Formula process for prolonging maintenance period of wind power lubricating grease

By optimizing the formulation process and combining specific process steps and ingredients, wind power greases with excellent performance are formed, which solves the problems of short maintenance cycles and frequent maintenance of traditional greases, extends service life, and improves equipment reliability and economic benefits.

CN119020083AInactive Publication Date: 2024-11-26SHENYANG JINCHANGDA GREASE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411126801.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional wind power greases are difficult to meet the harsh conditions of the wind power generation environment, resulting in short maintenance cycles and frequent maintenance, increasing maintenance costs and downtime, affecting the economic benefits of wind power generation.

Method used

Adopted the optimized formula process, including 150BS base oil, 500N base oil, dodecyl stearic acid, sebacic acid, lithium hydroxide, dianiline, T706 antirust agent, T202 antioxidant anti-corrosion agent, T361A antiwear agent, T614 Components such as tackifier, polyisobutylene PB2400 and fluorine oil are formed through specific process steps and temperature control to form wind power greases with excellent wear resistance, corrosion resistance, aging resistance and high and low temperature resistance.

Benefits of technology

It significantly extends the service life of grease, improves the operating reliability of wind power equipment, reduces maintenance costs and environmental pollution risks, improves the economic benefits of wind farms, and simplifies the operation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020083A_ABST
    Figure CN119020083A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lubricating grease preparation, in particular to a formula process for prolonging the maintenance period of wind power lubricating grease. The formula comprises the following raw materials: 150BS base oil, 500N base oil, 12-hydroxystearic acid, sebacic acid, lithium hydroxide, diphenylamine, oil soluble blue, a T706 antirust agent, a T202 oxidation and corrosion inhibitor, a T361A anti-wear agent, a T614 tackifier, polyisobutene PB2400 and fluorine oil. The process comprises the steps of weighing and feeding, heating and saponifying, compounding and refining, cooling and transferring, adjusting and homogenizing, agent adding and post-treatment, degassing and filling. According to the formula process for prolonging the maintenance period of the wind power lubricating grease, the maintenance period of the wind power lubricating grease can be effectively prolonged, the maintenance frequency is reduced, the maintenance cost is reduced, and the economic benefit of wind power generation is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grease preparation, and in particular to a formulation process for increasing the maintenance cycle of wind power grease. Background Art

[0002] In modern wind power generation technology, the reliability and maintenance cost of wind turbines are important factors affecting their economic benefits. The gearbox of a wind turbine is one of the most critical components in the entire system, and its lubrication condition is directly related to the operating efficiency and life of the entire unit. Due to the particularity of the wind power generation environment, such as large temperature changes, high humidity, wind and sand erosion, etc., higher requirements are placed on the performance of grease. Traditional greases are often difficult to meet these harsh conditions, resulting in short maintenance cycles and frequent replacement, increased maintenance costs and downtime, and thus affecting the overall economic benefits of wind power generation.

[0003] In order to solve this problem, in recent years, researchers have been committed to developing new wind power grease formulas to extend its maintenance cycle and reduce the number of maintenance times. In many studies, optimizing the ratio of base oil and additives to improve the grease's anti-wear, anti-corrosion, anti-aging and high and low temperature resistance has become the main way to improve the performance of wind power grease.

[0004] There are some grease products for wind power equipment on the market, but these products still have many shortcomings in practical applications. For example, although some greases have good low-temperature performance, they are easy to soften in high-temperature environments, resulting in reduced lubrication effect; other products have good anti-wear performance, but they perform poorly in terms of corrosion resistance and anti-aging. In addition, due to the special working environment of wind power equipment, higher requirements are also placed on the water resistance and anti-pollution ability of grease. Summary of the invention

[0005] The formulation process for increasing the maintenance period of wind power grease provided by the present invention can effectively extend the maintenance period of wind power grease, reduce the maintenance times, reduce the maintenance costs, and improve the economic benefits of wind power generation.

[0006] The technical solution adopted by the present invention is: a formulation process for increasing the maintenance cycle of wind power grease, wherein the formula raw materials include, by weight: 1560 parts of 150BS base oil, 1950 parts of 500N base oil, 390 parts of dodecyl stearic acid, 119 parts of sebacic acid, 109 parts of lithium hydroxide, 20 parts of diphenylamine, 0.85 parts of oil-soluble blue, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and corrosion inhibitor, 120 parts of T361A antiwear agent, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil.

[0007] As a further improvement of the present invention, the purity of the lithium hydroxide is 57%.

[0008] As a further improvement of the present invention, the process comprises the following steps:

[0009] Step 1, weighing and feeding: first weigh the raw materials according to the above weight parts, mix 109 parts of lithium hydroxide and 550 parts of water evenly to form 659 parts of lithium hydroxide aqueous solution, then put the weighed 1800 parts of 500N base oil into the saponification kettle, and then add 390 parts of dodecyl hydroxystearic acid and 119 parts of sebacic acid in sequence;

[0010] Step 2, heating and saponification: start the heating system of the hot coal furnace, control the temperature in the saponification kettle to rise to 90-100°C, wait for the dodecyl hydroxystearic acid to melt, drop 263.6 parts of lithium hydroxide aqueous solution into the saponification kettle, control the dropping time to 45-60 minutes, and then allow the material to undergo saponification reaction in the saponification kettle;

[0011] Step 3, compounding and refining: after the saponification reaction is completed, the temperature in the saponification kettle is controlled to rise to 100-105°C, and the remaining 395.4 parts of lithium hydroxide aqueous solution are added dropwise, and the dropping time is controlled to be 90-120 minutes, and then the temperature in the saponification kettle is controlled to rise to 148-152°C, 260 parts of 150BS base oil and 150 parts of 500N base oil are added and stirred, and then the temperature in the saponification kettle is controlled to rise to 207-209°C, and maintained at this temperature for 3-5 minutes;

[0012] Step 4, cooling and transfer: add 700 parts of 150BS base oil to the saponification kettle and stir. After the temperature of the saponification kettle drops to 180-195°C, keep it at this temperature for 30 minutes and continue stirring. Then filter it through a 120-mesh filter and transfer it to the refining kettle;

[0013] Step 5, adjustment and homogenization: add 300 parts of 150BS base oil to the refining kettle and stir, reduce the temperature in the refining kettle to 150-160°C, start the double pumps, use 80-mesh and 100-mesh filters for 45 minutes each, reduce the temperature in the refining kettle to 120-125°C, pour the mixture into the blending kettle, add 300 parts of 150BS base oil and mix evenly, then perform homogenization, and after the homogenization is completed, use a 100-mesh filter for cyclic filtration;

[0014] Step 6, dosing and post-treatment: After the temperature in the blending kettle is reduced to 100°C, 0.85 parts of oil-soluble blue are added, and the mixture is refluxed and stirred for 30 minutes. After the temperature in the blending kettle is reduced to 85°C, 20 parts of diphenylamine, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and anticorrosion agent, and 120 parts of T361A antiwear agent are added in sequence. After continuous stirring for 20 minutes, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil are added, and the mixture is refluxed and stirred for 30-45 minutes.

[0015] Step seven, degassing and filling: after the temperature in the blending kettle is reduced to 65-75°C, the mixture is transported into the degassing kettle through the pump body, and the vacuum degree of the degassing kettle is controlled to 0.09MPa. The negative pressure is maintained for 10 minutes. After the negative pressure ends, open the vent valve to eliminate the negative pressure, and finally fill it to obtain the finished grease.

[0016] As a further improvement of the present invention, in step 2, the heating system of the hot coal furnace adopts indirect heating to provide a uniform and stable heat source for the saponification kettle; during the saponification reaction, the stirring speed in the saponification kettle is controlled at 100-150 rpm to ensure that the materials are fully mixed and fully contacted.

[0017] As a further improvement of the present invention, in step three and step four, the stirring speed in the saponification kettle is controlled at 150-200 rpm to ensure that the materials are fully mixed and uniform.

[0018] As a further improvement of the present invention, in the step five, the stirring speed in the refining kettle is controlled at 200-250 rpm, the pressure of the homogenization treatment in the blending kettle is controlled at 20-22 MPa, and the homogenization treatment time is 30 minutes to ensure the homogeneity and stability of the mixture.

[0019] As a further improvement of the present invention, in step six, the stirring speed in the blending kettle is controlled at 200-250 rpm to ensure that each additive is fully mixed with the mixture.

[0020] As a further improvement of the present invention, in step seven, the delivery pressure of the pump body is ≤0.7 MPa to ensure that the mixture will not be affected by excessive shear force during the delivery process, thereby maintaining its structural stability.

[0021] The beneficial effects of the formula process for increasing the maintenance cycle of wind power grease provided by the present invention are mainly reflected in the following aspects:

[0022] (1) Significantly extend the service life of grease: By optimizing the formula and process, the present invention enables wind power grease to maintain stable performance in harsh working environments, thereby effectively extending its maintenance cycle, reducing replacement frequency, and lowering maintenance costs.

[0023] (2) Improving the operational reliability of wind power equipment: The grease of the present invention has excellent anti-wear, anti-corrosion, anti-aging and high and low temperature resistance, which can ensure the stable operation of wind power equipment under various extreme conditions and reduce equipment failures and downtime caused by lubrication problems.

[0024] (3) Reducing the risk of environmental pollution: Environmentally friendly additives such as polyisobutylene PB2400 and fluorinated oil are added to the grease formula of the present invention. These ingredients can improve the water resistance and pollution resistance of the grease and reduce the impact of the grease on the environment during use.

[0025] (4) Improving economic benefits: The present invention reduces the number of maintenance times and reduces maintenance costs, so that wind power grease can bring significant economic benefits to wind farm operators. At the same time, extending the service life of the grease also means reducing resource consumption, which is in line with the concept of sustainable development.

[0026] (5) Simplified operation process: The process flow of the present invention is reasonably designed, simple to operate, and easy to implement on the production site. By precisely controlling the temperature, stirring speed and time of each step, the quality stability and consistency of the grease are ensured. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The invention is a process flow chart of a formulation process for increasing the maintenance cycle of wind power grease. DETAILED DESCRIPTION

[0028] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0029] The invention provides a formulation process for increasing the maintenance cycle of wind power grease. The raw materials of the formulation include, by weight: 1560 parts of 150BS base oil, 1950 parts of 500N base oil, 390 parts of dodecyl hydroxystearic acid, 119 parts of sebacic acid, 109 parts of lithium hydroxide, 20 parts of diphenylamine, 0.85 parts of oil-soluble blue, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and corrosion inhibitor, 120 parts of T361A antiwear agent, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil.

[0030] In the present invention, the purity of lithium hydroxide is 57%.

[0031] In the present invention, the process comprises the following steps:

[0032] Step 1, weighing and feeding: first weigh the raw materials according to the above weight parts, mix 109 parts of lithium hydroxide and 550 parts of water evenly to form 659 parts of lithium hydroxide aqueous solution, then put the weighed 1800 parts of 500N base oil into the saponification kettle, and then add 390 parts of dodecyl hydroxystearic acid and 119 parts of sebacic acid in sequence;

[0033] Step 2, heating and saponification: start the heating system of the hot coal furnace, control the temperature in the saponification kettle to rise to 90-100°C, wait for the dodecyl hydroxystearic acid to melt, drop 263.6 parts of lithium hydroxide aqueous solution into the saponification kettle, control the dropping time to 45-60 minutes, and then allow the material to undergo saponification reaction in the saponification kettle;

[0034] Step 3, compounding and refining: after the saponification reaction is completed, the temperature in the saponification kettle is controlled to rise to 100-105°C, and the remaining 395.4 parts of lithium hydroxide aqueous solution are added dropwise, and the dropping time is controlled to be 90-120 minutes, and then the temperature in the saponification kettle is controlled to rise to 148-152°C, 260 parts of 150BS base oil and 150 parts of 500N base oil are added and stirred, and then the temperature in the saponification kettle is controlled to rise to 207-209°C, and maintained at this temperature for 3-5 minutes;

[0035] Step 4, cooling and transfer: add 700 parts of 150BS base oil to the saponification kettle and stir. After the temperature of the saponification kettle drops to 180-195°C, keep it at this temperature for 30 minutes and continue stirring. Then filter it through a 120-mesh filter and transfer it to the refining kettle;

[0036] Step 5, adjustment and homogenization: add 300 parts of 150BS base oil to the refining kettle and stir, reduce the temperature in the refining kettle to 150-160°C, start the double pumps, use 80-mesh and 100-mesh filters for 45 minutes each, reduce the temperature in the refining kettle to 120-125°C, pour the mixture into the blending kettle, add 300 parts of 150BS base oil and mix evenly, then perform homogenization, and after the homogenization is completed, use a 100-mesh filter for cyclic filtration;

[0037] Step 6, dosing and post-treatment: After the temperature in the blending kettle is reduced to 100°C, 0.85 parts of oil-soluble blue are added, and the mixture is refluxed and stirred for 30 minutes. After the temperature in the blending kettle is reduced to 85°C, 20 parts of diphenylamine, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and anticorrosion agent, and 120 parts of T361A antiwear agent are added in sequence. After continuous stirring for 20 minutes, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil are added, and the mixture is refluxed and stirred for 30-45 minutes.

[0038] Step seven, degassing and filling: after the temperature in the blending kettle is reduced to 65-75°C, the mixture is transported into the degassing kettle through the pump body, and the vacuum degree of the degassing kettle is controlled to 0.09MPa. The negative pressure is maintained for 10 minutes. After the negative pressure ends, open the vent valve to eliminate the negative pressure, and finally fill it to obtain the finished grease.

[0039] In step 2 of the present invention, the heating system of the hot coal furnace adopts an indirect heating method to provide a uniform and stable heat source for the saponification kettle; during the saponification reaction, the stirring speed in the saponification kettle is controlled at 100-150 rpm to ensure that the materials are fully mixed and fully contacted.

[0040] In step 3 and step 4 of the present invention, the stirring speed in the saponification kettle is controlled at 150-200 rpm to ensure that the materials are fully mixed and uniform.

[0041] In step five of the present invention, the stirring speed in the refining kettle is controlled at 200-250 rpm, the pressure of the homogenization treatment in the blending kettle is controlled at 20-22 MPa, and the homogenization treatment time is 30 minutes to ensure the homogeneity and stability of the mixture.

[0042] In step six of the present invention, the stirring speed in the blending kettle is controlled at 200-250 rpm to ensure that each additive is fully mixed with the mixture.

[0043] In step seven of the present invention, the delivery pressure of the pump body is ≤0.7 MPa to ensure that the mixture will not be affected by excessive shear force during the delivery process, thereby maintaining its structural stability.

[0044] Embodiment 1:

[0045] This embodiment provides a formulation process for increasing the maintenance cycle of wind power grease, as follows.

[0046] (i) Weighing and feeding: First, weigh 1560 parts of 150BS base oil, 1950 parts of 500N base oil, 390 parts of dodecyl hydroxystearic acid, 119 parts of sebacic acid, 109 parts of lithium hydroxide, 20 parts of diphenylamine, 0.85 parts of oil-soluble blue, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and corrosion inhibitor, 120 parts of T361A antiwear agent, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil according to weight parts, mix 109 parts of lithium hydroxide and 550 parts of water to form 659 parts of lithium hydroxide aqueous solution, then put the weighed 1800 parts of 500N base oil into a saponification kettle, and then add 390 parts of dodecyl hydroxystearic acid and 119 parts of sebacic acid in sequence;

[0047] (ii) Heating and saponification: Start the heating system of the hot coal furnace, control the temperature in the saponification kettle to rise to 96° C., wait for the dodecyl hydroxystearic acid to melt, drop 263.6 parts of lithium hydroxide aqueous solution into the saponification kettle, control the dropping time to be 50 minutes, and then allow the material to undergo saponification reaction in the saponification kettle, wherein during the saponification reaction, the stirring speed in the saponification kettle is controlled at 120 rpm;

[0048] (III) Compounding and refining: After the saponification reaction is completed, the temperature in the saponification kettle is controlled to rise to 102°C, and the remaining 395.4 parts of lithium hydroxide aqueous solution are added dropwise, and the dropping time is controlled to be 105 minutes. Then, the temperature in the saponification kettle is controlled to rise to 150°C, and 260 parts of 150BS base oil and 150 parts of 500N base oil are added and stirred, wherein the stirring speed in the saponification kettle is controlled at 180 rpm, and then the temperature in the saponification kettle is controlled to rise to 208°C and maintained at this temperature for 4 minutes;

[0049] (iv) Cooling and transfer: add 700 parts of 150BS base oil into the saponification kettle and stir. After the temperature of the saponification kettle drops to 188°C, keep it at this temperature for 30 minutes and continue stirring. The stirring speed in the saponification kettle is controlled at 180 rpm. Then filter it through a 120-mesh filter and transfer it to the refining kettle.

[0050] (V) Adjustment and homogenization: Add 300 parts of 150BS base oil to the refining kettle and stir, wherein the stirring speed in the refining kettle is controlled at 230 rpm, after the temperature in the refining kettle is reduced to 155°C, start the double pumps, and use 80-mesh and 100-mesh filter screens for 45 minutes each, and then reduce the temperature in the refining kettle to 122°C, then pour the mixture into the blending kettle, add 300 parts of 150BS base oil and mix evenly, and then perform homogenization treatment, the pressure of the homogenization treatment is controlled at 21MPa, the homogenization treatment time is 30 minutes, and after the homogenization treatment is completed, use a 100-mesh filter screen for cyclic filtration;

[0051] (VI) Additives and post-treatment: After the temperature in the blending kettle is lowered to 100°C, 0.85 parts of oil-soluble blue are added, and the mixture is refluxed and stirred for 30 minutes. After the temperature in the blending kettle is lowered to 85°C, 20 parts of diphenylamine, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and anticorrosion agent, and 120 parts of T361A antiwear agent are added in sequence. After continuous stirring for 20 minutes, the stirring speed in the blending kettle is controlled at 230 rpm, and 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil are added, and the mixture is refluxed and stirred for 38 minutes.

[0052] (VII) Degassing and filling: After the temperature in the blending kettle is reduced to 70°C, the mixture is transported into the degassing kettle through a pump body with a delivery pressure of 0.7MPa. The vacuum degree of the degassing kettle is controlled to 0.09MPa, and the negative pressure is maintained for 10 minutes. After the negative pressure ends, open the vent valve to eliminate the negative pressure, and finally fill it to obtain the finished grease.

[0053] Embodiment 2:

[0054] This embodiment provides a formulation process for increasing the maintenance cycle of wind power grease, as follows.

[0055] (i) Weighing and feeding: First, weigh 1560 parts of 150BS base oil, 1950 parts of 500N base oil, 390 parts of dodecyl hydroxystearic acid, 119 parts of sebacic acid, 109 parts of lithium hydroxide, 20 parts of diphenylamine, 0.85 parts of oil-soluble blue, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and corrosion inhibitor, 120 parts of T361A antiwear agent, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil according to weight parts, mix 109 parts of lithium hydroxide and 550 parts of water to form 659 parts of lithium hydroxide aqueous solution, then put the weighed 1800 parts of 500N base oil into a saponification kettle, and then add 390 parts of dodecyl hydroxystearic acid and 119 parts of sebacic acid in sequence;

[0056] (ii) Heating and saponification: Start the heating system of the hot coal furnace, control the temperature in the saponification kettle to rise to 96° C., wait for the dodecyl hydroxystearic acid to melt, drop 263.6 parts of lithium hydroxide aqueous solution into the saponification kettle, control the dropping time to be 50 minutes, and then allow the material to undergo saponification reaction in the saponification kettle, wherein during the saponification reaction, the stirring speed in the saponification kettle is controlled at 110 rpm;

[0057] (III) Compounding and refining: After the saponification reaction is completed, the temperature in the saponification kettle is controlled to rise to 102°C, and the remaining 395.4 parts of lithium hydroxide aqueous solution are added dropwise, and the dropping time is controlled to be 105 minutes. Then, the temperature in the saponification kettle is controlled to rise to 150°C, and 260 parts of 150BS base oil and 150 parts of 500N base oil are added and stirred, wherein the stirring speed in the saponification kettle is controlled at 160 rpm, and then the temperature in the saponification kettle is controlled to rise to 208°C and maintained at this temperature for 4 minutes;

[0058] (iv) Cooling and transfer: add 700 parts of 150BS base oil into the saponification kettle and stir. After the temperature of the saponification kettle drops to 188°C, keep it at this temperature for 30 minutes and continue stirring. The stirring speed in the saponification kettle is controlled at 152 rpm. Then, filter it through a 120-mesh filter and transfer it to the refining kettle.

[0059] (V) Adjustment and homogenization: Add 300 parts of 150BS base oil to the refining kettle and stir, wherein the stirring speed in the refining kettle is controlled at 210 rpm, after the temperature in the refining kettle is reduced to 155°C, start the double pumps, use 80-mesh and 100-mesh filter screens for 45 minutes each, and then reduce the temperature in the refining kettle to 122°C, then pour the mixture into the blending kettle, add 300 parts of 150BS base oil and mix evenly, and then perform homogenization treatment, the pressure of the homogenization treatment is controlled at 20MPa, the homogenization treatment time is 30 minutes, and after the homogenization treatment is completed, use a 100-mesh filter screen for cyclic filtration;

[0060] (VI) Additives and post-treatment: After the temperature in the blending kettle is lowered to 100°C, 0.85 parts of oil-soluble blue are added, and the mixture is refluxed and stirred for 30 minutes. After the temperature in the blending kettle is lowered to 85°C, 20 parts of diphenylamine, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and anticorrosion agent, and 120 parts of T361A antiwear agent are added in sequence. After continuous stirring for 20 minutes, the stirring speed in the blending kettle is controlled at 210 rpm, and 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil are added, and the mixture is refluxed and stirred for 38 minutes.

[0061] (VII) Degassing and filling: After the temperature in the blending kettle is reduced to 70°C, the mixture is transported into the degassing kettle through a pump body with a delivery pressure of 0.65MPa. The vacuum degree of the degassing kettle is controlled to 0.09MPa, and the negative pressure is maintained for 10 minutes. After the negative pressure ends, open the vent valve to eliminate the negative pressure, and finally fill it to obtain the finished grease.

[0062] Embodiment 3:

[0063] This embodiment provides a formulation process for increasing the maintenance cycle of wind power grease, as follows.

[0064] (i) Weighing and feeding: First, weigh 1560 parts of 150BS base oil, 1950 parts of 500N base oil, 390 parts of dodecyl hydroxystearic acid, 119 parts of sebacic acid, 109 parts of lithium hydroxide, 20 parts of diphenylamine, 0.85 parts of oil-soluble blue, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and corrosion inhibitor, 120 parts of T361A antiwear agent, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil according to weight parts, mix 109 parts of lithium hydroxide and 550 parts of water to form 659 parts of lithium hydroxide aqueous solution, then put the weighed 1800 parts of 500N base oil into a saponification kettle, and then add 390 parts of dodecyl hydroxystearic acid and 119 parts of sebacic acid in sequence;

[0065] (ii) Heating and saponification: Start the heating system of the hot coal furnace, control the temperature in the saponification kettle to rise to 96° C., wait for the dodecyl hydroxystearic acid to melt, drop 263.6 parts of lithium hydroxide aqueous solution into the saponification kettle, control the dropping time to be 50 minutes, and then allow the material to undergo saponification reaction in the saponification kettle, wherein during the saponification reaction, the stirring speed in the saponification kettle is controlled at 140 rpm;

[0066] (III) Compounding and refining: After the saponification reaction is completed, the temperature in the saponification kettle is controlled to rise to 102° C., and the remaining 395.4 parts of lithium hydroxide aqueous solution are added dropwise, and the dropping time is controlled to be 105 minutes. Then, the temperature in the saponification kettle is controlled to rise to 150° C., 260 parts of 150BS base oil and 150 parts of 500N base oil are added and stirred, wherein the stirring speed in the saponification kettle is controlled at 192 rpm, and then the temperature in the saponification kettle is controlled to rise to 208° C. and maintained at this temperature for 4 minutes;

[0067] (iv) Cooling and transfer: add 700 parts of 150BS base oil into the saponification kettle and stir. After the temperature of the saponification kettle drops to 188°C, keep it at this temperature for 30 minutes and continue stirring. The stirring speed in the saponification kettle is controlled at 190 rpm. Then, filter it through a 120-mesh filter and transfer it to the refining kettle.

[0068] (V) Adjustment and homogenization: Add 300 parts of 150BS base oil to the refining kettle and stir, wherein the stirring speed in the refining kettle is controlled at 240 rpm, and after the temperature in the refining kettle is reduced to 155°C, start the double pumps, and use 80-mesh and 100-mesh filters for 45 minutes each, and then reduce the temperature in the refining kettle to 122°C, and then pour the mixture into the blending kettle, add 300 parts of 150BS base oil and mix evenly, and then perform homogenization treatment, the pressure of the homogenization treatment is controlled at 22MPa, the homogenization treatment time is 30 minutes, and after the homogenization treatment is completed, use a 100-mesh filter for cyclic filtration;

[0069] (VI) Additives and post-treatment: After the temperature in the blending kettle is lowered to 100°C, 0.85 parts of oil-soluble blue are added, and the mixture is refluxed and stirred for 30 minutes. After the temperature in the blending kettle is lowered to 85°C, 20 parts of diphenylamine, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and anticorrosion agent, and 120 parts of T361A antiwear agent are added in sequence. After continuous stirring for 20 minutes, the stirring speed in the blending kettle is controlled at 245 rpm, and 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil are added, and the mixture is refluxed and stirred for 38 minutes.

[0070] (VII) Degassing and filling: After the temperature in the blending kettle is reduced to 70°C, the mixture is transported into the degassing kettle through a pump body with a delivery pressure of 0.6MPa. The vacuum degree of the degassing kettle is controlled to 0.09MPa, and the negative pressure is maintained for 10 minutes. After the negative pressure ends, open the vent valve to eliminate the negative pressure, and finally fill it to obtain the finished grease.

[0071] Performance Testing

[0072] The performance of the greases obtained in the above Examples 1-3 was tested. At the same time, common greases on the market were used as comparative examples. The performance test data are shown in the following table.

[0073]

[0074]

[0075] It can be seen from the above table that the lubricating greases obtained in Examples 1-3 of the present invention are superior to the common lubricating greases on the market in terms of performance. The dropping point, as an indicator of the heat resistance of the grease, is higher in Examples 1-3 than in the comparative example, further proving its superior heat resistance. The cone penetration reflects the hardness of the grease, and the cone penetration values ​​of Examples 1-3 are within a reasonable range, indicating that they have appropriate hardness to meet different application requirements. In terms of corrosion resistance, Examples 1-3 all passed the test, indicating that they have good protective effect on metals in high temperature environments. The corrosion test results show that the grease of Examples 1-3 has low corrosion to T2 copper sheets and will not cause damage to metal parts. The test results of water runoff and steel mesh oil separation show that the grease of Examples 1-3 has better stability under high temperature and long-term use, is not easy to lose and separate oil, thereby ensuring the durability of the lubrication effect. The evaporation test results also show that the grease of Examples 1-3 has low evaporation loss at high temperatures, which helps to extend the lubrication cycle and reduce maintenance costs.

[0076] In summary, the grease prepared by the formulation process for increasing the maintenance cycle of wind power grease of the present invention has excellent performance in high temperature stability, low temperature performance, corrosion resistance, loss resistance and evaporation loss, and is particularly suitable for occasions such as wind power equipment that have high requirements on grease performance. Therefore, through the formulation process of the present invention, the service life of the grease can be significantly improved, the maintenance cost can be reduced, and the reliability of equipment operation can be improved.

[0077] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A formulation process for increasing the maintenance cycle of wind power grease, characterized in that: The formula raw materials counted by weight include: 1560 parts of 150BS base oil, 1950 parts of 500N base oil, 390 parts of dodecyl stearic acid, 119 parts of sebacic acid, 109 parts of lithium hydroxide, 20 parts of diphenylamine, 0.85 parts of oil-soluble blue, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and corrosion inhibitor, 120 parts of T361A anti-wear agent, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluoro oil.

2. The formulation process for increasing the maintenance cycle of wind power grease according to claim 1 is characterized in that: The purity of the lithium hydroxide is 57%.

3. The formulation process for increasing the maintenance cycle of wind power grease according to claim 2 is characterized in that: The process includes the following steps: Step 1, weighing and feeding: first weigh the raw materials according to the above weight parts, mix 109 parts of lithium hydroxide and 550 parts of water evenly to form 659 parts of lithium hydroxide aqueous solution, then put the weighed 1800 parts of 500N base oil into the saponification kettle, and then add 390 parts of dodecyl hydroxystearic acid and 119 parts of sebacic acid in sequence; Step 2, heating and saponification: start the heating system of the hot coal furnace, control the temperature in the saponification kettle to rise to 90-100°C, wait for the dodecyl hydroxystearic acid to melt, drop 263.6 parts of lithium hydroxide aqueous solution into the saponification kettle, control the dropping time to 45-60 minutes, and then allow the material to undergo saponification reaction in the saponification kettle; Step 3, compounding and refining: after the saponification reaction is completed, the temperature in the saponification kettle is controlled to rise to 100-105°C, and the remaining 395.4 parts of lithium hydroxide aqueous solution are added dropwise, and the dropping time is controlled to be 90-120 minutes, and then the temperature in the saponification kettle is controlled to rise to 148-152°C, 260 parts of 150BS base oil and 150 parts of 500N base oil are added and stirred, and then the temperature in the saponification kettle is controlled to rise to 207-209°C, and maintained at this temperature for 3-5 minutes; Step 4, cooling and transfer: add 700 parts of 150BS base oil to the saponification kettle and stir. After the temperature of the saponification kettle drops to 180-195°C, keep it at this temperature for 30 minutes and continue stirring. Then filter it through a 120-mesh filter and transfer it to the refining kettle; Step 5, adjustment and homogenization: add 300 parts of 150BS base oil to the refining kettle and stir, reduce the temperature in the refining kettle to 150-160°C, start the double pumps, use 80-mesh and 100-mesh filters for 45 minutes each, reduce the temperature in the refining kettle to 120-125°C, pour the mixture into the blending kettle, add 300 parts of 150BS base oil and mix evenly, then perform homogenization, and after the homogenization is completed, use a 100-mesh filter for cyclic filtration; Step 6, dosing and post-treatment: After the temperature in the blending kettle is reduced to 100°C, 0.85 parts of oil-soluble blue are added, and the mixture is refluxed and stirred for 30 minutes. After the temperature in the blending kettle is reduced to 85°C, 20 parts of diphenylamine, 2.1 parts of T706 rust inhibitor, 60 parts of T202 antioxidant and anticorrosion agent, and 120 parts of T361A antiwear agent are added in sequence. After continuous stirring for 20 minutes, 120 parts of T614 tackifier, 124 parts of polyisobutylene PB2400, and 100 parts of fluorine oil are added, and the mixture is refluxed and stirred for 30-45 minutes. Step seven, degassing and filling: after the temperature in the blending kettle is reduced to 65-75°C, the mixture is transported into the degassing kettle through the pump body, and the vacuum degree of the degassing kettle is controlled to 0.09MPa. The negative pressure is maintained for 10 minutes. After the negative pressure ends, open the vent valve to eliminate the negative pressure, and finally fill it to obtain the finished grease.

4. The formulation process for increasing the maintenance cycle of wind power grease according to claim 3 is characterized in that: In the step 2, the heating system of the hot coal furnace adopts indirect heating to provide a uniform and stable heat source for the saponification kettle; during the saponification reaction, the stirring speed in the saponification kettle is controlled at 100-150 rpm to ensure that the materials are fully mixed and fully contacted.

5. The formulation process for increasing the maintenance cycle of wind power grease according to claim 3 is characterized in that: In step 3 and step 4, the stirring speed in the saponification kettle is controlled at 150-200 rpm to ensure that the materials are fully mixed and uniform.

6. The formulation process for increasing the maintenance cycle of wind power grease according to claim 3 is characterized in that: In the step 5, the stirring speed in the refining kettle is controlled at 200-250 rpm, the pressure of the homogenization treatment in the blending kettle is controlled at 20-22 MPa, and the homogenization treatment time is 30 minutes to ensure the homogeneity and stability of the mixture.

7. The formulation process for increasing the maintenance cycle of wind power grease according to claim 3 is characterized in that: In step six, the stirring speed in the blending kettle is controlled at 200-250 rpm to ensure that each additive is fully mixed with the mixture.

8. The formulation process for increasing the maintenance cycle of wind power grease according to claim 3 is characterized in that: In the step seven, the delivery pressure of the pump body is ≤0.7 MPa to ensure that the mixture is not affected by excessive shear force during the delivery process, thereby maintaining its structural stability.