Semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion and preparation method and application thereof

By using glucose derivatives and azepine/pyrimidine compound compositions in the semiconductor chip cleaning solution to form a protective film, the galvanic corrosion problem during contact between Co and Cu is solved, and the reliability and surface quality of the chip are significantly improved.

CN119020116APending Publication Date: 2024-11-26ZHEJIANG AUFIRST MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410970564.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During post-CMP cleaning, galvanic corrosion occurs at the interface when Co and Cu contact, resulting in loss of metal or copper in the barrier layer at the trench, seriously affecting the reliability of the device.

Method used

Using a semiconductor chip cleaning solution including glucose derivatives and azelocycle/pyrimidine compounds, the composition is dissolved by ultrasonic to form a stable copper complex, forming a protective film, and inhibiting copper-cobalt galvanic corrosion.

Benefits of technology

Effectively inhibit the surface corrosion of copper, reduce its surface roughness, and promote the removal of BTA residues, significantly reducing the galvanic corrosion problem between Cu and Co.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020116A_ABST
    Figure CN119020116A_ABST
Patent Text Reader

Abstract

The invention provides a semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion as well as a preparation method and application of the semiconductor chip cleaning solution. The semiconductor chip cleaning fluid for inhibiting copper-cobalt galvanic corrosion comprises the following components by weight: 1-5 parts of a glucose derivative; 1-10 parts of an inhibitor; 1-10 parts of organic amine; and 80-90 parts of ultrapure water. The semiconductor chip cleaning fluid for inhibiting the copper-cobalt galvanic corrosion can effectively inhibit the surface corrosion of copper, reduce the surface roughness of the copper and promote the removal of BTA residues at the same time. The semiconductor chip cleaning fluid for inhibiting copper-cobalt galvanic corrosion has very good application prospects and large-scale industrial popularization potential in the field of semiconductor chip cleaning.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to chip cleaning liquid technology, and in particular to a semiconductor chip cleaning liquid for inhibiting copper-cobalt galvanic corrosion, and a preparation method and application thereof. Background Art

[0002] As the feature size of ultra-large-scale integrated circuits shrinks to 14nm or even smaller, the width of the copper trench will be further reduced. For copper deposition, the aspect ratio will become more challenging, and the traditional Ta / TaN double-layer barrier structure will lead to serious copper deposition problems, such as pinching off the trench opening and filling the copper gap with voids. At the same time, the increase in the ratio of barrier metal to copper leads to increased interconnect resistance and resistance-capacitance signal delay. In order to solve the above problems, Co and Ru are being developed internationally as barrier metals, which can not only effectively reduce the thickness of the barrier layer, but also improve electrical properties. Both Co and Ru have good barrier properties and adhesion; but Co has a lower hardness (with a Mohs hardness of 5.0 and Ru has a Mohs hardness of 6.5) and is easy to achieve a high removal rate; the reaction product of Co is cleaner; Co has a lower resistivity (Co has a resistivity of 6.3μΩ·cm and Ru has a resistivity of 7.1μΩ·cm) and is cheaper.

[0003] During the post-CMP cleaning process, due to the standard electrode potential difference between metal Co and Cu (Cu / Cu when the standard hydrogen electrode potential is 0), 2+ The standard electrode potential difference is +0.34V, Co / Co 2+ The standard electrode potential difference is -0.28V, and the interface between Co and Cu is prone to galvanic corrosion when they are in contact, resulting in the loss of barrier metal or copper in the groove, which seriously affects the reliability of the device. Therefore, controlling the galvanic corrosion of the Cu and Co interface is an urgent problem to be solved. Summary of the invention

[0004] The purpose of the present invention is to propose a semiconductor chip cleaning liquid for inhibiting copper-cobalt galvanic corrosion, aiming at the problem that galvanic corrosion is very likely to occur at the interface when Co and Cu contact during the existing post-CMP cleaning process, resulting in the loss of barrier metal or copper in the groove, which seriously affects the reliability of the device. The cleaning liquid can effectively inhibit the surface corrosion of copper, reduce its surface roughness, and promote the removal of BTA residues.

[0005] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising", etc. and similar meanings, as well as closed-ended "composed of", "composed of", etc. and similar meanings.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion, comprising the following components in weight proportions:

[0007]

[0008] Furthermore, the glucose derivative is one or more of O-(D-glucose alkylene) amino-N-phenyl carbamate, β-D-pyranoglucopyranosyl taraxyl ester, 2-O-α-D-pyranoglucopyranosyl-L-ascorbic acid and 4-O-[4,6-O-(phenylmethylene)-α-D-pyranoglucopyranosyl]-D-glucose.

[0009] Furthermore, the glucose derivative is preferably 4-O-[4,6-O-(phenylmethylene)-α-D-glucopyranosyl]-D-glucose.

[0010] Furthermore, the glucose derivative is 1-4 parts.

[0011] Furthermore, the inhibitor is a nitrogen heterocyclic and / or pyrimidine compound.

[0012] Furthermore, the nitrogen heterocycle and / or pyrimidine additive is one or more of 2-methylpyrido[3,4-d]pyrimidin-4(1H)-one, 4-aminopyrazolo[3,4-d]pyrimidine, 1H-pyrazolo[3,4-D]pyrimidine-3-carboxylic acid and 4-amino-1-phenylpyrazolo[3,4-d]pyrimidine.

[0013] Furthermore, the inhibitor is preferably 4-amino-1-phenylpyrazolo[3,4-d]pyrimidine.

[0014] Furthermore, the inhibitor is 4-10 parts.

[0015] Furthermore, the mass ratio of the glucose derivative to the inhibitor is 0.1-5:1, for example, 0.1:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, or 5:1.

[0016] Furthermore, the mass ratio of the glucose derivative to the inhibitor is preferably 0.1-1:1.

[0017] The glucose derivative selected in the present invention is a multidentate ligand, for example, 4-O-[4,6-O-(phenylmethylene)-α-D-pyranose glucopyranosyl]-D-glucose is an excellent multidentate ligand that can form a variety of metal complexes. The inhibitor of the present invention selects nitrogen heterocycles and / or pyrimidine compounds, for example, 4-amino-1-phenylpyrazolo[3,4-d]pyrimidine is a very strong inhibitor with a coordinated nitrogen atom in the molecule. 4-O-[4,6-O-(phenylmethylene)-α-D-pyranose glucopyranosyl]-D-glucose and 4-amino-1-phenylpyrazolo[3,4-d]pyrimidine are combined with 4-O-[4,6-O-(phenylmethylene)-α-D-pyranose glucopyranosyl]-D-glucose as the crosslinking ligand and 4-amino-1-phenylpyrazolo[3,4-d]pyrimidine as the terminal ligand to binuclearly chelate copper ions.

[0018] Furthermore, the organic amine is one or more of formamide, acetamide, N,N-dimethylformamide and N,N-dimethylacetamide.

[0019] Furthermore, the organic amine is preferably N,N-dimethylacetamide.

[0020] Furthermore, the organic amine is 6-10 parts.

[0021] Another object of the present invention is to disclose a method for preparing a semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion, comprising the following steps:

[0022] Glucose derivatives, organic amines, inhibitors, and ultrapure water are added to a container, which is sealed and ultrasonicated at 25-100° C. until they are completely dissolved, thereby obtaining the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion.

[0023] Furthermore, after sealing, ultrasonication is performed at 25-50° C. until the mixture is completely dissolved.

[0024] Another object of the present invention is to disclose an application of a semiconductor chip cleaning liquid for inhibiting copper-cobalt galvanic corrosion in the field of semiconductor chip cleaning.

[0025] Furthermore, the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion is used to clean the semiconductor chip, comprising the following steps:

[0026] Step 1: diluting the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion with ultrapure water by 10-100 times, and then soaking the semiconductor chip with the aqueous solution to obtain a soaked semiconductor chip;

[0027] Step 2: Rinse the soaked semiconductor chip in ultrapure water to complete the cleaning process of the semiconductor chip.

[0028] Furthermore, in step 1, the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion is diluted 10-30 times with ultrapure water.

[0029] Furthermore, the soaking temperature in step 1 is 25-100° C., and the soaking time is 2-15 hours.

[0030] Furthermore, the soaking temperature in step 1 is preferably 25-50° C., and the soaking time is preferably 2-4 hours.

[0031] Furthermore, in step 2, rinse in ultrapure water at least twice.

[0032] The semiconductor chip cleaning liquid for inhibiting copper-cobalt galvanic corrosion, the preparation method and application thereof of the present invention have the following advantages compared with the prior art:

[0033] 1) The glucose derivative used in the present invention contains multiple hydroxyl groups and can form a stable complex with copper. Since the glucose derivative is a multidentate ligand, it is easy to generate a multinuclear complex once it comes into contact with copper. The present invention uses a combination of glucose derivatives and inhibitors. The coordinated oxygen atoms in the glucose derivatives and the coordinated nitrogen atoms in the inhibitors interact with each other, and a binuclear copper complex with the glucose derivative as the cross-linked ligand and the inhibitor as the terminal ligand can be obtained, thereby protecting the chip from corrosion.

[0034] 2) The glucose derivatives and inhibitors used in the present invention contain a large amount of hydroxyl groups, which can form a protective film on the chip surface to prevent the chip from being corroded and reduce the galvanic corrosion problem between copper and cobalt.

[0035] In summary, the glucose derivatives and additives in the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion of the present invention can effectively inhibit the surface corrosion of copper, reduce its surface roughness, and promote the removal of BTA residues. The semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion of the present invention has very good application prospects and large-scale industrial promotion potential in the field of semiconductor chip cleaning. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a microscope picture of a Cu wafer magnified 100 times before cleaning.

[0037] Figure 2 This is a microscope picture magnified 100 times after a Cu wafer is cleaned with the cleaning solution of Example 1.

[0038] Figure 3 This is a microscope picture magnified 100 times after the Cu wafer was cleaned using Comparative Example 2.

[0039] Figure 4This is a microscope picture magnified 100 times after the Cu wafer was cleaned using Comparative Example 1. DETAILED DESCRIPTION

[0040] The present invention is further described below with reference to the examples. The description of the technical features described below is based on representative embodiments and specific examples of the present invention, but the present invention is not limited to these embodiments and specific examples. It should be noted that:

[0041] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0042] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0043] In this specification, the numerical range expressed using "above" or "below" means a numerical range including the number.

[0044] In this specification, the word "may" includes both performing a certain process and not performing a certain process.

[0045] In this specification, the use of "optional" or "optional" indicates that certain substances, components, execution steps, application conditions and other factors are used or not used.

[0046] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 15-25°C.

[0047] In this manual, the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.

[0048] Examples 1-6

[0049] The present invention discloses a plurality of semiconductor chip cleaning solutions for inhibiting copper-cobalt galvanic corrosion, the components and mass ratios of which are shown in Table 1.

[0050] The preparation method of the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion is as follows:

[0051] Step 1: Weigh each component in its respective amount;

[0052] Step 2: Add glucose derivatives, organic amines, inhibitors, and ultrapure water to the container in sequence, then seal and ultrasonicate at 50° C. until completely dissolved, thereby obtaining the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion.

[0053] Table 1 Components and mass ratios included in Examples 1-6

[0054]

[0055]

[0056] Comparative Example 1-2

[0057] Comparative Example 1-2 discloses two semiconductor chip cleaning solutions, the components and weight ratios of which are shown in Table 2, and the preparation methods thereof are the same as those of Example 1.

[0058] Table 2 Components and mass ratios included in Comparative Examples 1-2

[0059]

[0060] The various properties of the above embodiments or comparative examples are tested below, and the test methods and test results are as follows:

[0061] 1. Metal corrosion and galvanic corrosion

[0062] The electrochemical method was used to test the corrosion rate of copper and the galvanic corrosion of copper and cobalt in different cleaning solutions. The specific test method is: using copper and cobalt disk electrodes (3mm in diameter) as electrochemical working electrodes, platinum as the counter electrode, and a saturated Ag / AgCl electrode as the reference electrode. The cleaning solutions of the embodiments and comparative examples were used as electrolyte solutions. The open circuit potential-time (OCP-t) curve and dynamic potential polarization curve (Tafel) of the working electrode were measured respectively.

[0063] The scanning range of OCP-t is -0.4V~0.4V, and the scanning time is 1200s. The scanning range of Tafel curve is OCP±0.4V, and the scanning rate is 0.01V / s. The corrosion voltage and corrosion current can be obtained by processing the dynamic potential polarization curve using Tafel extrapolation method, and the corrosion rate ( Right now / minute), the corrosion voltage difference between Cu and Co is calculated by the formula shown in formula (b), that is, |ΔEcorr| (the smaller the value of |ΔEcorr|, the milder the galvanic corrosion between Cu and Co). The results are shown in Table 3 below.

[0064]

[0065] |ΔEcorr|=|Ecorr,Cu-Ecorr,Co| (b)

[0066] ER: corrosion rate, unit

[0067] M: molar mass, in g / mol;

[0068] Icorr: self-corrosion current, unit A / cm 2 ;

[0069] n: electrochemical reaction charge number;

[0070] F: Faraday constant;

[0071] ρ: electrode density, unit: g / cm 3 .

[0072] Table 3 Test results

[0073]

[0074] It can be seen from Table 3 that the semiconductor chip cleaning solutions for inhibiting copper-cobalt galvanic corrosion in Examples 1-6 of the present invention have much lower corrosion rates on Cu and Co than the semiconductor chip cleaning solutions in Comparative Examples 1-2, and the galvanic corrosion is milder or almost non-existent than that in Comparative Examples 1-2.

[0075] 2. Static corrosion test

[0076] The copper wafer was cut into 2cm*2cm square pieces, treated with 3wt% citric acid at room temperature for 5min, washed with pure water, dried with nitrogen, and microscope pictures were taken. Figure 1 The semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion in Example 1 and the semiconductor chip cleaning solution in Comparative Examples 1-2 were diluted 30 times with ultrapure water, and the copper wafers were soaked at room temperature for 4 hours for corrosion. After being washed with pure water, dried with nitrogen, and then microscope pictures were taken for comparison. The results are shown in FIG. Figure 2-4 shown.

[0077] Depend on Figure 1 It can be seen that the Cu wafer was not corroded before cleaning. Figure 2 It can be seen that after the Cu wafer is cleaned with the cleaning solution of Example 1, it is basically not corroded. Figure 3 It can be seen that the Cu wafer is slightly corroded after being cleaned with the cleaning solution of Comparative Example 2. Figure 4 It can be seen that the Cu wafer is severely corroded after being cleaned with the cleaning solution of Comparative Example 1.

[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion, characterized in that: The composition includes the following components in weight ratio:

2. The semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion according to claim 1, characterized in that: The glucose derivative is one or more of O-(D-glucosylalkylene)amino-N-phenylcarbamate, β-D-pyranoglucopyranosyl taraxyl ester, 2-O-α-D-pyranoglucopyranosyl-L-ascorbic acid and 4-O-[4,6-O-(phenylmethylene)-α-D-pyranoglucopyranosyl]-D-glucose.

3. The semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion according to claim 1, characterized in that: The inhibitor is a nitrogen heterocyclic compound and / or a pyrimidine compound.

4. The semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion according to claim 1, characterized in that: The mass ratio of the glucose derivative to the inhibitor is 0.1-5:

1.

5. The semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion according to claim 1, characterized in that: The organic amine is one or more of formamide, acetamide, N,N-dimethylformamide and N,N-dimethylacetamide.

6. A method for preparing a semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion according to any one of claims 1 to 5, characterized in that: The following steps are involved: Glucose derivatives, organic amines, inhibitors, and ultrapure water are added to a container, which is sealed and ultrasonicated at 25-100° C. until they are completely dissolved, thereby obtaining the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion.

7. Use of the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion according to any one of claims 1 to 5 in the field of semiconductor chip cleaning.

8. The use according to claim 7, characterized in that: Using the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion to clean semiconductor chips comprises the following steps: Step 1: diluting the semiconductor chip cleaning solution for inhibiting copper-cobalt galvanic corrosion with ultrapure water by 10-100 times, and then soaking the semiconductor chip with the aqueous solution to obtain a soaked semiconductor chip; Step 2: Rinse the soaked semiconductor chip in ultrapure water to complete the cleaning process of the semiconductor chip.

9. The use according to claim 8, characterized in that: The soaking temperature in step 1 is 25-100° C., and the soaking time is 2-15 hours.

10. The use according to claim 8, characterized in that: Step 2 Rinse at least twice in ultrapure water.

Citation Information

Cited By

  • CMP (chemical mechanical polishing) post-cleaning solution for semiconductor cobalt process and preparation method and application of CMP post-cleaning solution