Method for efficiently smelting full scrap steel in electric arc furnace
By performing EBT filling in the arc furnace and setting the scrap steel smelting ratio energy value, controlling the melt pool temperature and carbon content, the problem of low smelting technology of the entire scrap steel arc furnace is solved, and efficient smelting and cost reduction are achieved, adaptable environmental protection policy requirements.
Patent Information
- Application Number
- CN202411125089.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The existing full scrap steel arc furnace smelting technology is inefficient, resulting in an increase in production costs and a decline in corporate profits. It is affected by strict environmental protection policies, resulting in small enterprises exiting the market.
By performing EBT filling, panel and furnace shell inspection in an arc furnace, a reasonable scrap steel smelting energy ratio value is set, the melt pool temperature and carbon content are controlled, and continuous charging and oxygen injection technology is used to adjust the scrap steel feed rate and power supply. The system ensures that the melt pool temperature is between 1550 and 1580℃, and reduces the slag feed rate during the refining stage to improve smelting efficiency.
It has achieved efficient smelting of all scrap steel arc furnaces, reducing the consumption of electrical and chemical energy, improving metal yield and smelting efficiency, reducing production costs, and adapting to the strict requirements of environmental protection policies.
Smart Images

Figure CN119020549A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a high-efficiency smelting method of a full-scrap steel electric arc furnace. Background Art
[0002] The global electric arc furnace industry market size is growing. From the perspective of regional distribution, the Asia-Pacific region is the main consumer region of the global electric arc furnace industry market, accounting for more than 40% of the global market share. According to data, the global electric arc furnace industry market size has begun to rise. In 2022, the global electric arc furnace industry market size is about 1.211 billion US dollars, and the future development prospects are also very broad.
[0003] At present, with the implementation of environmental protection policies, the production and emissions of the electric arc furnace industry have been more strictly regulated, resulting in some small electric arc furnace companies being unable to afford environmental protection investment and being forced to withdraw from the market. The prices of electric arc furnace raw materials such as scrap steel and scrap iron continue to rise, resulting in an increase in the production cost of electric arc furnaces and a decrease in corporate profits. Therefore, it is particularly important to realize efficient all-scrap steel electric arc furnace smelting technology under existing conditions. Summary of the invention
[0004] The purpose of the present invention is to overcome the problem of low efficiency of the existing all-scrap steel electric arc furnace smelting technology and to provide an all-scrap steel electric arc furnace high-efficiency smelting method.
[0005] The specific plan is as follows:
[0006] A method for efficiently smelting all scrap steel in an electric arc furnace comprises the following steps:
[0007] Step 1: Preparation
[0008] Before charging, the EBT charging operation and general inspection of the panel, furnace shell, ejector, refractory material and electrode length are carried out; the final repair of the arc furnace body or furnace wall is completed before charging. The target chemical analysis is different from the previous heat, and the residues of the previous heat in the arc furnace need to be emptied;
[0009] Step 2: Continuous slag charging and smelting stage
[0010] Add lime, dolomite, carbon balls and scrap steel into the furnace, perform oxygen injection operation, set the scrap steel smelting specific energy value, gradually adjust the scrap steel feeding rate, make the temperature of the molten pool be 1550-1570°C, and perform smelting operation;
[0011] Step 3: Refining Phase
[0012] Increase the specific energy value and reduce the slag feed rate to raise the molten pool temperature to 1560-1580°C, and carry out refining operations. During the refining process, monitor the temperature in the molten pool and the carbon content of the samples in the molten pool. When the temperature in the molten pool is greater than or equal to 1600°C, and / or the carbon content is less than or equal to 0.06wt%, the smelting is completed and steel is tapped.
[0013] Furthermore, the optimal steel retention at the beginning of the electric arc furnace is 30%-40% of the maximum furnace capacity volume ratio.
[0014] Furthermore, the scrap steel in step 2 is continuously fed, and the flow rate of the porous plug used should be set at 3×(70~110)Nm 3 / h.
[0015] Furthermore, the oxygen injection operation in step 2 starts 1-3 minutes after the scrap steel is continuously fed.
[0016] Furthermore, the oxygen injection in step 2 includes furnace door oxygen lance injection and furnace wall oxygen lance injection, wherein the furnace door oxygen lance injection is opened before the furnace wall oxygen lance injection, and the flow rate of the furnace door oxygen lance injection is 2500-3500Nm 3 / h, the flow rate of the furnace wall oxygen lance injection is 1500-3500Nm 3 / h, the flow rate of furnace wall carbon gun injection is 20-40kg / min.
[0017] Furthermore, in step 2, the lime is continuously fed at a rate of 100-350 kg / min; the dolomite is continuously fed at a rate of 100-200 kg / min; and the carbon balls are continuously fed at a rate of 100-150 kg / min.
[0018] Furthermore, the amount of lime and dolomite added in step 2 satisfies that the slag basicity in the smelting stage is maintained in the range of (CaO%+MgO%) / SiO2%=2.2-2.3.
[0019] Furthermore, the temperature of the molten pool in step 2 is controlled by the following method: when the measured value of T is greater than 1570°C, the set specific energy value is reduced, which corresponds to an increase in the scrap steel feeding rate; when the measured value of T is less than 1550°C, the set specific energy value is increased, which corresponds to a decrease in the scrap steel feeding rate.
[0020] Furthermore, in step 3, the power of the arc furnace is reduced to ensure the coverage of the arc, and the flow rate of the argon bottom blowing flow is set at 3×(70~110)Nm 3 / min.
[0021] Furthermore, at least one of the following (1)-(11) is present:
[0022] (1) The total time of the smelting and refining stages is 30-40 minutes per 200 tons of scrap steel;
[0023] (2) The metal recovery rate is 90-95%;
[0024] (3) The power consumption per ton of scrap steel is 330.0-335.0 kWh / t;
[0025] (4) Electrode consumption is 0.92-0.97 kg / t;
[0026] (5) Oxygen consumption per ton of scrap steel is 35.1-35.6 Nm 3 / t;
[0027] (6) Natural gas consumption is 0.5-1.0Nm 3 / t;
[0028] (7) The unit consumption of carbon powder during oxygen injection is 20-24kg / t;
[0029] (8) The carbon ball consumption is 5-10kg / t when entering the furnace;
[0030] (9) The lime consumption per ton of scrap steel is 18-24 kg / t;
[0031] (10) The dolomite consumption per ton of scrap steel is 11-15 kg / t;
[0032] (11) The bottom blowing stirring gas consumption per ton of scrap steel is 0.06-0.10Nm 3 / t.
[0033] Beneficial effects:
[0034] The present invention improves the utilization efficiency of electrical energy and chemical energy by controlling a reasonable power supply system and a slag supply system, and strictly controls operations in the continuous charging stage and the refining stage according to the actual situation in the furnace, while also accurately controlling the steel tapping temperature and composition, thereby achieving a role in efficient smelting of all-scrap steel electric furnaces and reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solution of the present invention, the accompanying drawings will be briefly introduced below. Obviously, the accompanying drawings in the following description only relate to some embodiments of the present invention, but are not intended to limit the present invention.
[0036] Figure 1 A diagram showing a setting scheme for the specific energy consumption of scrap steel in the smelting process provided by the present invention;
[0037] Figure 2 A diagram showing a setting scheme for the continuous feeding speed of scrap steel in the smelting process provided by the present invention;
[0038] Figure 3 The apparent power setting scheme diagram of the smelting process provided by the present invention;
[0039] Figure 4 A diagram of the total flow rate setting scheme of the furnace wall oxygen lance in the smelting process provided by the present invention;
[0040] Figure 5 A diagram of the total flow rate setting scheme of the furnace door oxygen lance in the smelting process provided by the present invention;
[0041] Figure 6 This is a diagram of a setting scheme for the total carbon flow rate entering the furnace during the smelting process provided by the present invention. DETAILED DESCRIPTION
[0042] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. In the examples, those without specifying specific techniques or conditions are carried out according to the techniques or conditions described in the literature in this area or according to the product specification. Those without specifying the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially. In the following examples, if not clearly stated, "%" refers to weight percentage.
[0043] This embodiment provides a method for high-efficiency smelting of all scrap steel in an electric arc furnace, comprising the following steps:
[0044] Step 1: Preparation
[0045] Before charging, the EBT (Eccentric Bottom Tapping) furnace is charged and the panel, furnace shell, ejector, refractory material and electrode length are generally checked; the final repair of the EAF furnace body or furnace wall is completed before charging. The target chemical analysis is different from the previous heat, and the residues of the previous heat in the EAF need to be emptied;
[0046] Step 2: Continuous slag charging and smelting stage
[0047] Add slag materials including lime, dolomite, carbon balls and scrap steel into the furnace, perform oxygen injection operation, set the scrap steel smelting specific energy value, gradually adjust the scrap steel feeding rate, make the temperature of the molten pool be 1550-1570°C, and perform smelting operation;
[0048] Step 3: Refining Phase
[0049] Increase the specific energy value and reduce the slag feed rate to raise the molten pool temperature to 1560-1580°C, and carry out refining operations. During the refining process, monitor the temperature in the molten pool and the carbon content of the samples in the molten pool. When the temperature in the molten pool is greater than or equal to 1600°C, and / or the carbon content is less than or equal to 0.06wt%, the smelting is completed and steel is tapped.
[0050] In this embodiment, the optimal steel retention at the beginning of the electric arc furnace is 30%-40% of the maximum furnace capacity volume ratio.
[0051] In this embodiment, the scrap steel in step 2 is continuously fed, and the flow rate of the porous plug used should be set at 3×(70-110)Nm 3 / h.
[0052] In this embodiment, the oxygen injection operation in step 2 starts after the scrap steel is continuously fed for 1-3 minutes.
[0053] In this embodiment, the oxygen injection in step 2 includes furnace door oxygen lance injection and furnace wall oxygen lance injection, wherein the furnace door oxygen lance injection is opened before the furnace wall oxygen lance injection, and the flow rate of the furnace door oxygen lance injection is 2500-3500Nm 3 / h, the flow rate of the furnace wall oxygen lance injection is 1500-3500Nm 3 / h, the flow rate of furnace wall carbon gun injection is 20-40kg / min.
[0054] In this embodiment, in step 2, the lime is continuously fed at a rate of 100-350 kg / min; the dolomite is continuously fed at a rate of 100-200 kg / min; and the carbon balls are continuously fed at a rate of 100-150 kg / min.
[0055] In this embodiment, the amount of lime and dolomite added in step 2 satisfies: the slag basicity in the smelting stage is maintained in the range of (CaO%+MgO%) / SiO2%=2.2-2.3.
[0056] In this embodiment, the temperature of the molten pool in step 2 is controlled by the following method: when the measured value of T is greater than 1570°C, the set specific energy value is reduced, which corresponds to an increase in the scrap steel feed rate; when the measured value of T is less than 1550°C, the set specific energy value is increased, which corresponds to a decrease in the scrap steel feed rate. In this case, high-valent iron oxides may be formed, inhibiting the foaming of the slag, thereby reducing the output of the applied electrical energy. The reduction in the feed rate may not be sufficient to melt these high-valent iron oxides and heat the molten pool. In this case, the measure to be taken is to stop the slag charging for a few minutes until the arc stability condition is restored.
[0057] In this embodiment, in step 3, the arc furnace power is reduced to ensure the arc coverage, and the flow rate of the argon bottom blowing flow is set at 3×(70-110)Nm 3 / min.
[0058] In this embodiment, at least one of the following (1)-(11) is present:
[0059] (1) The total time of the smelting and refining stages is 30-40 minutes per 200 tons of scrap steel;
[0060] (2) The metal recovery rate is 90-95%;
[0061] (3) The power consumption per ton of scrap steel is 330.0-335.0 kWh / t;
[0062] (4) Electrode consumption is 0.92-0.97 kg / t;
[0063] (5) Oxygen consumption per ton of scrap steel is 35.1-35.6 Nm 3 / t;
[0064] (6) Natural gas consumption is 0.5-1.0Nm 3 / t;
[0065] (7) The unit consumption of carbon powder during oxygen injection is 20-24kg / t;
[0066] (8) The carbon ball consumption is 5-10kg / t when entering the furnace;
[0067] (9) The lime consumption per ton of scrap steel is 18-24 kg / t;
[0068] (10) The dolomite consumption per ton of scrap steel is 11-15 kg / t;
[0069] (11) The bottom blowing stirring gas consumption per ton of scrap steel is 0.06-0.10Nm 3 / t.
[0070] Example 1
[0071] (1) Furnace preparation
[0072] The present invention selects an electric furnace with a total capacity of 270t, a nominal steel output of 175t, a steel retention of 95t, a transformer rated power of 140MVA, and an allowable overload of 20MVA.
[0073] Before charging, EBT filling (sand filling operation at EBT outlet) and general inspection of panels, furnace shell, ejectors, refractory materials, electrode length, final repair of furnace body or furnace wall must be completed before charging. If the target chemical analysis is different from the previous heat, the furnace needs to be emptied to remove the residues of the previous heat. The optimal steel retention at the beginning of the heat is about 95t.
[0074] 4t of lime, 2.5t of dolomite and 1.2t of carbon balls are added to the electric arc furnace. This stage takes a total of 3 minutes.
[0075] (2) Continuous slag charging and smelting
[0076] By setting the appropriate smelting specific energy value (kW·h / t), see Figure 1 , gradually increase the slag feeding rate, see Figure 2 After 3 minutes of reducing the specific energy consumption of scrap steel, the scrap steel feeding rate will reach the nominal value, and the total amount of scrap steel added will be 206 tons. The injection operation of oxygen and carbon powder will start after 2 minutes of continuous slag charging to ensure rapid slag foaming so that high power can be used as early as possible. The apparent power setting of the arc furnace can be seen in Figure 3 Specifically, oxygen injection includes furnace door oxygen lance and furnace wall oxygen lance, where the furnace door oxygen lance is opened before the furnace wall oxygen lance. The flow rate setting scheme of the two can be found in Figure 4 and Figure 5 For the total flow setting scheme of carbon powder and carbon balls, please refer to Figure 6 In order to improve the efficiency of carbon powder injection, a supersonic oxygen lance will be used to carry carbon powder into the slag layer.
[0077] During the continuous feeding of slag, the flow rate of the porous plug (for bottom blowing gas holes) should be set to 3×90Nm 3 / h. Check the temperature of the molten pool every 5 minutes and keep it at about 1570℃. For temperature control, the following strategy should be adopted: fix the power supply and change the slag feeding rate as needed. During this stage, lime and dolomite are continuously fed at a feeding rate of 150kg / min and 105kg / min respectively. Lime and dolomite are continuously added from the start of power-on. The slag basicity during the melting period should be (CaO%+MgO%) / SiO2%=2.3, where CaO%, MgO% and SiO2% refer to the weight percentages of CaO, MgO and SiO2 in the slag in the furnace, respectively.
[0078] In the first 15 minutes of the nominal value range of the continuous feeding stage, the carbon balls are continuously fed at a rate of 105 kg / min. When the T measured value is >1570℃, measures should be taken to reduce the set specific energy value (kWh / t), which corresponds to an increase in the slag feed rate. When the T measured value is <1550℃, measures should be taken to increase the set specific energy value kWh / t, which corresponds to a decrease in the slag feed rate.
[0079] (3) Refining stage
[0080] During the refining phase, a higher specific energy value is set, the slag feed rate is reduced, and the bath temperature is allowed to increase. Once all the slag has been fed into the furnace, the arc is kept heating until the tapping temperature is reached.
[0081] At 1580°C, the temperature and samples were collected at the beginning of refining, and the chemical analysis results showed that the C content was 0.15wt% to 0.25wt%, and the P and S contents were <0.030wt%. During the refining process, the power was reduced to ensure the arc coverage, and the bottom blowing flow rate of argon was set to 3×90Nm 3 / min. During the refining process, the temperature and carbon content were measured. The final temperature before tapping was 1610°C and the carbon content was 0.06wt%. The total time of the continuous feeding stage and the refining stage was 30min.
[0082] After the composition and temperature are qualified, the steel is tapped. The tapping time is about 3 minutes, and the total smelting cycle is 36 minutes. The other technical and economic indicators are shown in Table 1.
[0083] Table 1 Technical and economic indicators
[0084] Metal recovery rate 92.0% Electricity consumption per ton of steel 333.0kWh / t Electrode consumption 0.94kg / t Oxygen consumption per ton of steel <![CDATA[35.5Nm 3 / t]]> Natural gas consumption <![CDATA[0.8Nm 3 / t]]> Injection toner consumption 22kg / t Carbon ball consumption 6kg / t Lime consumption per ton of steel 21kg / t Dolomite consumption per ton of steel 13kg / t Bottom blowing stirring gas consumption per ton of steel <![CDATA[0.09Nm 3 / t]]>
[0085] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0086] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0087] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A high-efficiency smelting method of all-scrap steel in an electric arc furnace, characterized in that: The steps include: Step 1: Preparation Before charging, the EBT furnace is charged and the panel, furnace shell, ejector, refractory material and electrode length are generally checked; the final repair of the arc furnace body or furnace wall is completed before charging. The target chemical analysis is different from the previous heat, and the residues of the previous heat in the arc furnace need to be emptied; Step 2: Slag continuous charging and smelting stage Add lime, dolomite, carbon powder and scrap steel into the furnace, perform oxygen injection operation, set the scrap steel smelting specific energy value, gradually adjust the scrap steel feeding rate, make the molten pool temperature 1550 ~ 1570 ℃, and perform smelting operation; Step 3: Refining Phase Increase the specific energy value and reduce the slag feed rate to raise the molten pool temperature to 1560-1580°C, and carry out refining operations. During the refining process, monitor the temperature in the molten pool and / or the carbon content of the samples in the molten pool. When the temperature in the molten pool is greater than or equal to 1600°C, and / or the carbon content is less than or equal to 0.06wt%, the smelting is completed and steel is tapped.
2. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 1, characterized in that: The optimum steel retention of the electric arc furnace is 30%-40% of the maximum furnace capacity volume ratio.
3. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 1, characterized in that: In step 2, the scrap steel is continuously fed, and the flow rate of the porous plug is set at 3×(70-110)Nm 3 / h.
4. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 1, characterized in that: The oxygen injection operation in step 2 starts after the scrap steel is continuously fed for 1-3 minutes.
5. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 4, characterized in that: The oxygen injection in step 2 includes furnace door oxygen lance injection and furnace wall oxygen lance injection, wherein the furnace door oxygen lance injection is opened before the furnace wall oxygen lance injection, and the flow rate of the furnace door oxygen lance injection is 2500-3500Nm 3 / h, the flow rate of the furnace wall oxygen lance injection is 1500-3500Nm 3 / h, the flow rate of carbon powder sprayed by the furnace wall carbon gun is 20-40kg / min.
6. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 1, characterized in that: In step 2, the lime is continuously fed at a rate of 100-350 kg / min; the dolomite is continuously fed at a rate of 100-200 kg / min; and the carbon balls are continuously fed at a rate of 100-150 kg / min.
7. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 6, characterized in that: The amount of lime and dolomite added in step 2 satisfies: the slag basicity in the smelting stage is maintained in the range of (CaOwt%+MgOwt%) / SiO2wt%=2.2-2.
3.
8. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 1, characterized in that: The temperature of the molten pool in step 2 is controlled by the following method: When the T measured value is greater than 1570°C, the set specific energy value is reduced, which corresponds to an increase in the scrap steel feeding rate; when the T measured value is less than 1550°C, the set specific energy value is increased, which corresponds to a decrease in the scrap steel feeding rate.
9. The method for high-efficiency smelting of all scrap steel in an electric arc furnace according to claim 1, characterized in that: In step 3, the power of the arc furnace is reduced to ensure the arc coverage, and the flow rate of the argon bottom blowing flow is set at 3×(70~110)Nm 3 / min.
10. A high-efficiency electric arc furnace smelting method for all scrap steel according to any one of claims 1 to 9, characterized in that: Having at least one of the following (1)-(11): (1) The total time of the smelting and refining stages is 30-40 minutes per 200 tons of scrap steel; (2) The metal recovery rate is 90-95%; (3) The power consumption per ton of scrap steel is 330.0-335.0 kWh / t; (4) Electrode consumption is 0.92-0.97 kg / t; (5) Oxygen consumption per ton of scrap steel is 35.1-35.6 Nm 3 / t; (6) Natural gas consumption is 0.5-1.0Nm 3 / t; (7) The unit consumption of carbon powder during oxygen injection is 20-24kg / t; (8) The carbon ball consumption is 5-10kg / t when entering the furnace; (9) The lime consumption per ton of scrap steel is 18-24 kg / t; (10) The dolomite consumption per ton of scrap steel is 11-15 kg / t; (11) The bottom blowing stirring gas consumption per ton of scrap steel is 0.06-0.10Nm 3 / t.