]]> 135 Comparative Example 1 <![CDATA[NaNd 0.5 Is 0.5 (WO4)2]]> 76 Comparative Example 2 <![CDATA[NaYb 0.8 Nd 0.1 Is 0.1 (WO4)2]]> 61
[0083] It can be seen from the results in Table 1 that, compared with Comparative Examples 1 and 2, the Ln-Yb co-doped high-efficiency quantum shear luminescent material prepared in the present invention has a high quantum yield.
Claims
1. A Ln-Yb co-doped high-efficiency quantum shear luminescent material, It is characterized in that The chemical formula of the high-efficiency quantum shear luminescent material is: NaYb x Ln1 y Ln2 z (WO 4 ) 2 ; Among them, 0.1≤x≤0.5, 0.5≤y+z≤0.9, y≥0, z≥0, x+y+z=1, y and z are not 0 at the same time.
2. A method for preparing the high-efficiency quantum shear luminescent material according to claim 1, It is characterized in that The preparation method comprises the following steps: Step 1: Na 2 CO 3 , WO 3 , Yb 2 O 3 , Ln1 oxide and Ln2 oxide are weighed according to the molar ratio of Na, W, Yb, Ln1 and Ln2 in the above chemical formula, mixed evenly, and ground to obtain raw material powder; Step 2, calcining the raw material powder obtained in step 1 at a certain temperature for a certain time, and then cooling to room temperature; Step 3: Grind the cooled solid into powder to obtain the high-efficiency quantum shear luminescent material.
3. The preparation method according to claim 2, It is characterized in that In step 1, the oxide of Ln1 and the oxide of Ln2 are both Er 2 O 3 , Pr 6 O 11 、CeO 2 , Tb 4 O 7 , Nb 2 O 3 、Eu 2 O 3 or Nd 2 O 3 One of them, and the oxide of Ln1 is different from the oxide of Ln2.
4. The preparation method according to claim 2, It is characterized in that In step 2, the calcination temperature is 800-1400°C.
5. The preparation method according to claim 4, It is characterized in that The calcination temperature is 1000°C.
6. The preparation method according to claim 4 or 5, It is characterized in that In step 2, the calcination time is 2 to 10 hours.
7. The preparation method according to claim 6, It is characterized in that The calcination time was 4 hours.
8. The preparation method according to claim 2, It is characterized in that In step 3, the particle size of the powder is 1 to 20 μm.
9. The preparation method according to claim 8, It is characterized in that The particle size of the powder is 5 μm.