Cr3+ / Cr4 + ion doped NIR-II fluorescent material as well as preparation and application thereof

Through the Cr3+/Cr4+ ion-doped NIR-II fluorescent material, the quad-coordination lattice and sintering atmosphere regulation, the problems of limited emission range of Cr3+ ion-doped materials and difficulty in preparing Cr4+ materials in the prior art are solved, achieving high efficiency The broadband near-infrared emission has expanded the application of near-infrared spectral analysis technology.

CN119020035APending Publication Date: 2024-11-26NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411013355.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The peak wavelength of existing Cr3+ ion-doped near-infrared fluorescent materials is mostly concentrated within 800nm, making it difficult to achieve efficient emission of above 800nm, and Cr4+ ion-doped near-infrared fluorescent materials are difficult to prepare because CrO2 is easy to decompose at high temperatures.

Method used

The peak value is prepared by using Cr3+/Cr4+ ion doped NIR-II fluorescent material by occupies the four-coordinated lattice positions in the matrix and is regulated in different sintering atmospheres (non-oxidizing atmosphere and oxidizing atmosphere). Fluorescent materials with wavelengths in the range of 900-1700nm achieve uniform distribution and efficient emission of the overall spectrum.

Benefits of technology

The preparation of fluorescent materials with Cr3+ or Cr4+ as the luminescence center has been realized. The peak wavelength can reach more than 1167nm, the fluorescence intensity is enhanced, and the spectral range is expanded. It is suitable for near-infrared LED/LD devices, covering broadband near-infrared spectrum, and expanding near-infrared spectrum analysis. Application of technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020035A_ABST
    Figure CN119020035A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of near-infrared fluorescent material preparation technologies and near-infrared light source devices, and particularly relates to a Cr < 3 + > / Cr < 4 + > ion doped NIR-II fluorescent material and preparation and application thereof. The luminescent center of the fluorescent material is Cr < 3 + > / Cr < 4 + > ions, NIR-II near-infrared fluorescence is emitted under excitation of ultraviolet-visible light with the wavelength of 250-650 nm, and the fluorescence spectrum wavelength of the fluorescent material is 900-1700 nm; the chemical general formula is SrLaCrxGa (3-x) O7 or SrLaCrxScyGa (3-x-y) O7, x represents the doping concentration (0.001 < = x < = 0.025) of Cr < 3 + > / Cr < 4 + > ions, and y represents the doping concentration (0.001 < = y < = 0.05) of Sc < 3 + >. The fluorescent material with Cr < 3 + > or Cr < 4 + > ions as a luminescence center is respectively obtained by regulating and controlling the sintering atmosphere, and the fluorescent material product wholly emits near-infrared light located in NIR-II under the excitation of ultraviolet-visible light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of near-infrared fluorescent material preparation technology and near-infrared light source devices, and particularly relates to a Cr 3+ / Cr 4+ Ion-doped NIR-II fluorescent materials and their preparation and applications. Background Art

[0002] Near-infrared luminescence has the characteristics of deep penetration, high sensitivity and low background. Near-infrared spectroscopy technology has shown wide application value in the fields of biomedicine, food testing and smart wearables. Near-infrared light source is the prerequisite for the application of near-infrared spectroscopy analysis technology. It is usually required that the spectrum output by the near-infrared light source is wide enough to cover a wide enough range. The development and research of new broadband near-infrared fluorescent materials and their application in near-infrared light source devices have attracted widespread attention from researchers around the world.

[0003] Cr 3+ With special 3d 3 The changes of electron configuration and crystal field environment affect Cr 3+ The 3d electron transition of Cr 3+ In a six-coordinated weak crystal field environment, due to the spin-allowed 4 T2- 4 A2 transition, broadband near-infrared emission from 650-1200nm can be observed. 3+ Ion-doped near-infrared fluorescent materials have peak wavelengths concentrated within 800nm; Cr with peak wavelengths greater than 800nm ​​and high internal and external quantum yields 3+ There are few ion-doped near-infrared fluorescent materials. 4+ The ion has a broadband emission from 1000-1500nm and has potential feasibility in non-invasive detection applications. However, CrO2 can decompose into Cr3O2 at 250-500℃, so it is difficult to obtain Cr 4+ The preparation method of doped near-infrared fluorescent materials needs further exploration. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a Cr 3+ / Cr 4+ An ion-doped near-infrared II (NIR-II) fluorescent material and its application, and a preparation method thereof are provided. The NIR-II fluorescent material emits NIR-II near-infrared light under ultraviolet-visible light excitation, and the overall spectrum presents a uniform distribution.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] In one aspect, the present invention provides a Cr 3+ / Cr 4+ Ion-doped NIR-II fluorescent materials, whose luminescence centers are Cr 3+ and Cr 4+ ions, occupying four-coordinated lattice positions in the matrix material.

[0007] The general chemical formula of the fluorescent material is SrLaCr x Ga (3-x) O7 or SrLaCr x Sc y Ga (3-x-y) O7, x represents Cr 3+ / Cr 4+ Ion doping concentration, and 0.001≤x≤0.025, y represents Sc 3+ The doping concentration is 0.001≤y≤0.05. The luminescent center of the fluorescent material is Cr 3+ or Cr 4+ ion.

[0008] Preferably, Cr 3+ / Cr 4+ The source material of the doping ions is Cr2O3.

[0009] Preferably, when the sintering atmosphere is nitrogen, argon or other non-oxidizing atmosphere, the luminescent center of the obtained fluorescent material is Cr 3+ When the sintering atmosphere is oxygen, air or other oxidizing atmosphere, the luminescent center of the obtained fluorescent material is Cr 4+ .

[0010] Preferably, the fluorescence spectrum wavelength of the fluorescent material is between 900-1700 nm.

[0011] Preferably, the excitation wavelength of the fluorescent material is ultraviolet-visible light in the range of 250-650nm, and can emit near-infrared light in NIR-II.

[0012] On the other hand, the present invention provides a method for preparing the above-mentioned Cr 3+ / Cr 4+ The method for ion-doping NIR-II fluorescent materials comprises the following steps: weighing raw materials SrCO3, La2O3, Ga2O3, Cr2O3 and Sc2O3 according to the stoichiometric ratio, mixing them evenly and putting them into a crucible, sintering them at 1200-1400°C for 3-5 hours in a reducing or oxidizing atmosphere, and cooling them to room temperature to obtain the fluorescent material.

[0013] Preferably, the raw materials SrCO3, La2O3, Ga2O3, and Cr2O3 are weighed according to the stoichiometric ratio, mixed evenly, sintered at 1400°C for 4 hours in a nitrogen atmosphere, and then cooled to room temperature to obtain the fluorescent material SrLaCr 0.009 Ga 2.991 O7.

[0014] Alternatively, the raw materials SrCO3, La2O3, Ga2O3, and Cr2O3 are weighed according to the stoichiometric ratio, mixed evenly, sintered at 1400°C for 4 hours in an air atmosphere, and then cooled to room temperature to obtain the fluorescent material SrLaCr 0.009 Ga 2.991 O7.

[0015] Or weigh the raw materials SrCO3, La2O3, Ga2O3, Cr2O according to the stoichiometric ratio 3、 Sc2O3, mixed evenly, sintered at 1400℃ for 4 hours in a nitrogen atmosphere, and then cooled to room temperature to obtain the fluorescent material SrLaCr 0.009 Sc 0.03 Ga 2.961 O7.

[0016] In addition, the present invention provides the above-mentioned Cr 3+ / Cr 4+ Application of ion-doped NIR-II fluorescent materials, specifically, the fluorescent materials are used in near-infrared LED / LD devices.

[0017] Compared with the prior art, the advantages and positive effects of the present invention are:

[0018] (1) Provides a Cr at a four-coordinated lattice position 3+ or Cr 4+ The NIR-II fluorescent material with luminescence center is prepared by 3+ SrLaCr for the luminescence center x Ga (3-x) The peak wavelength of the fluorescence spectrum of O7 is above 900 mm and can reach around 1167 mm. 4+ SrLaCr for the luminescence center x Ga (3-x) O7 can achieve broadband emission with a higher peak wavelength in the fluorescence spectrum, and the overall spectrum is evenly distributed.

[0019] (2) The present invention also prepares SrLaCr x Sc y Ga (3-x-y)O7, the fluorescence intensity is further enhanced, and the peak wavelength can be red-shifted to 1208nm, further improving the spectral width of the near-infrared light source output, which can cover a sufficiently wide range and expand the application of near-infrared spectral analysis technology.

[0020] (3) The preparation method of the present invention is simple. By rationally matching the raw materials and regulating the parameters thereof, SrLaCr can be prepared which emits NIR-II near-infrared light as a whole under the excitation of ultraviolet-visible light in the range of 250-650nm. x Ga (3-x) O7 or SrLaCr x Sc y Ga (3-x-y) O7. This method converts the sintering atmosphere into a non-oxidizing atmosphere and an oxidizing atmosphere, which can achieve the goal of changing from Cr 3+ and Cr 4+ Cr 3+ or Cr 4+ Ion-doped NIR-II fluorescent materials facilitate the application of near-infrared LED / LD devices, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The XRD spectra of the fluorescent material of Example 1 prepared by different temperatures and different sintering times of the present invention;

[0022] Figure 2 The fluorescence emission spectrum of the fluorescent material prepared in Example 1 of the present invention;

[0023] Figure 3 The XRD spectrum of the fluorescent material prepared in Example 2 of the present invention;

[0024] Figure 4 The fluorescence emission spectrum of the fluorescent material prepared in Example 2 of the present invention;

[0025] Figure 5 The XRD spectrum of the fluorescent material prepared in Example 3 of the present invention;

[0026] Figure 6 Scanning electron microscope photo, X-ray spectrum and element distribution photo of the fluorescent material prepared in Example 3 of the present invention

[0027] Figure 7 The excitation and emission spectra of the fluorescent material prepared in Example 3 of the present invention;

[0028] Figure 8 The XRD spectrum of the fluorescent material prepared in Example 4 of the present invention;

[0029] Fig. 9 The fluorescence emission spectrum of the fluorescent material prepared in Example 4 of the present invention;

[0030] Fig.10 The XRD spectrum of the fluorescent material prepared in Example 5 of the present invention;

[0031] Fig.11 The fluorescence emission spectrum of the fluorescent material prepared in Example 5 of the present invention;

[0032] Fig.12 This is the XRD spectrum of the fluorescent material prepared in Example 6 of the present invention;

[0033] Fig.13 The fluorescence emission spectra of the fluorescent materials prepared in Example 6 and Example 3 of the present invention obtained under the excitation of light of different wavelengths;

[0034] Fig.14 The UV-visible-infrared absorption spectra of the fluorescent materials prepared in Example 6 and Example 3 of the present invention;

[0035] Fig.15 This is the XRD spectrum of the fluorescent material prepared in Example 7 of the present invention;

[0036] Fig.16 The fluorescence emission spectra of the fluorescent materials prepared in Example 7 and Example 3 of the present invention;

[0037] Fig.17 The UV-visible absorption spectra of the fluorescent materials prepared in Example 7 and Example 3 of the present invention;

[0038] Fig.18 The photos taken by a common camera and an infrared camera after the near-infrared LED device of Example 8 of the present invention is lit;

[0039] Fig.19 This is the luminescence spectrum of the near-infrared LED device of Example 8 of the present invention when driven by different currents. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] According to the chemical formula SrLaCr 0.003 Ga 2.997The stoichiometric ratio of O7 was 5 mmol SrCO3, 2.5 mmol La2O3, 7.4925 mmol Ga2O3 and 0.0075 mmol Cr2O3 were weighed respectively, mixed evenly and put into a crucible. Under a nitrogen (N2) atmosphere, the preparation temperature was 1400°C and sintered for 4 hours to obtain a NIR-II near-infrared fluorescent material.

[0043] Figure 1 When preparing Example 1, different sintering temperatures and sintering times were used, and the XRD spectra of the obtained fluorescent materials were obtained. When the sintering time was fixed at 4 hours and the sintering temperature was gradually increased in the range of 1200-1500℃, as the sintering temperature increased, the product impurities gradually disappeared and the crystallinity increased; but the XRD spectra of the products obtained at 1400℃ and 1500℃ were not much different. When the sintering temperature was 1400℃ and the sintering time was 3 hours, it can be concluded from the XRD spectrum that the product crystallinity was not high; when the sintering time was increased to 4 hours, its crystallinity was significantly improved compared with the product obtained in 3 hours; when the sintering time was increased to 5 hours, its crystallinity was not significantly changed compared with the product obtained in 4 hours. Based on this, 1400℃ and sintering for 4 hours were selected as the optimal parameters. .

[0044] Figure 2 The fluorescence emission spectrum of the fluorescent material prepared in Example 1 obtained by excitation at 450nm, emitting an emission band located in the range of 950-1500nm, with a peak at about 1167nm, which corresponds to Cr 3+ The stimulus is located at 2 The electrons at the T1 level fall back to 4 T1 energy level process.

[0045] Example 2

[0046] According to the chemical formula SrLaCr 0.005 Ga 2.995 The stoichiometric ratio of O7 was 5 mmol SrCO3, 2.5 mmol La2O3, 7.4875 mmol Ga2O3 and 0.0125 mmol Cr2O3 were weighed respectively, mixed evenly and put into a crucible. Under a nitrogen (N2) atmosphere, the preparation temperature was 1400°C and sintered for 4 hours to obtain a NIR-II near-infrared fluorescent material.

[0047] Figure 3 This is the XRD spectrum of the fluorescent material prepared in Example 2. It can be seen that its diffraction peak still completely corresponds to the diffraction peak of SrLaGa3O7, and there is no obvious difference from the XRD spectrum of the fluorescent material prepared in Example 1.

[0048] Figure 4This is the fluorescence emission spectrum of the fluorescent material prepared in Example 2 obtained by excitation at 450nm. Compared with the fluorescence emission spectrum of the fluorescent material in Example 1, there is no obvious change in the peak wavelength and the shape of the emission spectrum, but the luminous intensity is improved compared with Example 1.

[0049] Example 3

[0050] According to the chemical formula SrLaCr 0.009 Ga 2.991 The stoichiometric ratio of O7 was 5 mmol SrCO3, 2.5 mmol La2O3, 7.4775 mmol Ga2O3 and 0.0225 mmol Cr2O3 were weighed respectively, mixed evenly and put into a crucible. Under a nitrogen (N2) atmosphere, the preparation temperature was 1400°C and sintered for 4 hours to obtain a NIR-II near-infrared fluorescent material.

[0051] Figure 5 This is the XRD spectrum of the fluorescent material prepared in Example 3. It can be seen that its diffraction peak still completely corresponds to the diffraction peak of SrLaGa3O7, and there is no obvious difference from the XRD spectra of the fluorescent materials prepared in Examples 1 and 2.

[0052] Figure 6 The scanning electron microscope photo, X-ray spectrum and element distribution photo of the fluorescent material prepared in Example 3. The prepared sample contains Sr, La, Ga, O and Cr elements, and the distribution is uniform.

[0053] Figure 7 The fluorescence excitation and emission spectra of the fluorescent material prepared in Example 3. The three excitation bands in the excitation spectrum correspond to Cr 3+ stimulated 4 T1( 4 F) → 4 T1( 4 P), 4 T1→ 4 A2 and 4 T1→ 4 T2 electron transition, indicating that the phosphor obtained in N2 is Cr 3+ Doping did not occur due to Cr 3+ To Cr 4+ Compared with the fluorescent emission spectra of the fluorescent materials in Examples 1 and 2, the peak wavelength and the emission spectrum shape have no significant changes, but the luminous intensity is further improved compared with Examples 1 and 2.

[0054] Example 4

[0055] According to the chemical formula SrLaCr 0.009 Ga 2.991The stoichiometric ratio of O7 is 5 mmol SrCO3, 2.5 mmol La2O3, 7.4775 mmol Ga2O3 and 0.0225 mmol Cr2O3. After being evenly mixed, they are put into a crucible. Under an argon (Ar2) atmosphere, the preparation temperature is 1400°C and sintered for 4 hours to obtain a NIR-II near-infrared fluorescent material.

[0056] Figure 8 This is the XRD spectrum of the fluorescent material prepared in Example 4. It can be seen that its diffraction peak still completely corresponds to the diffraction peak of SrLaGa3O7, and there is no obvious difference from the XRD spectrum of the fluorescent material prepared in Example 3.

[0057] Fig. 9 This is the fluorescence emission spectrum of the fluorescent material prepared in Example 4 obtained by excitation at 450nm. Compared with the fluorescence emission spectrum of the fluorescent material in Example 3, there is no obvious change in the peak wavelength and the shape of the emission spectrum, and the luminous intensity is not much different from that in Example 3.

[0058] Example 5

[0059] According to the chemical formula SrLaCr 0.011 Ga 2.989 The stoichiometric ratio of O7 was 5 mmol SrCO3, 2.5 mmol La2O3, 7.4725 mmol Ga2O3 and 0.0275 mmol Cr2O3 were weighed respectively, mixed evenly and put into a crucible. Under a nitrogen (N2) atmosphere, the preparation temperature was 1400°C and sintered for 4 hours to obtain a NIR-II near-infrared fluorescent material.

[0060] Fig.10 This is the XRD spectrum of the fluorescent material prepared in Example 5. It can be seen that its diffraction peak still completely corresponds to the diffraction peak of SrLaGa3O7, and there is no obvious difference from the XRD spectrum of the fluorescent materials prepared in Examples 1, 2, and 3.

[0061] Fig.11 This is the fluorescence emission spectrum of the fluorescent material prepared in Example 5 obtained by 450nm excitation. Compared with the fluorescence emission spectrum of the fluorescent material in Example 3, the peak wavelength and the emission spectrum shape have no obvious changes, but the luminescence intensity is lower than that in Example 3. 3+ With further increase in concentration, the luminescence intensity continued to decrease due to the concentration quenching mechanism. 0.025 Ga 2.975 O7 exhibits the weakest luminescence intensity, and its emission spectrum is almost undetectable. 0.009 Ga 2.991 O7 exhibits the maximum intensity luminescence, and therefore, the value range of x is set to 0.001≤x≤0.025.

[0062] Example 6

[0063] According to the chemical formula SrLaCr 0.009 Ga 2.991 The stoichiometric ratio of O7 was 5 mmol SrCO3, 2.5 mmol La2O3, 7.4775 mmol Ga2O3 and 0.0225 mmol Cr2O3 were weighed respectively, mixed evenly and put into a crucible. Under air atmosphere, the preparation temperature was 1400°C and sintered for 4 hours to obtain NIR-II near-infrared fluorescent material.

[0064] Fig.12 This is the XRD spectrum of the fluorescent material prepared in Example 6. It can be seen that its diffraction peak still completely corresponds to the diffraction peak of SrLaGa3O7, and there is no obvious difference from the XRD spectrum of the fluorescent materials prepared in Examples 1, 2, 3, and 4.

[0065] Fig.13 SrLaCr prepared in Example 6 and Example 3 0.009 Ga 2.991 The fluorescence emission spectra of O7 fluorescent material obtained by excitation at 450 and 610 nm respectively, the excitation wavelength and sintering atmosphere have obvious effects on the peak value, luminous intensity and half-wave peak width of the luminescence band.

[0066] Fig.14 SrLaCr prepared in Example 6 and Example 3 0.009 Ga 2.991 The UV-visible-infrared absorption spectrum of O7 fluorescent material. The absorption spectrum of Example 3 does not contain Cr in the near-infrared wavelength range. 4+ The characteristic absorption peak of Cr further indicates that the luminescence center of the sample prepared under N2 atmosphere is only Cr 3+ The absorption spectrum of Example 6 shows Cr in the near-infrared band. 4+ The characteristic absorption peak of Cr 3+ To Cr 4+ The absorption peaks in the UV-visible band correspond to Cr 4+ The electrons are excited to transition from the ground state to different excited states, and no obvious Cr 3+ The absorption bands caused by the transition of electrons from the ground state to different excited states indicate that Cr 3+ Completely converted to Cr 4+ .

[0067] In addition, we changed the sintering atmosphere from air to oxygen and obtained similar results, which will not be described here.

[0068] Example 7

[0069] According to the chemical formula SrLaCr0.009 Sc 0.03 Ga 2.961 O7 stoichiometric ratio, 5 mmol SrCO3, 2.5 mmol La2O3, 7.4025 mmol Ga2O3, 0.075 mmol Sc2O3 and 0.0225 mmol Cr2O3 were weighed respectively, mixed evenly and put into a crucible, under nitrogen (N2) atmosphere, the preparation temperature was 1400℃, sintered for 4 hours to obtain NIR-II near-infrared fluorescent material.

[0070] Fig.15 This is the XRD spectrum of the fluorescent material prepared in Example 7. It can be seen that its diffraction peak completely corresponds to the diffraction peak of SrLaGa3O7, and there is no obvious difference from the XRD spectrum of the fluorescent material prepared in Example 3.

[0071] Fig.16 The fluorescence emission spectra obtained by 450nm excitation of the fluorescent materials prepared in Example 7 and Example 3. Compared with Example 3, the fluorescence intensity of Example 7 is enhanced, and the peak wavelength is red-shifted to 1208nm.

[0072] Fig.17 The UV-visible absorption spectra of the fluorescent materials prepared in Example 7 and Example 3 are shown in the inset. The curve obtained by converting the absorption-visible spectra using the Tauc's equation is shown in the figure. 0.009 Ga 2.991 O7 and SrLaCr 0.009 Sc 0.03 Ga 2.961 The band gap values ​​of O7 are 4.78 and 4.97 eV respectively. As the band gap increases, the energy difference between the conduction band and the lowest excited energy level becomes wider, resulting in Cr 3+ The ionization probability of Cr is reduced and the 3+ The difficulty of transferring from the lowest excitation energy level to the conduction band leads to a stronger luminescence intensity. In the range of y values ​​(0.001≤y≤0.05), as Sc 3+ With the increase of doping concentration, the band gap value first increases and then decreases; when y=0.03, the band gap value is the largest and the highest luminous intensity is obtained here.

[0073] Example 8

[0074] A near-infrared LED device was constructed by combining a 450nm blue LED chip with the fluorescent material prepared in Example 7. When the LED device was lit under different current driving conditions, it emitted near-infrared light of different intensities.

[0075] It is difficult to observe obvious differences between the Sc-doped and undoped Sc devices from the appearance pictures, and only the experimental results of the device assembled with Sc-doped fluorescent materials are provided here. Fig.18These are photos of the near-infrared LED device taken with an ordinary camera and an infrared camera after it was lit. Fig.19 This is the luminescence spectrum of the near-infrared LED device driven by different currents. The curves correspond to currents of 20-220mA from bottom to top.

Claims

1. A Cr 3+ / Cr 4+ Ion-doped NIR-II fluorescent material, characterized in that The chemical formula of the fluorescent material is SrLaCr x Ga (3-x) O7 or SrLaCr x Sc y Ga (3-x-y) O7, wherein 0.001≤x≤0.025, 0.001≤y≤0.05, and the luminescence center of the fluorescent material is Cr 3+ or Cr 4+ ion.

2. The Cr according to claim 1 3+ / Cr 4+ Ion-doped NIR-II fluorescent material, characterized in that Luminescence center Cr 3+ or Cr 4+ The ions occupy four-coordinated lattice positions in the matrix material, and Cr 3+ / Cr 4+ The raw material of doping ions is Cr2O3.

3. The Cr according to claim 1 3+ / Cr 4+ Ion-doped NIR-II fluorescent material, characterized in that When the sintering atmosphere is nitrogen, argon or other non-oxidizing atmosphere, the luminescent center of the obtained fluorescent material is Cr 3+ When the sintering atmosphere is oxygen, air or other oxidizing atmosphere, the luminescent center of the obtained fluorescent material is Cr 4+ .

4. The Cr according to claim 1 3+ / Cr 4+ Ion-doped NIR-II fluorescent material, characterized in that The fluorescence spectrum wavelength of the fluorescent material is between 900-1700 nm.

5. Cr according to claim 4 3+ / Cr 4+ Ion-doped NIR-II fluorescent material, characterized in that The fluorescent material emits near-infrared light in NIR-II under the excitation of ultraviolet-visible light with a wavelength of 250-650nm.

6. A method for preparing the fluorescent material according to any one of claims 1 to 5, characterized in that: The process comprises the following steps: weighing raw materials SrCO3, La2O3, Ga2O3, Cr2O3 or SrCO3, La2O3, Ga2O3, Cr2O3 according to the stoichiometric ratio; 3、 Sc2O3 are mixed evenly, sintered at 1200-1400°C for 3-5 hours in a reducing or oxidizing atmosphere, and cooled to room temperature to obtain a fluorescent material.

7. The method according to claim 6, characterized in that The process comprises the following steps: weighing raw materials SrCO3, La2O3, Ga2O3 and Cr2O3 according to the stoichiometric ratio, mixing them evenly, sintering them at 1400°C for 4 hours in a nitrogen atmosphere, and cooling them to room temperature to obtain the fluorescent material SrLaCr 0.009 Ga 2.991 O7.

8. The method according to claim 6, characterized in that The process comprises the following steps: weighing raw materials SrCO3, La2O3, Ga2O3 and Cr2O3 according to the stoichiometric ratio, mixing them evenly, sintering them at 1400°C for 4 hours in an air atmosphere, and cooling them to room temperature to obtain the fluorescent material SrLaCr 0.009 Ga 2.991 O7.

9. The method according to claim 6, characterized in that The steps include: weighing the raw materials SrCO3, La2O3, Ga2O3, Cr2O3 according to the stoichiometric ratio; 3、 Sc2O3, mixed evenly, sintered at 1400℃ for 4 hours in a nitrogen atmosphere, and cooled to room temperature to obtain the fluorescent material SrLaCr 0.009 Sc 0.03 Ga 2.961 O7.

10. A Cr according to any one of claims 1 to 5 3+ / Cr 4+ Application of ion-doped NIR-II fluorescent materials, characterized in that, The fluorescent material is applied to near-infrared LED / LD devices.

Citation Information

Cited By

  • Chromium ion single-doped ultra-wideband near-infrared fluorescent material, preparation method thereof and LED device

    CN122060495A