Ultrafine-grain low-cost 500Mpa-grade building wire and preparation method thereof

By adjusting chemical composition and process design in the production of 500Mpa grade building wires, ultra-fine crystal wires with high yield strength and strong yield ratio are achieved, solving the problems of high cost and unreasonable metallographic structure, and meeting the seismic building performance and cost reduction requirements.

CN119020700AInactive Publication Date: 2024-11-26HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410990624.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing 500Mpa-grade construction wire production process, the large amount of alloy elements has led to high production costs, and the rolling and cooling process design is unreasonable, making it difficult to meet the metallographic structure requirements of the new national standard, and bainite and martensite are prone to occur. Overcooling tissue, the risk of being incompatible with the failure of the strong.

Method used

Using low-cost chemical composition and process design, the nitrogen content is increased in moderation by reducing the content of manganese, vanadium, niobium, and titanium alloys, and the ferrite and pearlite structure are controlled through reasonable controlled rolling and fast cooling technology of large air volume. Ultra-refining, substituting for precipitation strengthening of microalloy elements, achieving high yield strength and strong yield ratio.

Benefits of technology

With the addition of a small amount of microalloy elements, a high yield strength and strong yield ratio of more than 500Mpa were obtained, and the total elongation of the maximum force was ≥10%, which met the requirements of seismic building performance, while reducing production costs. It is ferrite and pearlite, without bainite or martensite supercooled structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The invention discloses an ultra-fine grain low-cost 500 Mpa grade building wire and a preparation method thereof. The wire comprises the following chemical components: 0.20%-0.25% of C, 0.40%-0.60% of Si, 1.00%-1.25% of Mn, less than or equal to 0.035% of P, less than or equal to 0.035% of S, 0.010%-0.025% of V, 0.0090%-0.0120% of N and the balance of iron and inevitable impurity elements. The preparation method comprises the steps of steelmaking, continuous casting, heating, wire rolling and wire cooling. According to the invention, the low-temperature controlled rolling and large-air-volume rapid cooling process is adopted, an ultrafine ferrite and pearlite structure is obtained, through grain ultrafine control, under the condition that only a small amount of microalloy elements are added, the yield strength of the building wire is greater than or equal to 530 Mpa, the strength-to-yield ratio is greater than or equal to 1.26, the maximum force total elongation is greater than or equal to 10%, the requirements of anti-seismic building performance are met, and the production cost is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel production, and in particular relates to an ultrafine-grained low-cost 500Mpa-level building wire and a preparation method thereof. Background Art

[0002] At present, the 500Mpa-grade construction wire produced by steel enterprises mainly adopts the method of adding niobium, vanadium and titanium microalloy elements to improve the strength. The rolling and cooling process does not carry out special controlled rolling and controlled cooling design, resulting in a large amount of alloy addition and high production costs. From the perspective of sustainable development of national strategic resources, it is also uneconomical. Therefore, it is urgent to develop a new production process for low-cost 500Mpa-grade construction steel.

[0003] With the formulation and implementation of the new national standard GB / T 1499.2 for construction steel in 2018, the standard clearly requires that the metallographic structure be ferrite plus pearlite, and tempered martensite is basically not allowed to appear, which puts forward strict requirements on the structure of rolled materials. For small-sized construction wire rods, if the rolling and cooling process design is unreasonable, bainite and martensite supercooling structures are very likely to appear, making it difficult to meet the standard requirements. In addition, although controlled rolling and controlled cooling can further refine the grains, the refinement of the grains will reduce the strength-to-yield ratio, and there is a risk of the strength-to-yield ratio not being suitable. Therefore, while considering low cost, it is also necessary to focus on the above possible problems and find a reasonable process window. Summary of the invention

[0004] In view of the above problems, the present invention discloses an ultrafine-grained, low-cost 500Mpa-grade building wire and a preparation method thereof. By adding only a small amount of micro-alloy elements, the building wire with a high yield strength of more than 500Mpa, a strength-to-yield ratio ≥1.26, and a maximum force total elongation ≥10% is obtained, which meets the performance requirements of earthquake-resistant buildings and greatly reduces the production cost.

[0005] To solve the above problems, the present invention adopts the following technical solutions: The invention discloses an ultrafine-grained low-cost 500Mpa-level building wire material, whose chemical composition and mass percentage are as follows: C: 0.20-0.25%, Si: 0.40-0.60%, Mn: 1.00-1.25%, P≤0.035%, S≤0.035%, V: 0.010-0.025%, N: 0.0090-0.0120%, and the rest are iron and unavoidable impurity elements.

[0006] Furthermore, the structures of the construction wires described in the present invention are all ferrite and pearlite, without bainite and martensite supercooled structures; the average ferrite grain size is 3.6-5.5um, and the grain size grade is 12-13.

[0007] Furthermore, the yield strength of the construction wire material of the present invention is ≥530Mpa, the tensile strength is ≥690Mpa, the strength-to-yield ratio is ≥1.26, and the total elongation at maximum force is ≥10%, which meets the performance requirements of earthquake-resistant buildings.

[0008] The method for preparing the ultrafine-grained low-cost 500Mpa-level construction wire of the present invention comprises the steps of steelmaking, continuous casting, heating, wire rolling and wire cooling.

[0009] Furthermore, in the continuous casting process of the present invention, the superheat degree is 15-40°C, the steel drawing speed is 2.8-3.0 m / min, and the cross-sectional size of the ingot is 150*150 mm.

[0010] Furthermore, in the heating process of the present invention, the heating temperature is 1120-1160° C. and the heating time is 90-120 min.

[0011] Furthermore, in the wire rolling process of the present invention, after the steel billet is heated, it is sequentially subjected to rough rolling, intermediate rolling, finishing rolling, final rolling, and wire drawing. After the rolling is completed, the required 8mm / 10mm diameter construction wire is achieved.

[0012] Furthermore, in the wire rolling process of the present invention, the final rolling temperature is 860-890°C, and the wire laying temperature is 850-880°C.

[0013] Furthermore, in the wire cooling process of the present invention, all the heat preservation covers are opened, and fans 1# to 4# are turned on, with the air volume of the fans increased by 30% to 60%, wherein the rated air volume of a single fan is 200,000m 3 / h.

[0014] The inventive principle of the present invention is: The wire material of the present invention mainly reduces and lowers the content of manganese, vanadium, niobium and titanium alloy elements in terms of chemical composition, and appropriately increases the nitrogen content to further improve the precipitation strengthening effect of vanadium. In terms of process, the phase change time is reduced mainly through reasonable control of rolling and large air volume rapid cooling process, and ultra-fine ferrite and pearlite structures are obtained. The material strength is improved through fine grain strengthening, and the precipitation strengthening of microalloying elements is replaced by fine grain strengthening to achieve the purpose of reducing microalloying elements.

[0015] The beneficial effects of the present invention are: The present invention adopts low-temperature controlled rolling and large air volume rapid cooling process to obtain ultra-fine ferrite and pearlite structures. Through ultra-fine grain control, a high yield strength of more than 500Mpa is obtained by adding only a small amount of microalloy. Compared with ordinary production processes, the addition amount of microalloy elements such as Nb, V, and Ti can be saved, and the production cost can be greatly reduced.

[0016] The present invention adopts reasonable composition and controlled rolling and controlled cooling design, and finds a suitable process window through a large number of experiments. While ensuring that ultrafine grains obtain high strength, the strength-to-yield ratio is ≥1.26, the maximum force total elongation is ≥10%, and the metallographic structure is ferrite plus pearlite, without bainite martensite supercooling structure, which meets the seismic performance and metallographic structure requirements of construction steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the metallographic structure of the construction wire material of Example 1.

[0018] Figure 2 The metallographic structure of the construction wire material in Example 2 DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1

[0020] An ultrafine-grained, low-cost 500Mpa-grade construction wire, the chemical composition of which is: C: 0.20%, Si: 0.45%, Mn: 1.25%, P: 0.030%, S: 0.035%, V: 0.020%, N: 0.0100%, and the rest is iron and unavoidable impurity elements; the preparation method thereof includes steelmaking, continuous casting, heating, wire rolling, and wire cooling processes, wherein the key control parameters are as follows: (1) Smelting is performed according to the above composition, and then continuous casting is performed according to the following parameters: superheat 30°C, drawing speed 3.0 m / min, and continuous casting is performed into square billets with a cross-sectional size of 150*150 mm.

[0021] (2) The billet is heated at a temperature of 1150°C for 110 min.

[0022] (3) After the billet is heated, it undergoes rough rolling, intermediate rolling, finishing rolling, final rolling and wire drawing in sequence. After the rolling is completed, the required 8mm diameter construction wire is achieved. The final rolling temperature is 880℃, the wire drawing temperature is 870℃, the insulation covers are all opened, and the 1#~4# fans are turned on. The fan air volume is opened by 30-40%, and the rated air volume of a single fan is 200000m3 / h.

[0023] The wire material of this embodiment has a yield strength of 565 MPa, a tensile strength of 715 MPa, a strength-to-yield ratio of 1.26, a maximum force total elongation of 12%, and a metallographic structure of ultra-fine ferrite and pearlite, wherein the average ferrite grain size is 3.6 μm, the grain size grade is 13, and there is no bainite and martensite supercooled structure. Figure 1 As shown, both the performance and microstructure meet the requirements of earthquake-resistant building standards. Example 2

[0024] An ultrafine-grained, low-cost 500Mpa-grade building wire, the chemical composition of which is: C: 0.25%, Si: 0.40%, Mn: 1.10%, P: 0.035%, S: 0.030%, V: 0.010%, N: 0.0090%, and the rest is iron and unavoidable impurity elements; the preparation method thereof includes steelmaking, continuous casting, heating, wire rolling, and wire cooling processes, wherein the key control parameters are as follows: (1) Smelting is performed according to the above composition, and then continuous casting is performed according to the following parameters: superheat 40°C, drawing speed 2.8 m / min, and continuous casting is performed into square billets with a cross-sectional size of 150*150 mm.

[0025] (2) The billet is heated at a temperature of 1160°C for 120 min.

[0026] (3) After the billet is heated, it undergoes rough rolling, intermediate rolling, finishing rolling, final rolling and wire drawing in sequence. After the rolling is completed, the required 10 mm diameter construction wire is achieved. The final rolling temperature is 890 ° C, the wire drawing temperature is 880 ° C, the insulation covers are all opened, and the 1#~4# fans are turned on. The fan air volume is opened at 50~60%, and the rated air volume of a single fan is 200000m3 / h.

[0027] The yield strength of the building wire in this embodiment is 540Mpa, the tensile strength is 690Mpa, the strength-to-yield ratio is 1.28, the maximum force total elongation is 15%, and the metallographic structure is ultra-fine ferrite and pearlite structure, wherein the average ferrite grain size is 5.5um, the grain size grade is 12, and there is no bainite and martensite supercooling structure, such as Figure 2 As shown, the performance and microstructure meet the standard requirements for earthquake-resistant building steel. Example 3

[0028] An ultrafine-grained, low-cost 500Mpa-grade building wire, the chemical composition of which is: C: 0.23%, Si: 0.60%, Mn: 1.00%, P: 0.030%, S: 0.030%, V: 0.025%, N: 0.0120%, and the rest is iron and unavoidable impurity elements; the preparation method thereof includes steelmaking, continuous casting, heating, wire rolling, and wire cooling processes, wherein the key control parameters are as follows: (1) The above composition is used for smelting, and then continuous casting is carried out according to the following parameters: superheat of 15°C, drawing speed of 2.9 m / min, and continuous casting into square billets with a cross-sectional size of 150*150 mm.

[0029] (2) The billet is heated at a temperature of 1140°C for 90 min.

[0030] (3) After the billet is heated, it undergoes rough rolling, intermediate rolling, finishing rolling, final rolling and wire drawing in sequence. After the rolling is completed, the required 8mm diameter construction wire is achieved. The final rolling temperature is 860℃, the wire drawing temperature is 850℃, the insulation covers are all opened, and the 1#~4# fans are turned on. The fan air volume is opened by 30-40%, and the rated air volume of a single fan is 200000m3 / h.

[0031] The wire of this embodiment has a yield strength of 570Mpa, a tensile strength of 725Mpa, a strength-to-yield ratio of 1.27, and a maximum force total elongation of 13%. The metallographic structure is ultra-fine ferrite and pearlite structure, wherein the average ferrite grain size is 4.0um, the grain size level is 13, there is no bainite and martensite undercooling structure, and the performance and microstructure meet the requirements of earthquake-resistant building standards. Example 4

[0032] An ultrafine-grained, low-cost 500Mpa-grade construction wire, the chemical composition of which is: C: 0.21%, Si: 0.50%, Mn: 1.20%, P: 0.028%, S: 0.027%, V: 0.015%, N: 0.0100%, and the rest is iron and unavoidable impurity elements; the preparation method thereof includes steelmaking, continuous casting, heating, wire rolling, and wire cooling processes, wherein the key control parameters are as follows: (1) The above composition is used for smelting, and then continuous casting is carried out according to the following parameters: superheat of 25°C, drawing speed of 2.8 m / min, and continuous casting into square billets with a cross-sectional size of 150*150 mm.

[0033] (2) The billet is heated at a temperature of 1120°C for 100 min.

[0034] (3) After the billet is heated, it undergoes rough rolling, intermediate rolling, finishing rolling, final rolling and wire drawing in sequence. After the rolling is completed, the required 10mm diameter construction wire is achieved. The final rolling temperature is 870℃, the wire drawing temperature is 860℃, the insulation covers are all opened, and the 1#~4# fans are turned on. The fan air volume is opened by 40-50%, and the rated air volume of a single fan is 200000m3 / h.

[0035] The building wire material of this embodiment has a yield strength of 530 MPa, a tensile strength of 690 MPa, a strength-to-yield ratio of 1.30, a maximum force total elongation of 16%, and a metallographic structure of ultra-fine ferrite and pearlite structure, wherein the average ferrite grain size is 5.4 um, the grain size grade is 12, and there is no bainite and martensite supercooling structure. Both the performance and microstructure meet the standard requirements for earthquake-resistant building steel.

[0036] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An ultra-fine-grained, low-cost 500Mpa-grade building wire, characterized in that: Its chemical composition and its mass percentage are: C: 0.20-0.25%, Si: 0.40-0.60%, Mn: 1.00-1.25%, P≤0.035%, S≤0.035%, V: 0.010-0.025%, N: 0.0090-0.0120%, and the rest are iron and unavoidable impurity elements.

2. The ultra-fine-grained, low-cost 500Mpa-grade building wire according to claim 1, characterized in that: The structures of the construction wires are ferrite and pearlite, without bainite and martensite supercooled structures; the average ferrite grain size is 3.6-5.5um, and the grain size grade is 12-13.

3. The ultra-fine-grained, low-cost 500Mpa-grade building wire according to claim 1, characterized in that: The yield strength of the construction wire is ≥530Mpa, the tensile strength is ≥690Mpa, the strength-to-yield ratio is ≥1.26, and the total elongation at maximum force is ≥10%.

4. A method for preparing ultrafine-grained low-cost 500Mpa-grade building wire according to any one of claims 1 to 3, characterized in that: It includes steelmaking, continuous casting, heating, wire rolling and wire cooling processes.

5. The method for preparing an ultrafine-grained low-cost 500Mpa-grade building wire according to claim 4, characterized in that: In the continuous casting process, the superheat degree is 15 to 40° C. and the steel drawing speed is 2.8 to 3.0 m / min.

6. The method for preparing the ultrafine-grained low-cost 500Mpa-grade building wire according to claim 4, characterized in that: In the heating process, the heating temperature is 1120-1160° C. and the heating time is 90-120 min.

7. The method for preparing ultrafine-grained low-cost 500Mpa-grade building wire according to claim 4, characterized in that: In the wire rolling process, after the steel billet is heated, it undergoes rough rolling, intermediate rolling, finishing rolling, final rolling and wire drawing in sequence. After the rolling is completed, the construction wire with the required diameter is achieved.

8. A method for preparing ultrafine-grained low-cost 500Mpa-grade building wire according to claim 4 or 7, characterized in that: In the wire rolling process, the final rolling temperature is 860-890°C and the wire drawing temperature is 850-880°C.

9. The method for preparing ultrafine-grained low-cost 500Mpa-grade building wire according to claim 4, characterized in that: The wire diameter is 8 to 10 mm.

10. The method for preparing ultrafine-grained low-cost 500Mpa-grade building wire according to claim 4, characterized in that: In the wire cooling process shown in the figure, all the heat preservation covers are opened, and fans 1# to 4# are turned on, with the air volume of the fans increased by 30% to 60%. The rated air volume of a single fan is 200,000m 3 / h.

Citation Information

Patent Citations

  • HRB500 and HRB500E coiled reinforcing steel bar production process

    CN103225043A

  • 500 MPa-grade V-containing micro-alloyed high-strength-yield-ratio anti-seismic steel bar wire rod and production method thereof

    CN109468534A

  • 500Mpa coiled steel bar and preparation method thereof

    CN110408843A

  • Low-carbon high-strength hot rolling wire with compound reinforced ultrafine grains and its production process

    CN1654695A

  • Ultra-high-strength reinforcing bar and manufacturing method thereof

    US20220364194A1