Long-life chip cleaning solution capable of stably etching TiN as well as preparation method and application of long-life chip cleaning solution
By using cyclic compounds such as tetrasulfonic acid phthalocyanine and hydrogen peroxide, alkali and fluorinazole compounds in the TiN chip cleaning solution, the short life of TiN chip cleaning solution is solved and the The problem of unstable etching speed achieves stable etching and complete cleaning effects.
Patent Information
- Application Number
- CN202411075844.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing TiN chip cleaning solution has a short life and an unstable etching speed, especially in the presence of copper ions, which leads to a decrease in the etching speed and the accumulation of titanyl ions leads to a further decrease in the etching speed.
A cyclic compound such as tetrasulfonic acid phthalocyanine is used to combine with hydrogen peroxide and alkali to form a stable complex, inhibiting hydrogen peroxide decomposition and titanyl ion deposition, and promotes the coordination and hydrophilicity of hydroxyl and sulfonic acid groups. The forward reaction of TiN and hydrogen peroxide root increases the etching speed and uses fluorinated indazole compounds as corrosion inhibitors to stabilize the fluorine source.
The stable etching speed of TiN hard mask is achieved, the life of the cleaning solution is extended, and the residue on the surface of the chip can be completely cleaned without ultrasonic treatment, and there is no residue after subsequent rinsing of pure water.
Smart Images

Figure CN119020039A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to chip cleaning liquid technology, in particular to a long-life chip cleaning liquid capable of stably etching TiN, and a preparation method and application thereof. Background Art
[0002] Thanks to the development of the Damascus process, the application of copper metal interconnection in integrated circuits (ICs) has been promoted. Plasma dry etching is usually used in the copper (Cu) / low-k dual-damascene manufacturing process. During the etching process, polymer and particle residues are generated on the sidewalls and bottom. These residues must be removed before the next process step. As the technology node develops towards 45nm and smaller, the reduction in the size of semiconductor devices makes it more difficult to achieve critical profile control of through holes and trenches. IC device companies are studying the use of various hard masks to improve the etching selectivity of low-k materials and thus obtain better profile control.
[0003] Currently, titanium nitride (TiN) is the primary material used for metal hardmasks. However, excessively thick TiN can cause undercutting of the hardmask and complicate subsequent chemical mechanical polishing (CMP). Therefore, partial or complete TiN removal can significantly save resources and simplify the process.
[0004] During the cleaning process, the cleaning solution needs to maintain a stable etching rate over a long period of time, and increasing the TiN etching rate can ensure improved production line efficiency. Hydrogen peroxide can be used as an etchant for TiN, but in the presence of copper ions, hydrogen peroxide decomposes rapidly, shortening the life of the cleaning solution. Furthermore, as TiN is continuously etched, a large amount of titanyl ions accumulate in the cleaning solution. When the titanyl ion concentration reaches saturation, the TiN etching rate decreases. Both of these shortcomings are issues that need to be urgently addressed in existing TiN cleaning solutions. Summary of the Invention
[0005] The present invention aims to address the short lifespan and unstable etching rates of existing hydrogen peroxide chip cleaning solutions by providing a long-life chip cleaning solution that stably etches TiN. This solution effectively inhibits the decomposition of hydrogen peroxide and stably etches titanium nitride hard masks. This solution can stably etch the titanium nitride hard mask even when continuously fed to the chip, while ensuring complete removal of any residues on the chip.
[0006] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising", etc. and similar meanings, as well as closed-ended "composed of", "composed of", etc. and similar meanings.
[0007] To achieve the above object, the technical solution adopted by the present invention is: a long-life chip cleaning solution for stable TiN etching, comprising the following components in the following weight proportions:
[0008]
[0009] Furthermore, the cyclic compound is one or more of tetrasulfonic acid phthalocyanine, 5,28-dihydro-29H,31H-phthalocyanine, diaza-18-crown-6 and 1-aza-18-crown-6-ether.
[0010] Furthermore, the cyclic compound is preferably tetrasulfonic acid phthalocyanine.
[0011] Furthermore, the cyclic compound is 0.3-0.6 parts.
[0012] TiN reacts with hydrogen peroxide to generate tetravalent titanium ions, Ti 4+ In aqueous solution, it is titanium ion (TiO 2+ ) exists in the form of. As TiN is continuously etched, the titanium ion (TiO 2+ ) are continuously accumulated, when the titanium ion (TiO 2 + When the concentration of ) is about to reach saturation, the reaction becomes difficult to proceed in the forward direction, which leads to a decrease in the etching rate. The reaction principle is as follows.
[0013]
[0014] The cyclic compound used in the present invention can self-assemble with titanium ion like a spider web to form a stable complex. The consumption of titanium ion promotes the positive reaction between TiN and hydrogen peroxide, thereby ensuring a stable etching speed of TiN.
[0015] When tetrasulfonic acid phthalocyanine is used as the cyclic compound, it not only contains both sulfonic acid and hydroxyl groups that can coordinate with metal ions, helping to inhibit the self-decomposition of hydrogen peroxide under the catalytic action of metal ions, but phthalocyanine is also a completely symmetrical macrocyclic compound that can stably chelate titanium acyl ions in the middle, forming a stable titanium compound and promoting the forward reaction between TiN and hydrogen peroxide, thereby increasing the etching speed. At the same time, the hydroxyl and sulfonic acid groups have a certain degree of hydrophilicity, which can dissolve the formed titanium compound in water and facilitate rinsing.
[0016] Furthermore, the amount of hydrogen peroxide is 15-20 parts.
[0017] Furthermore, the mass ratio of the cyclic compound to hydrogen peroxide is 1:15-55.
[0018] Furthermore, the mass ratio of the cyclic compound to hydrogen peroxide is preferably 1:36.
[0019] Furthermore, the base is one or more of isobutanolamine, diethanolamine, monoethanolamine, diglycolamine, isopropanolamine and N-methylethanolamine.
[0020] Furthermore, the base is preferably diethanolamine and / or isobutanolamine.
[0021] Furthermore, the base is most preferably isobutanolamine.
[0022] Furthermore, the base is 10-15 parts.
[0023] Furthermore, the corrosion inhibitor is one or more of 4,5,6,7-tetrafluoro-1H-indazole, 5-trifluoromethyl-1H-indazole, 4,6-difluoro-1H-indazole and 4-fluoro-1H-indazole.
[0024] Furthermore, the corrosion inhibitor is preferably 4,5,6,7-tetrafluoro-1H-indazole.
[0025] Furthermore, the corrosion inhibitor is 0.2-0.4 parts.
[0026] Furthermore, the ultrapure water is 60-75 parts.
[0027] Another object of the present invention is to disclose a method for preparing a long-life chip cleaning solution for stably etching TiN, comprising the following steps:
[0028] The components are mixed and stirred until all the components are completely dissolved, thereby obtaining the cleaning solution with a stable etching rate and a long service life.
[0029] Another object of the present invention is to disclose the application of a long-life chip cleaning solution capable of stably etching TiN in the field of chip cleaning.
[0030] Furthermore, the chip is cleaned using a long-life chip cleaning solution that stably etches TiN, comprising the following steps:
[0031] Step 1: Immerse the chip in a heated long-life chip cleaning solution that stably etches TiN to obtain a cleaned chip;
[0032] Step 2: Rinse the cleaned chip with ultrapure water to complete the chip cleaning process.
[0033] Furthermore, the heating temperature is 30-50°C.
[0034] Furthermore, the soaking time is 5-30 minutes.
[0035] Furthermore, the ultrapure water is deionized water with a resistance of at least 18 MΩ.
[0036] Furthermore, the ultrapure water rinsing time is 1-5 minutes.
[0037] The long-life chip cleaning solution for stable TiN etching of the present invention, its preparation method and application have the following advantages compared with the prior art:
[0038] 1) TiN reacts with hydrogen peroxide to generate tetravalent titanium ions, Ti 4+ In aqueous solution, it is titanium ion (TiO 2+ ) exists in the form of. As TiN is continuously etched, titanium ions in the cleaning solution are continuously accumulated. When the concentration of titanium ions is about to reach saturation, it is difficult for the reaction to proceed in the forward direction, which leads to a decrease in the etching rate. The cyclic compound used in the present invention can self-assemble with titanium ions to form a stable complex like a spider web. The consumption of titanium ions promotes the forward reaction of TiN and hydrogen peroxide, thereby ensuring a stable etching rate of TiN. In particular, when tetrasulfonic acid phthalocyanine is selected as the cyclic compound, it not only contains sulfonic acid groups and hydroxyl groups that can coordinate with metal ions and help inhibit the self-decomposition of hydrogen peroxide under the catalytic action of metal ions, but phthalocyanine is also a completely symmetrical macrocyclic compound that can stably chelate titanium ions in the middle to form a stable titanium compound, which promotes the forward reaction process of TiN and hydrogen peroxide, thus improving the etching rate. At the same time, the hydroxyl group and sulfonic acid group have a certain hydrophilicity, which can dissolve the formed titanium compound in water and is easy to rinse.
[0039] 2) The long-life chip cleaning solution for stably etching TiN of the present invention uses fluorine-containing indazole compounds as corrosion inhibitors, which can stably replenish the fluorine source, achieve cleaning residues, and also chelate metal ions.
[0040] 3) The long-life chip cleaning solution for stable TiN etching of the present invention has no special requirements for the chip corrosion-free cleaning process and does not require ultrasonic treatment. It can completely wash away the pollutants and various particles adhered to the chip only under the immersion process, and only needs to be rinsed with pure water afterwards, and no dirt remains after washing.
[0041] In summary, the long-life chip cleaning solution for stably etching TiN of the present invention has very good application prospects and large-scale industrial promotion potential in the field of semiconductor chip cleaning. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is the SEM effect of a chip with a large amount of residue before cleaning; the magnification is 200,000 times.
[0043] Figure 2 This is a SEM image of the cleaning effect after the long-life chip cleaning solution provided in Example 1 is continuously added to 60 chips; the magnification is 200,000 times. DETAILED DESCRIPTION
[0044] The present invention will be further described below with reference to the following examples. The following description of the technical features is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:
[0045] Unless otherwise stated, the units used in this specification are international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0046] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints A and B.
[0047] In this specification, the numerical range expressed using "above" or "below" means a numerical range including the number.
[0048] In this specification, the use of "may" includes both the meaning of performing a certain process and the meaning of not performing a certain process.
[0049] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.
[0050] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 15-25°C.
[0051] In this manual, the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0052] Examples 1-6
[0053] Examples 1-6 provide a variety of long-life chip cleaning solutions for stable TiN etching, the components and weight ratios of which are shown in Table 1. The preparation method thereof comprises the following steps:
[0054] Step 1: Weigh each component in its respective amount;
[0055] Step 2: Add the above materials into a container and stir until all the materials are completely dissolved, thereby obtaining the cleaning solution with a stable etching rate and a long service life.
[0056] Table 1 Components and weight ratios included in Examples 1-6
[0057]
[0058]
[0059] Comparative Examples 1-3
[0060] Comparative Examples 1-3 provide a variety of chip cleaning solutions, the components and weight ratios of which are shown in Table 2. The preparation methods are the same as those in Example 1.
[0061] Table 2 Components and weight ratios included in Comparative Examples 1-3
[0062]
[0063] The various properties of the above embodiments or comparative examples are tested below, and the specific test results are shown in Table 3:
[0064] Table 3 Test data
[0065]
[0066]
[0067] Based on Table 3, it can be seen that compared with the initial TiN etching rate, the etching rate of the chip of Examples 1-6, a variety of long-life chip cleaning solutions for stable TiN etching, is reduced relatively slowly or hardly at all. Since hydrogen peroxide is easily decomposed by heat when heated continuously, for the same heating time, the hydrogen peroxide in the long-life chip cleaning solutions for stable TiN etching in Examples 1-6 is less decomposed, and the long-life chip cleaning solutions for stable TiN etching in Examples 1-6 have a long life. However, in Comparative Example 1, since tetrasulfonic acid phthalocyanine is not added, a large amount of hydrogen peroxide is decomposed, which shortens the life of the cleaning solution, and when the chip is continuously put into use, the TiN etching rate is only Comparative Example 2 uses β-cyclodextrin as the cyclic compound. Although it can ensure the cleaning effect, it cannot inhibit the decomposition of hydrogen peroxide. When the chip is continuously put into the etchant, the etching rate is only In Comparative Example 3, since no fluorine-containing corrosion inhibitor is added, the polymer cannot be stripped off from the sidewall or bottom, and the cleaning effect cannot be achieved. When the chips are continuously added, the etching rate of TiN is also reduced to a certain extent.
[0068] Figure 1 This is the SEM effect of a chip with a large amount of residue before cleaning; the magnification is 200,000 times. Figure 2 This is the SEM image of the cleaning effect after the long-life chip cleaning solution provided in Example 1 was continuously added to 60 chips; the magnification is 200,000 times. Figure 1 and Figure 2 It can be seen that the long-life chip cleaning solution prepared in Example 1 of the present invention leaves no residue on the chip surface after cleaning, and has a good cleaning effect.
[0069] in:
[0070] The test method for performance 1 cleaning effect is:
[0071] After dry etching, a large amount of residue remains on the sidewalls and bottom of the trench of a chip with silicon as the substrate. The chip is cleaned using the cleaning solutions of the above embodiments and comparative examples of the present invention. The cleaning method includes the following steps:
[0072] Step 1: Take 30 mL of the prepared cleaning solution and heat it in a water bath to 30°C. Place a chip in the cleaning solution heated in the water bath and soak for 10 minutes. Then add a new chip. Repeat the above steps until 60 chips are added continuously.
[0073] Step 2: Rinse the cleaned chip with ultrapure water for 2 minutes to complete the chip cleaning process. Use SEM to observe the cleaning effect after continuously adding 60 chips. The test results are shown in Figure 1-2 and Table 3.
[0074] Performance 2 The test method for titanium nitride etching rate is:
[0075] The four-point probe method was used to test the etching rate of titanium nitride with different cleaning solutions. 2 The titanium nitride sheet was placed in a cleaning solution at 30°C for 10 minutes, then rinsed twice in ultrapure water and dried. The thickness of the titanium nitride before and after immersion was then measured using the four-probe method, and the initial titanium nitride etching rate was calculated.
[0076] After 12 hours, add 2×2cm 2 Repeat the above operation and calculate the input of 60 pieces of 2×2cm titanium nitride 2 The etching rate of the titanium nitride sheet is shown in Table 3.
[0077] The ultrapure water used in the steps is all deionized water with a resistance of at least 18 MΩ.
[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A long-life chip cleaning solution for stable etching of TiN, characterized in that: The composition includes the following components in weight ratio:
2. The long-life chip cleaning solution for stable TiN etching according to claim 1, characterized in that: The cyclic compound is one or more of tetrasulfonate phthalocyanine, 5,28-dihydro-29H,31H-phthalocyanine, diaza-18-crown-6 and 1-aza-18-crown-6-ether.
3. The long-life chip cleaning solution for stable TiN etching according to claim 1, characterized in that: The mass ratio of the cyclic compound to hydrogen peroxide is 1:15-55.
4. The long-life chip cleaning solution for stable TiN etching according to claim 1, characterized in that: The base is one or more of isobutanolamine, diethanolamine, monoethanolamine, diglycolamine, isopropanolamine and N-methylethanolamine.
5. The long-life chip cleaning solution for stable TiN etching according to claim 1, characterized in that: The corrosion inhibitor is one or more of 4,5,6,7-tetrafluoro-1H-indazole, 5-trifluoromethyl-1H-indazole, 4,6-difluoro-1H-indazole and 4-fluoro-1H-indazole.
6. A method for preparing a long-life chip cleaning solution for stable etching of TiN according to any one of claims 1 to 5, characterized in that: The following steps are involved: The components are mixed and stirred until all the components are completely dissolved, thereby obtaining the cleaning solution with a stable etching speed and a long service life.
7. Use of the long-life chip cleaning solution for stably etching TiN as claimed in any one of claims 1 to 5 in the field of chip cleaning.
8. The use according to claim 7, characterized in that: The chip is cleaned using a long-life chip cleaning solution that stably etches TiN, including the following steps: Step 1: Immerse the chip in a heated long-life chip cleaning solution that stably etches TiN to obtain a cleaned chip; Step 2: Rinse the cleaned chip with ultrapure water to complete the chip cleaning process.
9. The use according to claim 8, characterized in that: The heating temperature is 30-50° C.; and / or the soaking time is 5-30 min.
10. The use according to claim 8, characterized in that: The ultrapure water rinsing time is 1-5 minutes.
Citation Information
Patent Citations
Grinding fluid for metal and grinding method
CN101058712A
Method for removing pollution impurities on surface of silicon wafer
CN111554564A
Plasma etching residue cleaning solution
CN113130292A
Semiconductor titanium nitride cleaning solution as well as preparation method and application thereof
CN117925335A
Titanium nitride etching solution, preparation method and application thereof, and cleaning method
CN118048155A