Method for reducing TOC (total organic carbon) in zinc oxide concentrate leachate

Through ultrasonic treatment and peeling agent capture technology, the problem of residual flotation agent on the surface of zinc oxide concentrate in oxosulfur mixed concentrate was solved, which significantly reduced the TOC content in the sulfuric acid leaching solution, increased the leaching rate of zinc, and avoided zinc It is difficult to burn and peel during electrodisposition.

CN119020607APending Publication Date: 2024-11-26KUNMING METALLURGY INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411072401.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

After flotation of oxosulfur mixed concentrate, flotation agents remain on the surface of zinc oxide concentrate, resulting in high TOC content in the sulfuric acid leaching solution, affecting the subsequent zinc electrostatic accumulation process, and it is easy to cause difficulty in peeling off the plate and zinc sheets.

Method used

The method of ultrasonic treatment combined with the peeling agent is adopted. After stirring zinc oxide concentrate with water, the adhered flotation agent is used to remove ultrasonic and add the peeling agent for the capture. The reaction temperature is 20~50℃, and the reaction time is After 5 to 40 minutes, solid-liquid separation is performed to obtain zinc oxide products to enter the sulfuric acid leaching process.

Benefits of technology

Effectively reduce the TOC content in the zinc oxide concentrate leaching liquid, and the zinc leaching rate exceeds 96%, avoiding the problem of peeling off the plate and zinc sheets, and ensuring the stability of the subsequent process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for reducing TOC (Total Organic Carbon) in a zinc oxide concentrate leaching solution, and belongs to the technical field of lead zinc ore beneficiation. The method comprises the following steps that zinc oxide concentrate and water are added into a stirring tank according to the liquid-solid ratio of (1.5-3): 1, and stirring and size mixing are conducted; the ore pulp is subjected to ultrasonic treatment, the flotation reagent attached to the surface of the zinc oxide concentrate is stripped, the ultrasonic intensity is 0.3-1 w / cm < 2 >, and the ultrasonic frequency is 20-35 kHz. And during ultrasonic treatment, a stripping agent is added while stirring to collect the flotation reagent, the dosage of the stripping agent is 0.1-2% of the mass of the zinc oxide concentrate in the ore pulp, the reaction time of stripping and collecting is 5-40 min, and the reaction temperature is 20-50 DEG C. And the treated ore pulp is subjected to solid-liquid separation, and obtained filter residues are zinc oxide products and enter the leaching procedure. After the zinc oxide concentrate is treated through the method, the flotation reagent left on the surface of the zinc oxide concentrate can be effectively removed, the zinc leaching rate of the zinc oxide concentrate is larger than 96%, the TOC content of leachate is smaller than 18 mg / L, and the problems that in the subsequent zinc electrodeposition process, plate burning occurs, and zinc sheets are difficult to strip are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lead-zinc ore dressing, and in particular relates to a method for reducing TOC in zinc oxide concentrate leaching solution. Background Art

[0003] Based on many years of previous research, low-grade oxygen-sulfur mixed stockpiles can be mixed with oxygen-sulfur mixed concentrates through mixed flotation, which has good economic efficiency and process stability. There are two key technical difficulties in the smelting application of this mixed concentrate: (1) Because it is a mixture of oxygen and sulfur, it is difficult to enter the existing smelting process; (2) After mixed flotation, the oxidized ore is coated and sulfided by the flotation reagents (xanthate, No. 2 oil, sodium lignin sulfonate, octadecylamine, etc.), and the existing mineral processing technology is difficult to separate oxygen and sulfur.

[0004] Since the oxygen-sulfur mixed concentrate is a beneficiation product, even if the zinc oxide and zinc sulfide are separated through the oxygen-sulfur separation process, a small amount of flotation agent still remains on the surface of the zinc oxide concentrate. The TOC content in the leachate after the zinc oxide concentrate is leached with sulfuric acid is high, which will lead to problems such as burning of the plate and difficulty in stripping of the zinc sheets in the subsequent zinc electrowinning process. Summary of the invention

[0005] The object of the present invention is to provide a method for reducing TOC in zinc oxide concentrate leachate.

[0006] The object of the present invention is achieved in that the method for reducing TOC in zinc oxide concentrate leachate comprises the following steps: Step 1: Add zinc oxide concentrate and water into a stirring tank at a liquid-to-solid ratio of 1.5-3:1, and stir to prepare the slurry.

[0007] Step 2: Ultrasonic treatment is performed on the pulp to remove the flotation reagent attached to the surface of the zinc oxide concentrate. The ultrasonic intensity is 0.3~1w / cm 2 , the ultrasonic frequency is 20~35kHz.

[0008] During the ultrasonic treatment, a stripping agent is added while stirring to collect the flotation agent. The amount of the stripping agent is 0.1-2% of the mass of the zinc oxide concentrate in the slurry. The reaction time of the stripping and collection is 5-40 minutes, and the reaction temperature is 20-50°C.

[0009] Step 3: The treated slurry is subjected to solid-liquid separation, and the resulting filter residue is the zinc oxide product, which enters the leaching process.

[0010] Compared with the prior art, the technical solution of the present invention has outstanding substantive features and significant progress in the following aspects: the method of the present invention is used to treat the zinc oxide concentrate obtained in the oxygen-sulfur mixed concentrate beneficiation process, and the synergistic application of ultrasonic treatment combined with stripping agent collection can effectively strip the flotation reagents (xanthate, No. 2 oil, sodium lignin sulfonate, octadecylamine, etc.) remaining on the surface of the zinc oxide concentrate. After the treated zinc oxide concentrate is leached with sulfuric acid, the zinc leaching rate is greater than 96%, and the TOC content of the leaching solution is less than 18 mg / L, which avoids the problem of burning plates and difficulty in stripping zinc sheets in the subsequent zinc electrowinning process. DETAILED DESCRIPTION

[0011] The present invention is further described below, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.

[0012] The method for reducing TOC in zinc oxide concentrate leaching solution of the present invention comprises the following steps: Step 1: Add zinc oxide concentrate and water into a stirring tank at a liquid-to-solid ratio of 1.5-3:1, and stir to prepare the slurry.

[0013] Step 2: Ultrasonic treatment is performed on the pulp to remove the flotation reagent attached to the surface of the zinc oxide concentrate. The ultrasonic intensity is 0.3~1w / cm 2 , the ultrasonic frequency is 20~35kHz.

[0014] During the ultrasonic treatment, a stripping agent is added while stirring to collect the flotation agent. The amount of the stripping agent is 0.1-2% of the mass of the zinc oxide concentrate in the slurry. The reaction time of the stripping and collection is 5-40 minutes, and the reaction temperature is 20-50°C.

[0015] Step 3: The treated slurry is subjected to solid-liquid separation, and the resulting filter residue is the zinc oxide product, which enters the leaching process.

[0016] The liquid-to-solid ratio in step 1 is preferably 2.5:1.

[0017] The stirring speed in step 1 is 300-600 r / min, preferably 500 r / min.

[0018] The ultrasonic intensity of the ultrasonic treatment in step 2 is preferably 0.8w / cm 2 , the ultrasonic frequency is preferably 30kHz.

[0019] The stripping agent in step 2 comprises, by weight, 15 to 30 parts of polysorbate-80, 30 to 60 parts of octylphenol polyoxyethylene ether, and 20 to 40 parts of nonylphenol polyoxyethylene ether, wherein the amount of at least one component is not 0. The preferred formula of the stripping agent comprises, by weight, 20 to 30 parts of polysorbate-80, 35 to 50 parts of octylphenol polyoxyethylene ether, and 25 to 35 parts of nonylphenol polyoxyethylene ether.

[0020] The stirring speed in step 2 is 400-800 r / min, preferably 500 r / min.

[0021] The preferred amount of the stripping agent in step 2 is 1% of the mass of the zinc oxide concentrate in the slurry.

[0022] The reaction time of the stripping and capturing in step 2 is preferably 20 min, and the reaction temperature is preferably 35°C.

[0023] The leaching process in step 3 refers to leaching the obtained zinc oxide product with sulfuric acid, with an acid-ore ratio of 0.7:1, a leaching temperature of 60°C, a leaching liquid-solid ratio of 4:1, and a leaching time of 2h. After the leaching is completed, the zinc content of the leached residue is analyzed by chemical titration, and the zinc leaching rate is greater than 96%. The TOC content of the leaching solution is analyzed by combustion oxidation-non-dispersive infrared absorption method, and the TOC content is less than 18mg / L.

[0024] Example 1 The method for reducing TOC in zinc oxide concentrate leaching solution is specifically: Step 1: Add 1000g zinc oxide concentrate and 2500g water into a stirring tank, stir and prepare the slurry at a stirring speed of 500r / min.

[0025] Step 2: Ultrasonic treatment is performed on the pulp to remove the flotation reagent attached to the surface of the zinc oxide concentrate. The ultrasonic intensity is 0.8w / cm 2 , the ultrasonic frequency is 30kHz.

[0026] While ultrasonic treatment, 10g of stripping agent was slowly added while stirring to collect the flotation agent, and the stirring speed was 500r / min. The stripping agent contained 2g of water, 2g of polysorbate-80, 3.5g of octylphenol polyoxyethylene ether, and 2.5g of nonylphenol polyoxyethylene ether. The reaction time of stripping and collecting was 20min, and the reaction temperature was 35°C.

[0027] Step 3: The treated slurry is subjected to solid-liquid separation, and the resulting filter residue is the zinc oxide product, which enters the sulfuric acid leaching process, with an acid-ore ratio of 0.7:1, a leaching temperature of 60°C, a leaching liquid-solid ratio of 4:1, and a leaching time of 2 hours. After the leaching is completed, the zinc content of the leached residue is analyzed by chemical titration, and the zinc leaching rate is 96.78%. The TOC content of the leaching solution is analyzed by combustion oxidation-non-dispersive infrared absorption method, and the TOC content is 17.13 mg / L.

[0028] Example 2 The method for reducing TOC in zinc oxide concentrate leaching solution is specifically: Step 1: Add 1000g zinc oxide concentrate and 3000g water into a stirring tank, stir and prepare the slurry, and the stirring speed is 300r / min.

[0029] Step 2: Ultrasonic treatment is performed on the pulp to remove the flotation reagent attached to the surface of the zinc oxide concentrate. The ultrasonic intensity is 0.3w / cm 2 , the ultrasonic frequency is 35kHz.

[0030] While ultrasonic treatment, 20g of stripping agent was slowly added while stirring to collect the flotation reagent, and the stirring speed was 400r / min. The stripping agent contained 1g of water, 4.5g of polysorbate-80, 8.5g of octylphenol polyoxyethylene ether, and 6g of nonylphenol polyoxyethylene ether. The reaction time of stripping and collecting was 40min, and the reaction temperature was 20°C.

[0031] Step 3: The treated slurry is subjected to solid-liquid separation, and the obtained filter residue is the zinc oxide product, which enters the sulfuric acid leaching process, and the process parameters of this process are the same as those in Example 1. After the leaching is completed, the zinc content analysis method of the leached residue and the TOC content analysis method of the leaching liquid are the same as those in Example 1, and the zinc leaching rate is 97.42% and the TOC content is 16.85 mg / L.

[0032] Example 3 The method for reducing TOC in zinc oxide concentrate leaching solution is specifically: Step 1: Add 1000g zinc oxide concentrate and 1500g water into a stirring tank, stir and prepare the slurry, and the stirring speed is 600r / min.

[0033] Step 2: Ultrasonic treatment is performed on the pulp to remove the flotation reagent attached to the surface of the zinc oxide concentrate. The ultrasonic intensity is 1w / cm 2 , the ultrasonic frequency is 20kHz.

[0034] While ultrasonic treatment, 5g of stripping agent was slowly added while stirring to collect the flotation agent, and the stirring speed was 800r / min. The stripping agent contained 0.8g of water, 1.2g of polysorbate-80, 1.8g of octylphenol polyoxyethylene ether, and 1.2g of nonylphenol polyoxyethylene ether. The reaction time of stripping and collecting was 5min, and the reaction temperature was 50°C.

[0035] Step 3: The treated slurry is subjected to solid-liquid separation, and the obtained filter residue is the zinc oxide product, which enters the sulfuric acid leaching process, and the process parameters of this process are the same as those in Example 1. After the leaching is completed, the zinc content analysis method of the leached residue and the TOC content analysis method of the leaching liquid are the same as those in Example 1, and the zinc leaching rate is 96.90%, and the TOC content is 15.81 mg / L.

[0036] Example 4 ——Comparison example The method for reducing TOC in zinc oxide concentrate leaching solution as a control example is as follows: Step 1: Add 1000g zinc oxide concentrate and 2500g water into a stirring tank, stir and prepare the slurry at a stirring speed of 500r / min.

[0037] Step 2: Ultrasonic treatment is performed on the pulp to remove the flotation reagent attached to the surface of the zinc oxide concentrate. The ultrasonic intensity is 0.2w / cm 2 , the ultrasonic frequency is 15kHz.

[0038] While ultrasonic treatment, 0.5g of stripping agent was slowly added while stirring to collect the flotation agent, and the stirring speed was 500r / min. The stripping agent contained 0g of water, polysorbate-800.05g, 0.3g of octylphenol polyoxyethylene ether, and 0.15g of nonylphenol polyoxyethylene ether. The reaction time of stripping and collecting was 20min, and the reaction temperature was 35°C.

[0039] Step 3: The treated slurry is subjected to solid-liquid separation, and the obtained filter residue is the zinc oxide product, which enters the sulfuric acid leaching process, and the process parameters of this process are the same as those in Example 1. After the leaching is completed, the zinc content analysis method of the leached residue and the TOC content analysis method of the leaching liquid are the same as those in Example 1, and the zinc leaching rate is 95.07% and the TOC content is 54.63 mg / L.

[0040] The working principle and working process of the present invention: The surface of sulfide ore is hydrophobic, and the surface of oxide ore is hydrophilic. However, due to the presence of a large number of mineral processing agents, the metal atoms on the surface of the mineral will interact with the flotation agent, causing the sulfide ore and the oxide ore to flocculate, and then form an oxygen-sulfur mixed concentrate after flotation. After ultrasonic treatment of the oxygen-sulfur mixed concentrate, the mineral processing agent can be desorbed from the surface of the oxygen-sulfur mixed concentrate, and the oxide ore and the sulfide ore are separated. However, the mineral processing agent still exists. The addition of RH-3000 can interact with the mineral processing agent, so that the mineral processing agent cannot adhere to the mineral surface, and the purpose of separating the oxide ore and the sulfide ore is achieved.

[0041] Since the emulsifier is made of polysorbate 80, octylphenol polyoxyethylene ether and nonylphenol polyoxyethylene ether, the different components form a synergistic effect. The surface of the reagent has more hydrophilic and hydrophobic chemical groups, which preferentially react with the polar and non-polar groups on the surface of the mineral processing reagent free in the slurry after ultrasound, so that the mineral processing reagent cannot be adsorbed on the mineral surface, and the organic matter on the surface of the zinc oxide concentrate is removed after solid-liquid separation, so as to reduce TOC in the zinc oxide concentrate leachate.

Claims

1. A method for reducing TOC in zinc oxide concentrate leachate, characterized in that The following steps are involved: Step 1: Add zinc oxide concentrate and water into a stirring tank at a liquid-to-solid ratio of 1.5-3:1, and stir to prepare the slurry; Step 2: Ultrasonic treatment is performed on the pulp to remove the flotation reagent attached to the surface of the zinc oxide concentrate. The ultrasonic intensity is 0.3~1w / cm 2 , ultrasonic frequency is 20~35kHz; During the ultrasonic treatment, a stripping agent is added while stirring to collect the flotation reagent. The amount of the stripping agent is 0.1-2% of the mass of the zinc oxide concentrate in the slurry. The reaction time for stripping and collection is 5-40 minutes, and the reaction temperature is 20-50°C. Step 3: The treated slurry is subjected to solid-liquid separation, and the resulting filter residue is the zinc oxide product, which enters the leaching process.

2. The method for reducing TOC in zinc oxide concentrate leachate according to claim 1, characterized in that: The liquid-to-solid ratio in step 1 is 2.5:

1.

3. The method for reducing TOC in zinc oxide concentrate leachate according to claim 1, characterized in that: The stirring speed in step 1 is 300-600 r / min.

4. The method for reducing TOC in zinc oxide concentrate leachate according to claim 1, characterized in that: The ultrasonic intensity of the ultrasonic treatment in step 2 is 0.8w / cm 2 , the ultrasonic frequency is 30kHz.

5. The method for reducing TOC in zinc oxide concentrate leachate according to claim 1, characterized in that: The stripping agent in step 2 comprises, by mass, 15 to 30 parts of polysorbate 80, 30 to 60 parts of octylphenol polyoxyethylene ether, and 20 to 40 parts of nonylphenol polyoxyethylene ether, wherein the amount of at least one component is not zero.

6. The method for reducing TOC in zinc oxide concentrate leachate according to claim 5, characterized in that: The stripping agent in step 2 comprises 20-30 parts of polysorbate-80, 35-50 parts of octylphenol polyoxyethylene ether, and 25-35 parts of nonylphenol polyoxyethylene ether, by mass.

7. The method for reducing TOC in zinc oxide concentrate leachate according to claim 1, characterized in that: The stirring speed in step 2 is 400-800 r / min.

8. The method for reducing TOC in zinc oxide concentrate leachate according to claim 1, characterized in that: The amount of the stripping agent used in step 2 is 1% of the mass of the zinc oxide concentrate in the slurry.

9. The method for reducing TOC in zinc oxide concentrate leachate according to claim 1, characterized in that: The reaction time of the stripping and collecting in step 2 is 20 minutes, and the reaction temperature is 35°C.