Novel plastic die steel material and heat treatment method thereof
Through the new heat treatment process and component optimization, the problem of unstable quality of domestic plastic mold steel was solved, and new plastic mold steel with high hardness and tensile strength was prepared, which met the performance needs of high-end molds, reduced costs and promoted scrap steel Recycling.
Patent Information
- Application Number
- CN202411249325.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-26
AI Technical Summary
The mass fluctuations of domestic plastic mold steel are large, and there are defects such as looseness, primary carbide residues, segregation and inclusions, resulting in uneven mechanical properties and corrosion resistance, which cannot meet the needs of high-end molds, and relying on imported materials leads to high costs.
New heat treatment processes are adopted, including smelting ingots, electroslag remelting, diffusion annealing, ingot hot forging, spherical annealing, quenching and tempering treatment, to optimize the mechanical properties and structural structure of the materials, and control chemical components such as C, Cr, The content of Si, Mn, Mo, V and Ni was prepared with a new type of plastic mold steel material with hardness ≥52HRC and tensile strength ≥2000MPa.
By optimizing the process and composition, the mechanical properties and corrosion resistance of plastic mold steel are significantly improved, production costs are reduced, scrap steel recycling is promoted, high-end mold needs are met, and manufacturing costs are reduced.
Smart Images

Figure CN119020674A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel materials and relates to a new type of plastic mould steel material and a heat treatment method thereof. Background Art
[0002] Under the premise of carbon peak and carbon neutrality, the use of short-process electric furnace smelting to produce steel is considered to be the trend of future steel production. Since electric furnace smelting can use scrap steel on a large scale, and scrap steel, as a strategic resource that can be used almost infinitely, occupies an important position in steel production. In recent years, in order to reduce production costs, many mold factories have used higher-purity alloy waste to achieve high-efficiency and high-value-added recycling of scrap steel.
[0003] With the rapid development of my country's plastic industry and the rise of specialized mold manufacturers, the demand for plastic mold steel has continued to rise, and the performance and quality requirements for steel have also increased. However, my country's research in the field of high-end mold steel has been slow. Most of the domestic high-end molds rely on imports, and the price of imported plastic mold steel is high. Therefore, it is very important to study and develop domestic plastic mold steel and the influence of heat treatment process on its organization and performance. 4Cr13 plastic mold steel is currently a more commonly used plastic mold steel. The mechanical properties require: hardness 48-52HRC, tensile strength 1715-1778MPa. With the gradual development of various products towards large-scale, the development of molds towards large-scale is an inevitable trend. For domestic large module steel, due to factors such as improper forging process and heat treatment process, the quality of domestic module products has fluctuated greatly for a long time, and there are often serious defects such as looseness, primary carbide residue, segregation and inclusions. This kind of organizational unevenness and the hardness and organizational differences at different positions of the module have adverse effects on the mechanical properties and corrosion resistance of the steel. Therefore, on the basis of reducing the cost of plastic mold steel, it is an urgent problem to develop materials that meet the requirements for the use of plastic mold steel and reduce the manufacturing cost of the mold industry. Summary of the invention
[0004] In view of the deficiencies of the prior art, the primary purpose of the present invention is to provide a new heat treatment process for plastic mold steel materials, which can effectively optimize the mechanical properties of the material, adjust the organizational structure, and improve the distribution and uniformity of carbides.
[0005] The second object of the present invention is to provide a new type of plastic mold steel material prepared by the above heat treatment process. The new type of plastic mold steel material has mechanical properties of hardness ≥ 52HRC and tensile strength ≥ 2000MPa.
[0006] The primary purpose of the present invention is achieved through the following technical solutions:
[0007] A new type of heat treatment process for plastic mold steel material includes the following steps:
[0008] (1) Smelting ingots: placing waste steel in an electric arc furnace to smelt into ferrochrome alloy molten iron, controlling the temperature in the electric arc furnace to be 1550-1600° C., transferring the molten iron into a refining furnace for refining after tapping, controlling the temperature in the refining furnace to be 1550-1600° C., alloying the molten iron to form molten steel, and injecting it into a mold to prepare a refined mold steel ingot;
[0009] (2) electroslag remelting: subjecting the refined steel ingot obtained in step (1) to electroslag remelting to obtain an ingot;
[0010] (3) Diffusion annealing: After the electroslag is finished, it is placed in a high-temperature annealing furnace and heated to 1200-1250°C for 3-5 hours until the primary carbides and banded structures in the ingot disappear, and the primary ingot product is obtained;
[0011] (3) Ingot hot forging: The initial ingot product in step (2) is heated to 1130-1170°C, kept warm for 2-5 hours, the initial forging temperature is 1100-1170°C, the final forging temperature is 850°C, and slowly cooled after forging to obtain a square billet of the required size, i.e., the initial product of the new plastic mold steel material;
[0012] (4) Post-forging heat treatment: The square billet obtained in step (3) is subjected to spheroidizing annealing, quenching and tempering treatment in sequence to prepare a new type of plastic mold steel material.
[0013] Preferably, the spheroidizing annealing in step (4) is specifically as follows: heating the square billet obtained in step (3) to 870-890°C and keeping it at that temperature for 0.5-1h, then cooling it to 690-710°C at a rate of 100-120°C / h and keeping it at that temperature for 4-6h, then cooling it to below 500°C, and air cooling it to room temperature after it is taken out of the furnace.
[0014] Preferably, the quenching in step (4) is specifically as follows: heating the billet after spheroidizing annealing to 1030-1050° C., keeping the temperature for 0.5-1 h, and oil quenching.
[0015] Preferably, the tempering in step (4) is specifically as follows: the quenched billet is tempered twice at a tempering temperature of 150-250° C. for 2-4 hours, and then air-cooled to room temperature after being taken out of the furnace.
[0016] The second object of the present invention is achieved by the following technical solutions:
[0017] A new type of plastic mold steel material is prepared by the above heat treatment process.
[0018] Preferably, the new plastic mold steel material comprises the following components in mass percentage: C 0.50%-0.60%, Cr 14.00%-16.00%, Mn 0.20%-0.50%, Si 0.10%-0.30%, Mo 0.05%-1.00%, V 0.05%-0.20%, Ni 0.10%-0.30%, P≤0.03%, S≤0.03%, and the balance Fe.
[0019] Preferably, the novel plastic mold steel material comprises the following raw materials in percentage by mass: C 0.55%, Cr14.96%, Mn 0.44%, Si 0.16%, Mo 0.10%, V 0.11%, Ni 0.20%, P 0.001%, S 0.001%, and the balance Fe.
[0020] Preferably, the novel plastic mold steel material comprises the following raw materials in percentage by mass: C 0.52%, Cr14.53%, Mn 0.44%, Si 0.16%, Mo 0.13%, V 0.10%, Ni 0.21%, P 0.005%, S 0.002%, and the balance Fe.
[0021] Preferably, the novel plastic mold steel material comprises the following raw materials in percentage by mass: C 0.53%, Cr14.55%, Mn 0.42%, Si 0.17%, Mo 0.15%, V 0.11%, Ni 0.21%, P 0.005%, S 0.002%, and the balance Fe.
[0022] Preferably, the properties of the new plastic mold steel material are as follows: hardness>52HRC, tensile strength≥2000MPa.
[0023] The components and functions of the various elements of the new plastic mold steel material of the present invention are as follows:
[0024] Carbon (C) is one of the most important elements in steel. The solubility of C in steel decreases as the content of Cr increases, and the strength of steel is improved in the form of interstitial solid solution. Under appropriate processes, an appropriate amount of C content produces fine carbon-rich phases, which is beneficial to improving the corrosion resistance of steel. However, if the C content is too high, the toughness of the steel will be reduced, while if the carbon content is too low, the strength of the steel will be reduced. Therefore, the C content of the present invention is in the range of 0.50-0.60%.
[0025] Chromium (Cr) as the main alloying element in plastic mold steel can not only improve the hardenability of steel, increase hardness and wear resistance, but also is the main element forming the passivation film on the surface of plastic mold steel, increase the corrosion potential of the steel matrix, and improve the corrosion resistance of steel. As the Cr content in the alloy steel increases, the corrosion rate also decreases. Therefore, the Cr content in the present invention is in the range of 14.00-16.00%.
[0026] Silicon (Si) is an effective solid solution strengthening element in steel, which improves the hardness of steel. Si can play a deoxidizing role during steelmaking and is a commonly used deoxidizer. Its concentration usually does not exceed 0.3wt.%. Since Si is easy to segregate at austenite grain boundaries, it reduces the grain boundary bonding force and causes brittleness. At the same time, Si is easy to cause element segregation in steel. Therefore, the Si content in the present invention is controlled at 0.10%-0.30%.
[0027] Manganese (Mn) is an alloy deoxidizer and desulfurizer in the smelting process, which can ensure that the steel is quenched at a wide cooling rate to obtain a martensitic structure. Mn can form MnS with S in the steel, thereby reducing the harmful effect of S on the steel. At the same time, due to the presence of high melting point sulfides, the addition of a small amount of Mn improves the high temperature machinability of the steel. Therefore, the content of Mn in the present invention is in the range of 0.20-0.50%.
[0028] Molybdenum (Mo) can improve the hardenability of steel. At a higher tempering temperature, it forms dispersed special carbides, which play a role in secondary hardening. A certain content of Mo can not only increase the strength and toughness, but also increase the corrosion resistance of steel. However, too high a Mo content causes a large amount of delta-ferrite to appear in the structure after quenching, which reduces the mechanical properties of the mold steel. Therefore, the content of Mo in the present invention is in the range of 0.05-1.00%.
[0029] Vanadium (V) is a strong carbide-forming element, which forms a hard phase with C to improve the wear resistance and corrosion resistance of the material. However, V is a strong ferrite stabilizer, and excessive V content reduces the strength and ductility of the matrix. Therefore, the V content in the present invention is in the range of 0.05-0.20%.
[0030] Nickel (Ni), as an austenite stabilizing element, can improve the hardenability and structural uniformity of plastic mold steel, thereby improving its mechanical properties and improving the polishing performance of steel. Therefore, the Ni content in the present invention is in the range of 0.10-0.30%.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] (1) The new plastic mold steel material provided by the present invention controls the chemical composition and dosage of the steel so that its performance can meet the requirements of plastic mold steel. At the same time, a high proportion of scrap steel is utilized, which greatly promotes the recycling of scrap steel and reduces production costs.
[0033] (2) The present invention sequentially undergoes the processes of electric furnace smelting, refining outside the furnace, homogenization annealing, electroslag remelting, forging, spheroidizing annealing, quenching and secondary tempering, so that the prepared new plastic mold steel material has mechanical properties of hardness ≥52HRC and tensile strength ≥2000MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a metallographic image of spheroidal carbide particles formed after spheroidizing annealing of the new plastic mold steel material in Example 3;
[0035] Figure 2 This is the SEM microstructure of the new plastic mold steel material in Example 3 after quenching;
[0036] Figure 3 This is the SEM microstructure of the new plastic mold steel material in Example 3 after tempering. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0038] The chemical compositions of Examples 1 to 3 of the present invention are shown in Table 1, and the specific processing technology of the new plastic mold steel material is as follows:
[0039] (1) Smelting ingots: smelting ferrochrome alloy molten iron in an electric arc furnace, and maintaining the molten iron temperature within the temperature range of the ferrochrome alloy molten iron required for entering the refining furnace. After tapping, the molten iron is transferred to the refining furnace for refining, alloying and temperature control operations are performed, and the molten steel is tapped at a temperature of 1550-1600°C. The molten steel is poured into an ingot mold to obtain a refined mold steel ingot;
[0040] (2) Electroslag remelting: The obtained steel ingot is subjected to electroslag remelting to reduce the influence of harmful elements and inclusions in the steel, improve the ingot structure, and enhance the purity and performance of the metal material;
[0041] (3) Diffusion annealing: The steel ingot is placed in a high-temperature annealing furnace and heated from room temperature to 1200-1250°C for 3-5 hours to make the primary carbides and banded structures disappear;
[0042] (4) Ingot hot forging: The refined steel ingot is first heated to 1130-1170℃, kept warm for 2-5h, the starting forging temperature is 1100-1170℃, the final forging temperature is 850℃, and slowly cooled after forging to obtain a square billet of the required size.
[0043] (5) Heat treatment after forging:
[0044] Spheroidizing annealing: heat to 870-890℃ and keep warm for 0.5-1h, then cool to 690-710℃ and keep warm for 4-6h, then cool to below 500℃, take out of the furnace and air cool to room temperature.
[0045] Quenching: heat to 1030-1050℃ and keep warm for 0.5-1h, then oil quench.
[0046] Tempering: Tempering is carried out immediately after quenching, the tempering temperature is 150-250℃, keep warm for 2-4h, take out of the furnace and air cool to room temperature, temper twice.
[0047] The actual performance test results of Examples 1 to 3 of the present invention are shown in Table 2.
[0048] Room temperature tensile test The room temperature tensile properties of materials are tested according to GB / T 228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method".
[0049] The Rockwell hardness test is carried out according to GB / T230.1-2018 "Metal Rockwell hardness test Part 1: Test method" to test the Rockwell hardness of the material.
[0050] See also Figure 1-3 . Figure 1 The spheroidal carbide particles are formed after the new plastic mold steel material in Example 3 of the present invention is spheroidized and annealed. Figure 1 It can be seen that the annealed carbides are small and evenly distributed. Figure 2 This is the SEM organization diagram of the new plastic mold steel material after quenching in Example 3 of the present invention. It can be seen that there is a small amount of precipitation phase in the coarse lath martensite. Figure 3 This is the SEM organization diagram of the new plastic mold steel material after secondary tempering in Example 3 of the present invention. It can be observed that there are many carbides on the matrix, which is very helpful to improve the mechanical properties of the material.
[0051] Table 1 shows the composition (wt.%) of the new plastic mold steel material prepared in Examples 1 to 3
[0052]
[0053] Table 2 is the test results of the new plastic mold steel materials prepared in Examples 1 to 3
[0054]
[0055] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A new type of heat treatment process for plastic mold steel material, characterized in that: The following steps are included: (1) Smelting ingots: placing waste steel in an electric arc furnace to smelt into ferrochrome alloy molten iron, controlling the temperature in the electric arc furnace to be 1550-1600° C., transferring the molten iron into a refining furnace for refining after tapping, controlling the temperature in the refining furnace to be 1550-1600° C., alloying the molten iron to form molten steel, and injecting it into a mold to prepare a refined mold steel ingot; (2) electroslag remelting: subjecting the refined steel ingot obtained in step (1) to electroslag remelting to obtain an ingot; (3) Diffusion annealing: After the electroslag is finished, it is placed in a high-temperature annealing furnace and heated to 1200-1250°C for 3-5 hours until the primary carbides and banded structures in the ingot disappear, and the primary ingot product is obtained; (3) Ingot hot forging: The initial ingot product in step (2) is heated to 1130-1170°C, kept warm for 2-5 hours, the initial forging temperature is 1100-1170°C, the final forging temperature is 850°C, and slowly cooled after forging to obtain a square billet of the required size, i.e., the initial product of the new plastic mold steel material; (4) Post-forging heat treatment: The square billet obtained in step (3) is subjected to spheroidizing annealing, quenching and tempering treatment in sequence to prepare a new type of plastic mold steel material.
2. The heat treatment process of the new plastic mold steel material according to claim 1 is characterized in that: The spheroidizing annealing in step (4) is specifically as follows: heating the square billet obtained in step (3) to 870-890°C and keeping the temperature for 0.5-1h, then cooling it to 690-710°C at a rate of 100-120°C / h and keeping the temperature for 4-6h, then cooling it to below 500°C, and air cooling it to room temperature after it is taken out of the furnace.
3. The heat treatment process of the new plastic mold steel material according to claim 1 is characterized in that: The quenching in step (4) is specifically as follows: heating the spheroidizing annealed billet to 1030-1050° C., keeping the temperature for 0.5-1 h, and oil quenching.
4. The heat treatment process of the new plastic mold steel material according to claim 1 is characterized in that: The tempering in step (4) is specifically as follows: the quenched billet is tempered twice at a tempering temperature of 150-250° C. for 2-4 hours, and then air-cooled to room temperature after being taken out of the furnace.
5. A new type of plastic mold steel material, characterized in that: Prepared according to the heat treatment process according to any one of claims 1 to 4.
6. The new plastic mold steel material according to claim 5, characterized in that: The steel comprises the following components in mass percentage: C 0.50%-0.60%, Cr 14.00%-16.00%, Mn 0.20%-0.50%, Si 0.10%-0.30%, Mo 0.05%-1.00%, V 0.05%-0.20%, Ni 0.10%-0.30%, P≤0.03%, S≤0.03%, and the balance is Fe.
7. The new plastic mold steel material according to claim 5, characterized in that: The invention comprises the following raw materials in percentage by mass: C 0.55%, Cr 14.96%, Mn 0.44%, Si 0.16%, Mo 0.10%, V 0.11%, Ni 0.20%, P 0.001%, S 0.001%, and the balance Fe.
8. The new plastic mold steel material according to claim 5, characterized in that: The invention comprises the following raw materials in percentage by mass: C 0.52%, Cr 14.53%, Mn 0.44%, Si 0.16%, Mo 0.13%, V 0.10%, Ni 0.21%, P 0.005%, S 0.002%, and the balance Fe.
9. The new plastic mold steel material according to claim 5, characterized in that: The invention comprises the following raw materials in percentage by mass: C 0.53%, Cr 14.55%, Mn 0.42%, Si 0.17%, Mo 0.15%, V 0.11%, Ni 0.21%, P 0.005%, S 0.002%, and the balance Fe.
10. The new plastic mold steel material according to any one of claims 5 to 9, characterized in that: The properties of the new plastic mold steel material are as follows: hardness>52HRC, tensile strength≥2000MPa.