Anthraquinone grafted modified carbon-based composite material, preparation method thereof and application of anthraquinone grafted modified carbon-based composite material in electrosynthesis of hydrogen peroxide

Through the anthraquinone grafting modified carbon-based composite material, the diazotization reaction between aminoanthraquinone and carbon-based material is used to form a covalent bond, which solves the problem of degradation of catalytic performance of traditional carbon-based catalysts under high current density, and achieves high efficiency The electrocatalytic oxygen reduction and hydrogen peroxide selectivity are suitable for industrial production.

CN119020804APending Publication Date: 2024-11-26ZHEJIANG YIPAI TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411133121.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The traditional anthraquinone method produces hydrogen peroxide with safety risks and the energy efficiency drops sharply under high current density. The catalytic performance of carbon-based catalysts deteriorates due to positive and negative ion crystallization reactions.

Method used

Anthraquinone grafted modified carbon-based composite materials are used to form stable covalent bonds through diazotization reaction between aminoanthraquinone and carbon-based materials, avoid positive and negative ion crystallization, and enhance the activity and selection of electrocatalytic oxygen reduction to synthesize hydrogen peroxide. sex.

Benefits of technology

It significantly improves the electrocatalytic oxygen reduction activity and selectivity of carbon-based materials, extends the catalytic performance, is suitable for large-scale industrial production, and is suitable for improving the catalytic performance of powder carbon materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020804A_ABST
    Figure CN119020804A_ABST
Patent Text Reader

Abstract

The invention provides an anthraquinone grafted modified carbon-based composite material, a preparation method thereof and application of the anthraquinone grafted modified carbon-based composite material in electrosynthesis of hydrogen peroxide, and belongs to the technical field of electrocatalysis. The preparation method comprises the following steps: adsorbing amino-anthraquinone on the surface of a carbon-based material by adopting a physical impregnation method; and then promoting the anthraquinone group to be grafted to the surface of the carbon-based material through an in-situ diazotization reaction. Stable covalent bonds are formed through diazotization reaction, high-activity anthraquinone groups are grafted to the surface of a carbon-based material, the grafted modified carbon-based composite material is obtained, and the activity and selectivity of the grafted modified carbon-based composite material for synthesizing hydrogen peroxide through electro-catalytic oxygen reduction can be remarkably improved. The grafting modification method disclosed by the invention is simple to operate, efficient, high in controllability and suitable for large-scale batch production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrocatalysis, and in particular to an anthraquinone grafted modified carbon-based composite material, a preparation method thereof, and an application of the composite material in electrosynthesis of hydrogen peroxide. Background Art

[0002] Hydrogen peroxide has now become one of the most important chemicals. The traditional high-energy consumption and high-pollution anthraquinone method for producing hydrogen peroxide is still the current mainstream industrial technology, but this technical route has great safety risks. Therefore, the development of an energy-saving, environmentally friendly and safe alternative technology has become a research hotspot. At present, the most promising large-scale industrial application technology is electrochemical synthesis technology, that is, direct synthesis of hydrogen peroxide (O 2 +2H 2 O+2e - →H 2 O 2 +2OH - ). The hydrogen peroxide produced by this technology is not only of very high purity, but also can be produced in a mobile manner, greatly reducing its transportation costs and storage risks.

[0003] For electrosynthesis of hydrogen peroxide technology, its energy efficiency depends largely on the electrocatalytic activity and hydrogen peroxide selectivity of the cathode catalyst. So far, carbon-based catalysts have attracted much attention due to their high selectivity, stability, conductivity and low cost. For example, graphite / carbon felt electrodes with high specific surface area are widely used as cathode catalysts for electrosynthesis of hydrogen peroxide. Under low current density conditions (~30mA / cm 2 ), this electrode shows excellent energy efficiency, but its energy efficiency drops sharply as the current density increases. The early Chinese patent CN94107429.3 (production method of alkaline hydrogen peroxide aqueous solution) proposed the use of anthraquinone sulfonate anions and quaternary ammonium salt cations as cathode catalysts. This homogeneous catalyst can be adsorbed on the surface of carbon felt, greatly improving the working current density of the electrolyzer. However, during the reaction process, the anthraquinone sulfonate anions and quaternary ammonium salt cations undergo a crystallization reaction, precipitating needle-shaped crystals, accumulating in the pores, blocking the carbon felt electrode, and degrading its catalytic performance. Summary of the invention

[0004] The object of the present invention is to provide an anthraquinone grafted modified carbon-based composite material and a preparation method thereof and application in the electrosynthesis of hydrogen peroxide. The anthraquinone grafted modified carbon-based composite material has excellent electrocatalytic oxygen reduction synthesis of hydrogen peroxide activity and selectivity.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing anthraquinone grafted modified carbon-based composite material, comprising the following steps:

[0007] The carbon-based material is mixed with an aminoanthraquinone compound solution and adsorbed to obtain an aminoanthraquinone-carbon-based material composite;

[0008] The aminoanthraquinone-carbon-based material composite is mixed with a diazo chemical reagent to perform a diazotization reaction to obtain an anthraquinone grafted modified carbon-based composite material;

[0009] The carbon-based material includes graphite felt or carbon-based powder material.

[0010] Preferably, the carbon-based powder material includes one or more of conductive carbon black, graphite and carbon nanotubes.

[0011] Preferably, the aminoanthraquinone compound in the aminoanthraquinone compound solution includes one or more of 1-aminoanthraquinone, 2-aminoanthraquinone, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone and 2,6-diaminoanthraquinone.

[0012] Preferably, the concentration of the aminoanthraquinone compound solution is 0.1-0.5 mol / L.

[0013] Preferably, the adsorption temperature is 25° C. and the adsorption time is 6 to 18 hours.

[0014] Preferably, the preparation method of the diazo chemical reagent comprises: mixing an acid, sodium nitrite and a hydroalcoholic solution to obtain a diazo chemical reagent; the acid comprises hydrochloric acid and / or sulfuric acid; and the volume ratio of water to alcohol in the hydroalcoholic solution is 4 to 9:1.

[0015] Preferably, the concentration of the acid in the hydroalcoholic solution is 0.1-0.5 mol / L; the concentration of the sodium nitrite in the hydroalcoholic solution is 0.01-0.05 mmol / L.

[0016] Preferably, the temperature of the diazotization reaction is 10-25° C., and the time is 10-60 min.

[0017] The present invention provides an anthraquinone grafted modified carbon-based composite material prepared by the preparation method described in the above technical solution.

[0018] The present invention provides application of the anthraquinone grafted modified carbon-based composite material described in the above technical solution in the electrosynthesis of hydrogen peroxide.

[0019] The present invention provides a method for preparing an anthraquinone grafted modified carbon-based composite material, firstly, the aminoanthraquinone is adsorbed on the surface of the carbon-based material by a physical impregnation method; then, an in-situ diazotization reaction is performed to promote the grafting of the anthraquinone group to the surface of the carbon-based material. The present invention forms a stable covalent bond through the diazotization reaction between the aminoanthraquinone and the carbon-based material, thereby grafting the highly active anthraquinone group to the surface of the carbon-based material, and obtaining a modified carbon-based composite material with the quinone group as the catalytic active center. Therefore, the method of the present invention does not have crystallization between positive and negative ions, does not affect the structure of the carbon-based material itself, and can significantly improve its activity and selectivity in electrocatalytic oxygen reduction to synthesize hydrogen peroxide.

[0020] The diazotization reaction process of the present invention is as follows: firstly, aminoanthraquinone (AQ-NH 2 ) combines with nitrite (AQ-NH 2 +2H + +NaNO 2 →AQ-N 2 + +Na + +2H 2 O), and then through multi-step proton transfer to generate aromatic diazonium salt (AQ-N 2 + ). However, the in-situ generated aromatic diazonium salt is unstable. During the reaction, the aromatic radicals are generated by ultrasonic excitation and release nitrogen. The formed aromatic radicals reconstruct the aromatic radicals on the surface of the carbon-based material to form a covalent bond (C-AQ), that is, the aromatic radicals are reconstructed on the carbon-based material and combined with the C in the carbon-based material to form a covalent bond.

[0021] The grafting modification method of the present invention is simple to operate, efficient, and highly controllable, and is suitable for large-scale batch production. In addition, the grafting modification method of the present invention is also suitable for improving the oxygen reduction catalytic performance of powdered carbon materials, proving that the grafting modification method of the present invention has good universality for carbon materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is the full XPS spectrum of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Example 1;

[0023] Figure 2 High-resolution O1s spectra of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Example 1;

[0024] Figure 3 The SEM images of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Example 1;

[0025] Figure 4 TEM images of the initial carbon black and the anthraquinone grafted modified carbon black prepared in Example 4;

[0026] Figure 5 The two-electrode electrolytic cell pressure variation diagram of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Examples 1 to 3;

[0027] Figure 6 RRDE polarization curves of the initial carbon black and the anthraquinone grafted modified carbon black prepared in Example 4;

[0028] Figure 7 It is the hydrogen peroxide selectivity of the initial carbon black and the anthraquinone grafted modified carbon black prepared in Example 4. DETAILED DESCRIPTION

[0029] The present invention provides a method for preparing anthraquinone grafted modified carbon-based composite material, comprising the following steps:

[0030] The carbon-based material is mixed with an aminoanthraquinone compound solution and adsorbed to obtain an aminoanthraquinone-carbon-based material composite;

[0031] The aminoanthraquinone-carbon-based material composite is mixed with a diazo chemical reagent to perform a diazotization reaction to obtain an anthraquinone grafted modified carbon-based composite material;

[0032] The carbon-based material includes graphite felt or carbon-based powder material.

[0033] In the present invention, unless otherwise specified, the required raw materials or reagents are commercially available products well known to those skilled in the art.

[0034] The present invention mixes the carbon-based material with an aminoanthraquinone compound solution and performs adsorption to obtain an aminoanthraquinone-carbon-based material composite.

[0035] In the present invention, the carbon-based material includes graphite felt or carbon-based powder material; the carbon-based powder material preferably includes one or more of conductive carbon black, graphite and carbon nanotubes; when the carbon-based powder material is two or more of the above, the present invention has no special limitation on different types of carbon-based powder materials, and can be adjusted according to actual needs.

[0036] When the carbon-based material is graphite felt, the present invention preferably immerses the graphite felt in acetone for ultrasonic cleaning to remove impurities adsorbed on the surface, then uses water for ultrasonic cleaning to remove residual acetone, then places it in a vacuum drying oven for vacuum drying, and then immerses it in an aminoanthraquinone compound solution; the vacuum drying temperature is preferably 60 to 100° C., more preferably 80 to 90° C.; the time is preferably 6 to 12 hours, more preferably 8 to 10 hours.

[0037] In the present invention, the aminoanthraquinone compounds in the aminoanthraquinone compound solution preferably include one or more of 1-aminoanthraquinone, 2-aminoanthraquinone, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone and 2,6-diaminoanthraquinone; when the aminoanthraquinone compounds are two or more of the above, the present invention has no special limitation on different types of aminoanthraquinone compounds, which can be adjusted according to actual needs.

[0038] In the present invention, the concentration of the aminoanthraquinone compound solution is preferably 0.1-0.5 mol / L, more preferably 0.1-0.3 mol / L, more preferably 0.25 mol / L; the solvent used for the aminoanthraquinone compound solution is preferably anhydrous ethanol.

[0039] When the carbon-based material is graphite felt, the carbon-based material and the aminoanthraquinone compound solution are preferably mixed by impregnation mixing; when the carbon-based material is a carbon-based powder material, the carbon-based material and the aminoanthraquinone compound solution are preferably mixed by ultrasonic dispersion.

[0040] In the present invention, the mass ratio of the carbon-based material to the aminoanthraquinone compound in the aminoanthraquinone compound solution is preferably 0.01 to 1: 1, and more preferably 0.02 to 0.07: 1. The present invention limits this ratio so that the amount of aminoanthraquinone adsorbed on the surface of the carbon-based material is large, the number of catalytic active sites is large, and the catalytic activity is improved.

[0041] In the present invention, the adsorption temperature is preferably 25°C, the time is preferably 6 to 18 hours, more preferably 10 to 16 hours, and further preferably 12 to 15 hours; the adsorption is preferably carried out under stirring conditions, and the present invention has no special limitation on the stirring, and the stirring rate can be controlled according to actual needs.

[0042] After the adsorption is completed, the present invention preferably removes the carbon-based material and vacuum-dries it to obtain an aminoanthraquinone-carbon-based material composite; the vacuum drying temperature is preferably 60 to 100° C., the time is preferably 6 to 12 hours, and more preferably 8 hours. When the carbon-based material is a carbon-based powder material, after the adsorption is completed, it is preferably vacuum-filtered and then vacuum-dried.

[0043] The present invention mixes the aminoanthraquinone-carbon-based material composite with a diazo chemical reagent to carry out a diazotization reaction to obtain an anthraquinone grafted modified carbon-based composite material.

[0044] In the present invention, the preparation method of the diazo chemical reagent preferably includes: mixing an acid, sodium nitrite and a hydroalcohol solution to obtain a diazo chemical reagent; the acid preferably includes hydrochloric acid and / or sulfuric acid; the mass fraction of the hydrochloric acid is preferably 37%, and the sulfuric acid is preferably 98wt% concentrated sulfuric acid; the volume ratio of water to alcohol in the hydroalcohol solution is preferably 4 to 9:1, more preferably 4 to 6:1; the alcohol is preferably ethanol or isopropanol.

[0045] In the present invention, the concentration of the acid in the hydroalcoholic solution is preferably 0.1-0.5 mol / L, more preferably 0.25-0.5 mol / L; the concentration of the sodium nitrite in the hydroalcoholic solution is preferably 0.01-0.05 mmol / L, more preferably 0.025-0.05 mol / L.

[0046] The present invention has no special limitation on the usage ratio of the aminoanthraquinone-carbon-based material composite and the diazo chemical reagent, and it is sufficient to ensure that the diazo chemical reagent is in a sufficient amount.

[0047] In the present invention, the temperature of the diazotization reaction is preferably 10-25°C, more preferably 15-20°C, and the time is preferably 10-60 min, more preferably 30-50 min; the diazotization reaction is preferably carried out under ultrasonic conditions. The present invention has no special limitation on the ultrasonic conditions, and any conditions well known in the art can be used.

[0048] In the present invention, the diazotization reaction process is as follows: firstly, aminoanthraquinone (AQ-NH 2 ) combines with nitrite (AQ-NH 2 +2H + +NaNO 2 →AQ-N 2 + +Na + +2H 2 O), and then through multi-step proton transfer to generate aromatic diazonium salt (AQ-N 2 + ). However, the in-situ generated aromatic diazonium salt is unstable. During the reaction, the aromatic radicals are generated by ultrasonic excitation and release nitrogen. The formed aromatic radicals reconstruct the aromatic radicals on the surface of the carbon-based material to form a covalent bond (C-AQ), that is, the aromatic radicals are reconstructed on the carbon-based material and combined with the C in the carbon-based material to form a covalent bond.

[0049] After completing the diazotization reaction, the present invention preferably washes and vacuum-dries the obtained product in sequence to obtain an anthraquinone grafted modified carbon-based composite material; the washing is preferably carried out in sequence with ethanol and water; the temperature of the vacuum drying is preferably 60 to 100°C, more preferably 80 to 90°C, and the time is preferably 6 to 12 hours, more preferably 8 to 10 hours.

[0050] When the carbon-based material is a carbon-based powder material, after the diazotization reaction is completed, the present invention preferably separates the carbon-based material by vacuum filtration, and then sequentially washes and vacuum-dries.

[0051] In addition, the prior art (Nature communications, 11.2020.2209.) constructs active quinone groups similar to those in early anthraquinone sulfonate catalysts by mechanical ball milling, and points out that the quinone functional groups on the surface of oxygen-doped carbon have the best adsorption energy for oxygen-containing intermediates and are active sites for the electrocatalytic synthesis of hydrogen peroxide. Therefore, the anthraquinone grafted modified carbon-based composite material prepared by the present invention uses the quinone group as the active center, which also serves as the active site for the electrocatalytic synthesis of hydrogen peroxide.

[0052] The present invention provides an anthraquinone grafted modified carbon-based composite material prepared by the preparation method described in the above technical solution.

[0053] The present invention provides the application of the anthraquinone grafted modified carbon-based composite material in the above technical solution in the electrosynthesis of hydrogen peroxide. The present invention has no special limitation on the application method, and the application can be carried out according to the process well known in the art.

[0054] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0055] Example 1

[0056] (1) Cut the graphite felt (Sichuan Junrui Carbon Fiber Materials Co., Ltd., i.e. the initial graphite felt) into 2*2cm 2 The cube (thickness 0.4 cm, mass 0.16 g) was immersed in an acetone solution and ultrasonically cleaned for 30 min, then ultrasonically cleaned with deionized water for 30 min, and placed in a vacuum drying oven at 60 °C for 8 h;

[0057] (2) adding 5.57 g of 1-aminoanthraquinone into 100 mL of anhydrous ethanol and stirring until completely dissolved to obtain a 1-aminoanthraquinone solution (0.25 mol / L); immersing the dried graphite felt obtained in (1) in the 1-aminoanthraquinone solution and stirring and immersing for 12 h at room temperature (25° C.); taking out the graphite felt and vacuum drying it at 60° C. for 8 h to obtain a graphite felt adsorbed with 1-aminoanthraquinone;

[0058] (3) Add 2.07 mL of 37% concentrated hydrochloric acid (analytical grade) and 0.17 g (2.5 mmol) of sodium nitrite to 100 mL of the aqueous alcohol solution (V 水 / V 醇=4:1, alcohol is isopropanol), to obtain a diazo chemical reagent; then immerse the graphite felt in step (2) in the diazo chemical reagent, and perform ultrasonic reaction at a constant temperature of 20°C for 30 minutes; the reacted graphite felt is cleaned with ethanol and deionized water in turn, placed in a vacuum drying oven, and dried at 60°C for 8 hours to obtain anthraquinone grafted modified graphite felt.

[0059] Example 2

[0060] The dosage of 1-aminoanthraquinone in Example 1 was changed from 5.57 g to 11.14 g; the dosage of concentrated hydrochloric acid was changed from 2.07 mL to 4.14 mL; the dosage of sodium nitrite was changed from 0.17 g to 0.34 g, and the other conditions were the same as in Example 1.

[0061] Example 3

[0062] The dosage of 1-aminoanthraquinone in Example 1 was changed from 5.57 g to 2.23 g; the dosage of concentrated hydrochloric acid was changed from 2.07 mL to 0.83 mL; the dosage of sodium nitrite was changed from 0.17 g to 0.07 g, and the other conditions were the same as in Example 1.

[0063] Example 4

[0064] (1) 5.57 g of 1-aminoanthraquinone was added to 100 mL of anhydrous ethanol solution and stirred until completely dissolved to obtain a 1-aminoanthraquinone solution (0.25 mol / L); 0.2 g of conductive carbon black (Capote XC-72R, i.e., initial carbon black) was added to the 1-aminoanthraquinone solution and ultrasonically dispersed for 30 min; then, the mixture was stirred and immersed for 12 h at room temperature (25° C.), vacuum filtered, and vacuum dried at 80° C. for 8 h to obtain a carbon black powder adsorbed with 1-aminoanthraquinone;

[0065] (2) Add 2.07 mL of 37% concentrated hydrochloric acid (analytical grade) and 0.17 g of sodium nitrite to 100 mL of the aqueous alcohol solution (V 水 / V 醇 =4:1, alcohol is isopropanol), to obtain a diazo chemical reagent; then add the carbon black powder adsorbed by 1-aminoanthraquinone in step (1) to the diazo chemical reagent, and react with ultrasound at a constant temperature of 20°C for 30 minutes; separate the carbon black particles by vacuum filtration, and wash them with ethanol and deionized water in turn, place the washed carbon black powder in a vacuum drying oven, and dry it at 80°C for 8 hours to obtain anthraquinone grafted modified carbon black.

[0066] Example 5

[0067] The only difference from Example 1 is that 1-aminoanthraquinone is replaced by 2-aminoanthraquinone.

[0068] Example 6

[0069] The only difference from Example 1 is that 1-aminoanthraquinone is replaced by 2,6-diaminoanthraquinone.

[0070] Example 7

[0071] The only difference from Example 4 is that 1-aminoanthraquinone is replaced by 2-aminoanthraquinone.

[0072] Example 8

[0073] The only difference from Example 4 is that 1-aminoanthraquinone is replaced by 2,6-diaminoanthraquinone.

[0074] Characterization

[0075] Figure 1 is the XPS full spectrum of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Example 1; Figure 1 It can be seen that the O1s peak intensity of the anthraquinone grafted modified graphite felt is significantly higher than that of the initial graphite felt (the oxygen content increases from the initial 2.1at% to 5.6at%), indicating the successful introduction of the anthraquinone functional group.

[0076] Figure 2 is a high-resolution O1s spectrum of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Example 1; Figure 2 It can be seen that the anthraquinone grafted modified graphite felt has a relatively higher carbonyl content (increased from 9.1 at % to 22.7 at %), which further proves that the anthraquinone group has been grafted onto the graphite felt surface through the diazo reaction.

[0077] Figure 3 is the SEM image of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Example 1; Figure 3 It can be seen that the morphology of graphite felt has basically not changed.

[0078] Figure 4 TEM images of the initial carbon black and the anthraquinone grafted modified carbon black prepared in Example 4; Figure 4 It can be seen that the morphology of carbon black has basically not changed.

[0079] Test Example 1

[0080] The electrical properties of the anthraquinone grafted modified graphite felts prepared in Examples 1 to 3 were tested in a conventional H-type cell using a two-electrode system, and the specific steps included:

[0081] (I) Prepare 5% NaOH electrolyte: accurately weigh 50 g of NaOH and place it in a beaker, add 950 g of water, stir to dissolve, and cool naturally to room temperature.

[0082] (II) Electrochemical test: using 2*2cm 2Graphite felt or initial graphite felt of different cases was used as cathode electrode, and nickel foam of the same size was used as anode; the electrolyte in the cathode and anode chambers was separated by a cationic membrane, and then the electrolyte was charged at 100 mA / cm 2 The constant current electrolysis was carried out for 40 min at a current density of 1.5 %. After the reaction was completed, the concentration of hydrogen peroxide in the cathode chamber solution was measured.

[0083] (III) Hydrogen peroxide concentration test (potassium titanium oxalate spectrophotometry): Take 1 mL of cathode electrolyte, add 2 mL of 3 mol / L sulfuric acid, 2 mL of 0.05 mol / L potassium titanium oxalate solution and 5 mL of pure water, and after color development for 10 minutes, measure its absorbance value at a wavelength of 385 nm with the reagent blank (water) as a reference.

[0084] The hydrogen peroxide concentration and absorbance value satisfy the standard curve: hydrogen peroxide concentration (mg / L) = (absorbance value - 0.00022) / 0.025.

[0085] Results Figure 5 and Table 1.

[0086] Figure 5 The two-electrode electrolytic cell pressure change diagram of the initial graphite felt and the anthraquinone grafted modified graphite felt prepared in Examples 1 to 3; Figure 5 As shown in the figure, the cell voltage (@100mA / cm 2 The current density) was reduced by 60mV (Example 3), 113mV (Example 1) and 173mV (Example 2) respectively compared with the initial graphite felt electrode.

[0087] Table 1 Hydrogen peroxide production and selectivity of different graphite felt electrodes in H-type cell test

[0088] sample Hydrogen peroxide content mg / L Hydrogen peroxide selectivity % Initial graphite felt 1562 55 Example 1 2493 88 Example 2 2698 95 Example 3 2271 81

[0089] Note: The volume of the solution in the cathode / anode chamber in the H-cell test is 60 mL.

[0090] It can be seen from Table 1 that, compared with the initial graphite felt electrode, the hydrogen peroxide selectivity of the anthraquinone grafted modified graphite felt prepared in Examples 1 to 3 is greatly improved.

[0091] The above experimental results show that anthraquinone grafting modification greatly improves the two-electron oxygen reduction catalytic activity and selectivity of graphite felt electrode.

[0092] Test Example 2

[0093] The electrocatalytic performance of the anthraquinone grafted modified carbon black prepared in Example 4 was tested using a rotating ring disk electrode (RRDE), comprising the following steps:

[0094] (I) Preparation of slurry: 4 mg of catalyst (anthraquinone grafted modified carbon black or initial carbon black), 560 μL of water, 420 μL of isopropanol, and 20 μL of binder (5 wt.% Nafion) were added into a 1.5 mL plastic centrifuge tube, and then ultrasonically dispersed at 20° C. for 1 h to obtain catalyst slurry;

[0095] (II) Preparation of working electrode: 10 μL of catalyst slurry was dropped onto an area of ​​0.2475 cm 2 The surface of the RRDE electrode was dried naturally to obtain a working electrode; a graphite rod was used as a counter electrode, and a Hg / HgO electrode was used as a reference electrode; the preparation method of the 5% NaOH electrolyte was the same as above;

[0096] (III) Electrochemical test: 100 mL of electrolyte was placed in a five-necked reaction bottle. Oxygen was continuously introduced (60 mL / min) during the test. Then, 100 cycles of cyclic voltammetry were performed until the electrode surface was stable. Finally, the LSV curve was tested (-0.8 to 0.15 V vs. Hg / HgO, voltage sweep rate 10 mV / s, electrode rotation speed 1600 rpm). The ring electrode oxidation voltage was 0.25 V vs Hg / HgO.

[0097] Figure 6 RRDE polarization curves of the initial carbon black and the anthraquinone grafted modified carbon black prepared in Example 4; Figure 6 It can be seen that compared with unmodified carbon black, anthraquinone grafted modified carbon black has better oxygen reduction electrocatalytic activity and exhibits higher hydrogen peroxide current.

[0098] Figure 7 is the hydrogen peroxide selectivity of the initial carbon black and the anthraquinone grafted modified carbon black prepared in Example 4; Figure 7 It can be seen that the hydrogen peroxide selectivity of the grafted modified carbon black is greatly improved, up to 95-100%.

[0099] Therefore, the covalent grafting modification method of the present invention is also applicable to optimizing powdered carbon materials.

[0100] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing anthraquinone grafted modified carbon-based composite material, It is characterized in that The following steps are involved: The carbon-based material is mixed with an aminoanthraquinone compound solution and adsorbed to obtain an aminoanthraquinone-carbon-based material composite; The aminoanthraquinone-carbon-based material composite is mixed with a diazo chemical reagent to perform a diazotization reaction to obtain an anthraquinone grafted modified carbon-based composite material; The carbon-based material includes graphite felt or carbon-based powder material.

2. The preparation method according to claim 1, It is characterized in that The carbon-based powder material includes one or more of conductive carbon black, graphite and carbon nanotubes.

3. The preparation method according to claim 1 or 2, It is characterized in that The aminoanthraquinone compound in the aminoanthraquinone compound solution includes one or more of 1-aminoanthraquinone, 2-aminoanthraquinone, 1,4-diaminoanthraquinone, 1,5-diaminoanthraquinone and 2,6-diaminoanthraquinone.

4. The preparation method according to claim 3, It is characterized in that The concentration of the aminoanthraquinone compound solution is 0.1-0.5 mol / L.

5. The preparation method according to claim 1 or 4, It is characterized in that The adsorption temperature is 25° C. and the adsorption time is 6 to 18 hours.

6. The preparation method according to claim 1, It is characterized in that The preparation method of the diazo chemical reagent comprises: mixing acid, sodium nitrite and a water-alcohol solution to obtain the diazo chemical reagent; the acid comprises hydrochloric acid and / or sulfuric acid; and the volume ratio of water to alcohol in the water-alcohol solution is 4 to 9:

1.

7. The preparation method according to claim 6, It is characterized in that The concentration of the acid in the water-alcohol solution is 0.1-0.5 mol / L; the concentration of the sodium nitrite in the water-alcohol solution is 0.01-0.05 mmol / L.

8. The preparation method according to claim 1, It is characterized in that The temperature of the diazotization reaction is 10-25° C., and the time is 10-60 min.

9. The anthraquinone grafted modified carbon-based composite material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the anthraquinone grafted modified carbon-based composite material according to claim 9 in the electrosynthesis of hydrogen peroxide.