Production process for increasing nitrogen content in vanadium-containing deformed steel bar

By adjusting the process parameters of the converter and LF refining furnace, optimizing the nitrogen blowing mode and using ferrosilicon nitride alloy, the problem of insufficient nitrogen content in the vanadium-containing rebar in the existing technology is solved, and the nitrogen content is stable and the production cost is achieved. reduce.

CN119020668AActive Publication Date: 2024-11-26FUJIAN SANGANG MINGUANG +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411114291.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The prior art is difficult to effectively increase the nitrogen content in vanadium-containing rebar, resulting in the failure of the steel's mechanical properties to meet the standards, and increasing the amount of vanadium nitrogen alloy will lead to the vanadium content exceeding the control range and increasing production costs.

Method used

By adjusting the process parameters of the converter and LF refining furnace, including controlling the end point temperature and carbon content of the converter, adjusting the nitrogen blowing mode, optimizing the power supply operation of the LF refining furnace and using ferrosilicon nitride alloy, it promotes nitrogen absorption in the molten steel.

Benefits of technology

The nitrogen content in the molten steel is significantly improved, so that it is controlled within the range of 0.012%-0.018%, ensuring that the mechanical properties of the HRB500E series products meet the standards and reducing production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a production process for increasing the nitrogen content in vanadium-containing deformed steel bar, which comprises the following process steps of: adjusting a converter loading system, and organizing production according to the molten iron consumption of 880kg / t; the final temperature of the converter is controlled to be 1600-1630 DEG C, and the final carbon content of the converter is controlled to be 0.06%-0.10%; a continuous blowing mode at the bottom of the converter is adjusted, nitrogen is injected in the whole process, the nitrogen blowing strength before the 60% oxygen step is 0.077 Nm < 3 > / t.mi < n >, and the nitrogen blowing strength from the 60% oxygen step to the end of blowing is 0.054 Nm < 3 > / t.mi < n >; a reblowing mode of the converter is improved, nitrogen is blown into the converter for 1.5 minutes by using an oxygen lance after turning down at the terminal stage, and then tapping operation is carried out; power transmission operation of the LF refining furnace is optimized; and adjusting the use of the silicon nitride iron alloy in the LF refining furnace. According to the method, the nitrogen content in the molten steel can be increased, and the nitrogen content of the produced vanadium-containing deformed steel bar finished product is controlled to be 0.012%-0.018%, so that the nitrogen content is greatly increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a production process for increasing the nitrogen content in vanadium-containing threaded steel. Background Art

[0002] HRB500E series earthquake-resistant steel bars are favored for their high strength and good performance and are widely used in buildings that require high earthquake resistance. Usually, trace elements of vanadium are added to steel to form carbides and nitrides in the steel for precipitation strengthening. However, in comparison, nitrides in steel are more stable than carbides, and nitrides can form a finer and evenly distributed strengthening phase, making the strengthening effect more obvious. Therefore, we need to ensure that the nitrogen content of HRB500E series products is controlled between 0.012% and 0.018%.

[0003] In the conventional production process, vanadium-nitrogen alloy is generally added to molten steel to increase the vanadium and nitrogen content in the molten steel. However, since the vanadium recovery rate is more stable than the nitrogen recovery rate, when the vanadium in the molten steel reaches the internal control requirements of the steel grade, the nitrogen content of the molten steel is less than 0.012%, which may not meet the mechanical properties of the steel. On the other hand, if the amount of vanadium-nitrogen alloy is increased to meet the control requirements of the nitrogen content, it is also easy to cause the vanadium content to exceed the control range, resulting in the scrapping of the steel. At the same time, vanadium-nitrogen alloy is also an expensive metal material, which will increase production costs.

[0004] Therefore, we need to find a way to increase the nitrogen content in molten steel in the process flow of converter, LF refining furnace, etc., and stably enhance the nitrogen content in molten steel, so as to ensure that the mechanical properties of HRB500E series products meet the standards. Summary of the invention

[0005] The object of the present invention is to provide a production process for increasing the nitrogen content in vanadium-containing threaded steel to solve some problems existing in the prior art.

[0006] To achieve the above object, the present invention adopts the following technical solution: a production process for increasing the nitrogen content in vanadium-containing threaded steel, specifically comprising the following process steps:

[0007] Step 1: Adjust the converter charging system and organize production according to the molten iron consumption of 880kg / t to facilitate converter endpoint control and promote nitrogen absorption by molten steel;

[0008] Step 2: Control the converter end temperature at 1600-1630°C, and control the converter end carbon at 0.06%-0.10%;

[0009] Step 3: Adjust the continuous blowing mode at the bottom of the converter, inject nitrogen during the whole process, and the nitrogen blowing intensity before the 60% oxygen step is 0.077Nm3 / t·min, 60% oxygen step to the end of blowing, nitrogen blowing intensity is 0.054Nm 3 / t·min;

[0010] Step 4: Improve the converter re-blowing mode. After the converter is turned down at the final stage, use an oxygen lance to blow nitrogen into the furnace for 1.5 minutes before tapping.

[0011] Step 5: Optimize the power supply operation of the LF refining furnace: When the LF furnace enters the station, open the bypass equipment, adjust the bottom argon flow rate to 500-800NL / min, and adjust the current of the transformer to 30000A to achieve 4-5 times of power supply to promote nitrogen absorption by molten steel;

[0012] Step 6: Adjust the use of ferrosilicon nitride in the LF refining furnace: After the LF refining furnace has refined the same components, add an appropriate amount of ferrosilicon nitride to the ladle according to the standard of 0.0005% nitrogen increase per 10kg ferrosilicon nitride, and perform power supply heating treatment to promote nitrogen increase in molten steel using ferrosilicon nitride.

[0013] In step 4, the nitrogen flow rate during the oxygen lance blowing process is controlled at 28500Nm 3 / h, and the oxygen lance position is maintained at 2.5m.

[0014] After adopting the above technical scheme, compared with the existing technology, it has the following beneficial effects: it can increase the nitrogen content in molten steel, so that the nitrogen content of the produced vanadium-containing threaded steel product is controlled within the ratio of 0.012%-0.018%, which is greatly improved. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0016] In view of the problems existing in the prior art, the present invention provides a production process for increasing the nitrogen content in vanadium-containing threaded steel. The present invention is described in detail below.

[0017] The technical solution adopted in this specific implementation is: a production process for increasing the nitrogen content in vanadium-containing threaded steel, which specifically includes the following process steps:

[0018] Step 1: Optimize the converter loading system and organize production according to the molten iron consumption of 880kg / t to facilitate converter endpoint control and promote nitrogen absorption by molten steel. Specifically, the production method of molten iron consumption of 880kg / t can be adopted to control the molten iron consumption and ensure the stability and accuracy of the converter endpoint, thereby promoting the absorption of nitrogen by molten steel;

[0019] Step 2: Optimize the converter endpoint control target: the converter endpoint temperature is controlled at 1600-1630℃, and the converter endpoint carbon is controlled at 0.06%-0.10%. By controlling the converter endpoint temperature and carbon, the nitrogen content in the molten steel can be effectively controlled to ensure the quality of the molten steel;

[0020] Step 3: Optimize the bottom blowing mode of the converter: nitrogen is blown into the converter bottom blowing throughout the whole process, and the nitrogen blowing intensity before the 60% oxygen step is 0.077Nm 3 / t·min, 60% oxygen step to the end of blowing, nitrogen blowing intensity is 0.054Nm 3 / t·min. By adjusting the nitrogen flow rate in the converter bottom blowing mode, the nitrogen content in the molten steel can be controlled and the continuity and stability of production can be ensured;

[0021] Step 4: Optimize the converter re-blowing mode: After the final furnace is poured, use an oxygen lance to blow nitrogen into the furnace for 1.5 minutes before tapping. The nitrogen flow rate during the nitrogen blowing process is 28500Nm 3 / h, and the oxygen lance position is controlled at 2.5m. By using the oxygen lance to blow nitrogen into the furnace after the final pouring, the nitrogen content in the molten steel can be increased and the production efficiency can be improved;

[0022] Step 5: Optimize the power supply operation of the LF refining furnace: After the LF furnace enters the station, open the bypass, adjust the bottom blowing argon flow rate to 500-800NL / min, adjust the transformer current to 30000A, and supply power 4-5 times to promote the absorption of nitrogen by molten steel. By adjusting the power supply parameters of the LF refining furnace, the absorption of nitrogen by molten steel can be promoted;

[0023] Step 6, optimize the use of ferrosilicon nitride in LF refining furnace: After the LF refining furnace has refined the same components, add ferrosilicon nitride into the ladle according to the nitrogen content of the molten steel and the standard of 0.005% nitrogen increase for 10kg ferrosilicon nitride, and then conduct power supply heating to promote nitrogen increase in the molten steel by using ferrosilicon nitride. By adding an appropriate amount of ferrosilicon nitride into the ladle, the absorption of nitrogen in the molten steel can be promoted.

[0024] The above description is only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in this field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.

Claims

1. A production process for increasing the nitrogen content in vanadium-containing threaded steel, characterized in that: The specific process steps include: Step 1: Adjust the converter charging system and organize production according to the molten iron consumption of 880kg / t to facilitate converter endpoint control and promote nitrogen absorption by molten steel; Step 2: Control the converter end temperature at 1600-1630°C, and control the converter end carbon at 0.06%-0.10%; Step 3: Adjust the continuous blowing mode at the bottom of the converter, inject nitrogen during the whole process, and the nitrogen blowing intensity before the 60% oxygen step is 0.077Nm 3 / t·min, 60% oxygen step to the end of blowing, nitrogen blowing intensity is 0.054Nm 3 / t·min; Step 4: Improve the converter re-blowing mode. After the converter is turned down at the final stage, use an oxygen lance to blow nitrogen into the furnace for 1.5 minutes before tapping. Step 5: Optimize the power supply operation of the LF refining furnace: When the LF furnace enters the station, open the bypass equipment, adjust the bottom argon flow rate to 500-800NL / min, and adjust the current of the transformer to 30000A to achieve 4-5 times of power supply to promote nitrogen absorption by molten steel; Step 6: Adjust the use of ferrosilicon nitride in the LF refining furnace: After the LF refining furnace has refined the same components, add an appropriate amount of ferrosilicon nitride to the ladle according to the standard of 0.0005% nitrogen increase per 10kg ferrosilicon nitride, and perform power supply heating treatment to promote nitrogen increase in molten steel using ferrosilicon nitride.

2. The production process for increasing the nitrogen content in vanadium-containing threaded steel according to claim 1, characterized in that: In step 4, the nitrogen flow rate during the oxygen lance blowing process is controlled at 28500Nm 3 / h, and the oxygen lance position is maintained at 2.5m.

Citation Information

Patent Citations

  • Method for increasing nitrogen content in vanadium-containing steel bar

    CN104673971A

  • Nitrogen increasing and controlling method and manufacturing method of vanadium microalloyed deformed steel bar

    CN112813229A

  • Method for controlling and predicting nitrogen content in molten steel

    CN115505681A

  • Method for nitrogen-enrichment of molten steel covered with slag

    US3230075A

  • Fabrication method for 500 mpa-grade high-strength high-toughness Anti-seismic rebar