Manufacture of intermediate modulus carbon fibers
Through high solidification concentration polymer stock liquid spinning and multi-stage oven treatment, the problem of increasing tensile strength and elastic modulus of carbon fiber is solved, and the high-performance preparation of carbon fiber is achieved, especially the development of improved tensile characteristics at lower temperatures carbon fiber.
Patent Information
- Application Number
- CN202411048641.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2015-03-12
- Filing Date
- 2016-02-15
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to simultaneously increase the tensile strength and elastic modulus of carbon fibers, and increasing the carbonization temperature will lead to a reduction in compression and shear strength. The traditional tensile method is limited by oxidation conditions, resulting in the obtained carbon fibers in the resin impregnation line. The tensile strength is reduced.
The polymer stock solution with high solidification concentration is spinned to form a dense precursor fiber structure, and oxidize and carbonize at lower temperatures. Combined with multi-stage oven treatment and surface treatment, a high tensile strength and elastic mold is prepared. amount of carbon fiber.
The tensile strength of carbon fiber is close to 800ksi and the elastic modulus is close to 40Msi, and the intermediate modulus characteristics are developed at lower carbonization temperatures, improving the surface functionality and mechanical properties of the fibers.
Smart Images

Figure BDA0004974232010000091 
Figure BDA0004974232010000101 
Figure BDA0004974232010000102
Abstract
Description
This application is a divisional application of the following application: Application date February 15, 2016; Application number 201680015296.1; Invention name “Manufacturing of intermediate modulus carbon fiber”. This patent application claims priority to pending serial number 62 / 132137 filed on March 12, 2015 and is incorporated herein in its entirety. Technical Field
[0001] The present disclosure generally relates to carbon fibers having high tensile strength and elastic modulus, and a method for making such carbon fibers. Background Art
[0002] Carbon fibers have been used in a variety of applications because of their desirable properties such as high strength and stiffness, high chemical resistance, and low thermal expansion. For example, carbon fibers can be formed into structural parts that combine high strength and high stiffness while having a significantly lighter weight than metal parts with equivalent properties. Carbon fibers are increasingly being used as structural components in composite materials for use in aerospace and automotive applications, among others. In particular, composite materials have been developed in which carbon fibers act as a reinforcing material in a resin or ceramic matrix.
[0003] In order to meet the stringent requirements of various industries, especially aerospace, it is necessary to continue to develop new carbon fibers with high tensile strength (about 800 ksi or greater) and high elastic modulus (about 40 Msi or greater) and without surface flaws or internal defects. Compared to carbon fibers with lower strength, carbon fibers with higher tensile strength and modulus alone can be used in less amount, and still achieve the same overall strength for a given carbon fiber reinforced composite part. As a result, composite parts containing these carbon fibers are lighter. The reduction in structural weight is important for the aerospace and automotive industries because it increases fuel efficiency and / or the load-bearing capacity of aircraft or automobiles incorporating such composite parts.
[0004] Carbon fibers from acrylonitrile are typically produced through a series of manufacturing steps or stages. Acrylonitrile monomer is first polymerized by mixing acrylonitrile monomer with one or more comonomers (e.g., itaconic acid, methacrylic acid, methyl acrylate, and / or methyl methacrylate) and reacting the mixture with a catalyst in a conventional solution polymerization or suspension process to form a polyacrylonitrile (PAN) polymer solution (spinning "dope"). PAN is currently the most widely used precursor for carbon fibers.
[0005] Once polymerized, the PAN dope is spun into precursor (acrylic) fibers using one of several different methods. In one method (dry spinning), the heated dope is pumped (filtered) through small holes in a spinneret into a tower or chamber of heated inert gas where the solvent evaporates, leaving behind solid fibers.
[0006] In another process (wet spinning), a heated polymer solution ("dope") is pumped through small holes in a spinneret into a coagulation bath where the dope coagulates and solidifies into fibers. Wet spinning can be further divided into one of the following subprocesses: (1) wet jet spinning, in which the spinneret is immersed in a coagulation bath; (2) air gap or dry jet spinning, in which the polymer jet exits the spinneret and passes through a small air gap (typically 2-10 mm) before contacting the coagulation bath; and (3) gel spinning, in which the dope is thermally induced to a phase change from a fluid solution to a gel network. In both dry and wet spinning processes, the fibers are then washed and stretched through a series of one or more baths.
[0007] After spinning and stretching the precursor fibers and before they are carbonized, the fibers need to be chemically altered to convert their linear molecular arrangement into a more thermally stable molecular ladder structure. This is achieved by heating the fibers in air to about 200°C-300°C (about 390°F-590°F) for about 30-120 minutes. This causes the fibers to absorb oxygen molecules from the air and rearrange their atomic bonding pattern. This oxidation or thermal stabilization step can be performed by various methods, such as drawing the fibers through a series of heated chambers or passing the fibers through hot rollers.
[0008] After oxidation, the stabilized precursor fibers are heated (carbonized) in one or two furnaces filled with a gas mixture that does not contain oxygen to a maximum temperature of about 1000°C-3000°C (about 1800°F-5500°F) for several minutes. As these fibers are heated, they begin to lose their non-carbon atoms in the form of various gases such as water vapor, hydrogen cyanide, ammonia, carbon monoxide, carbon dioxide, hydrogen and nitrogen. As the non-carbon atoms are expelled, the remaining carbon atoms form tightly bound carbon crystals aligned parallel to the long axis of the fiber.
[0009] The resulting carbon fibers have a surface that does not bond well with epoxy resins and other materials used in composites. To give the fibers better bonding properties, their surfaces are slightly oxidized. Adding oxygen atoms to the surface provides better chemical bonding properties and also removes weakly bonded crystallites for better mechanical bonding properties.
[0010] Once oxidized, the carbon fibers are coated ("sized") to protect them from damage during the winding or braiding process. The sizing material applied to the fibers is typically selected to be compatible with the epoxy resin used to form the composite. Typical sizing materials include epoxy, polyester, nylon, urethane, etc.
[0011] The high modulus of carbon fiber comes from the high crystallinity of the crystallites and the high degree of alignment in the fiber direction, while the high strength of carbon fiber is mainly achieved by eliminating defects and developing crystalline morphology in the fiber. It is believed that increasing the heat treatment temperature to develop larger and oriented graphite structures can improve Young's modulus, while removing defects has the potential to increase fiber strength.
[0012] Several methods of increasing tensile strength and modulus have been explored in the prior art. For example, it is generally known that modulus can be increased by increasing the carbonization temperature. However, an increase in carbonization temperature leads to a decrease in compression and shear strength. As a result, the method generally does not provide an effective means for preparing carbon fibers having improved elastic modulus and both compression and shear strength.
[0013] Other approaches have focused on stretching the precursor fibers before or during the process of converting the precursor fibers to carbon fibers. It has been previously recognized in the prior art that the modulus of carbon fibers can be improved by stretching the fibers in a post-spinning step, an oxidation step, a carbonization step, or a combination thereof. However, conventional wisdom holds that the amount of stretching in the oxidation step is limited by the level of tension in the fibers that develops in response to the onset of chemical reactions, such as thermally induced cyclization and / or oxidative crosslinking of PAN precursor fibers. The accumulation of tension causes the fibers to break at relatively low stretches under standard oxidation conditions (e.g., above 180°C). As a result, previous attempts to stretch PAN fibers during the oxidation process were generally limited to a maximum amount of stretch or a single continuous stretch. Excessive stretching in the post-precursor process results in lower diameter carbon fibers with lower compressive and shear strengths.
[0014] Conventional techniques for increasing the tensile strength of carbon fibers as resin-impregnated wires have been directed to the reduction of macroscopic defects, such as for reducing impurities present within the individual filaments constituting the carbon fibers, or for inhibiting the generation of macropores formed within the individual filaments, and for reducing defects generated on the surface of the individual filaments. Attempts to reduce internal impurities include improving the filtration of monomer or polymer stock solutions. Surface defects have been reduced by controlling the shape of fiber guides used in the production process of precursor fibers.
[0015] It is also known to densify undrawn fibers by optimizing the conditions of the coagulation bath. This technique obtains carbon fibers having high tensile strength and modulus by dissolving a specific acrylonitrile polymer containing 95 wt% or more of acrylonitrile in dimethylformamide as a solvent, wet spinning the resulting stock solution, drawing and washing the resulting precursor fibers, and oxidizing and carbonizing the washed fibers. However, when stabilizing, excessive densification tends to reduce oxygen permeability into the fibers, resulting in a decrease in tensile strength expressed as a resin-impregnated line of the carbon fibers obtained by this method.
[0016] Therefore, there is a need for carbon fibers having both high compressive strength and high elastic modulus, and methods for preparing such carbon fibers. In addition, there is a need for carbon fibers having both high tensile strength and high elastic modulus when impregnated with resin. Summary of the invention
[0017] The present invention provides carbon fibers with improved strength and modulus and a method for preparing these carbon fibers. The carbon fiber precursor fibers according to the present invention have been prepared from carbon fibers having a weight average molecular weight M of about 100,000 to about 300,000. w and a polydispersity M of 2.0 to 3.0 w / M n Polymer production, where M n is the number average molecular weight of the polymer. Preferably, the polydispersity M of the polymer used to produce the carbon fiber precursor fiber is w / M n is from 2.1 to 2.6. The solidified carbon fiber precursor fiber according to the present invention may have a porosity range of about 30% to about 70%.
[0018] The present invention further provides a method for producing carbon fiber. According to the present invention, a polymer solution having a polymer concentration of about 19% to about 24% is spun in a coagulation bath of about 70% to about 85% solvent and about 15% to about 30% water, thereby forming a carbon fiber precursor fiber. The coagulation bath may have a bath temperature from about 0°C to about 10°C. In one embodiment, the coagulation bath solvent is dimethyl sulfoxide ('DMSO').
[0019] In one embodiment, the polymer is a polyacrylonitrile-based polymer. In one embodiment, the polyacrylonitrile-based polymer is a copolymer formed by polymerization of acrylonitrile and a comonomer selected from itaconic acid, methacrylic acid, methacrylate, and combinations thereof. In one embodiment, the polymer has a copolymer content of up to about 4% of the monomer component and an acrylonitrile content of about 96% or more. The polymer may have a weight average molecular weight (MW) of about 100,000 to about 300,000, more preferably about 120,000 to about 180,000. w ).
[0020] In one embodiment, the polymer solution is spun by air gap spinning. The air gap spacing from the face of the spinneret to the surface of the coagulation bath may be about 2 mm to about 10 mm.
[0021] The carbon fiber precursor fibers from the coagulation bath have an average pore size of about 0.01 μm to about 0.03 μm, with a porosity of about 30% to about 70%. The carbon fiber precursor fibers from the coagulation bath may also have a swelling degree of from about 80% to about 120%.
[0022] The spun fibers are then drawn through one or more drawing and washing baths to stretch and remove solvent from the fibers. The bath temperature of the one or more drawing baths is from about 40° C. to about 100° C. In one embodiment, the carbon fiber precursor fibers are spun and drawn at a speed of about 100 to about 400 meters per minute. The carbon fiber precursor fibers are substantially free of solvent after drawing the fibers through the baths. By "substantially free of solvent," the carbon fiber precursor fibers have about 500 ppm or less of residual solvent.
[0023] The carbon fiber precursor fibers are then stabilized and carbonized at a maximum temperature of from about 1100° C. to about 1500° C. Preferably, the carbon fiber precursor fiber filaments are stabilized in air at an oxidation temperature of about 200° C. to about 300° C. at a draw ratio of about 0.80 to about 1.35. DETAILED DESCRIPTION
[0024] The present invention will now be described more fully hereinafter. These inventions may be embodied in many different forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided so that this disclosure will satisfy applicable legal requirements. Like numbers represent like elements throughout.
[0025] In one aspect, the present invention is directed to carbon fibers having improved tensile strength and elastic modulus. In another aspect, the present invention is directed to a method of making these carbon fibers. Carbon fibers prepared according to the methods described herein can have a tensile strength approaching and exceeding 800 ksi and an elastic modulus approaching and exceeding 40 Msi.
[0026] The method developed for producing intermediate modulus (IM) fibers is the basis of the present invention. The method of the present invention produces carbon fibers having tensile properties of a tensile strength of about 830 to about 870 ksi and a tensile modulus of about 43 to about 44 Msi.
[0027] As discussed in more detail below, carbon fibers according to the present invention can be prepared by coagulating a polymer stock solution at a high coagulation concentration (about 70 wt % or greater solvent and up to about 30 wt % water) to form a dense precursor fiber structure. This dense structure enables high stretching to be achieved by oxidation and pre-carbonization, allowing the development of intermediate modulus tensile properties at a carbonization temperature of less than about 1400°C rather than a typical carbonization temperature of about 1450°C or greater. Because the dense precursor fiber structure allows carbonization to be carried out at a lower temperature, the surface of the fiber can be provided with less graphite than the surface of the carbon fiber produced at a higher temperature of 1450°C or greater. In the context of the present invention, the term "fiber" includes a single filament or multiple filaments bundled together, also referred to as a "tow". A tow or bundle can include from about 1,000 to 50,000 individual filaments.
[0028] In the context of the present invention, the term "precursor fiber" refers to a fiber comprising a polymer material that can be converted into a carbon fiber having a carbon content of about 90% or greater by weight and particularly about 95% or greater when sufficient heat is applied. The precursor fiber can include both homopolymers and copolymers of acrylonitrile (AN), and can include copolymers such as methyl acrylate (MA), methacrylic acid (MAA), sodium methallyl sulfonate (SMAS), itaconic acid (ITA), vinyl bromide (VB), isobutyl methacrylate (IBMA), and combinations thereof. polymerization
[0029] PAN polymers can be made by solution polymerization or suspension polymerization. In solution polymerization, acrylonitrile (AN) monomer is mixed with a solvent and one or more comonomers to form a solution. Suitable solvents for solution polymerization include, among others, dimethyl sulfoxide (DMSO), dimethylformamide (DMF), and dimethylacetamide (DMAc). Examples of comonomers suitable for the synthesis of PAN polymers include one or more vinyl acids, such as methacrylic acid (MAA), acrylic acid (AA), and itaconic acid (ITA); vinyl esters, such as methacrylate (MA), ethyl acrylate (EA), butyl acrylate (BA), methyl methacrylate (MMA), ethyl methacrylate (EMA), propyl methacrylate, butyl methacrylate, β-hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, 2-ethylhexyl acrylate, isopropyl acetate, vinyl acetate (VA), and vinyl propionate; other vinyl derivatives (e.g., vinyl amides, such as vinyl imidazole (VIM), acrylamide (AAm), and diacetone acrylamide (DAAm); and vinyl halides, such as allyl chloride, vinyl bromide, vinyl chloride, and vinylidene chloride); ammonium salts of vinyl compounds and sodium salts of sulfonic acids (e.g., sodium vinyl sulfonate, sodium p-styrene sulfonate (SSS), sodium methallyl sulfonate (SMS), and sodium 2-acrylamido-2-methylpropane sulfonate (SAMPS)), and the like. Preferably, the comonomer is itaconic acid and / or methacrylic acid.The solution is then heated to a temperature above room temperature (ie greater than 25°C), for example to a temperature of about 40°C to about 85°C.
[0030] After heating, an initiator is added to the solution to initiate polymerization. PAN polymerization can be initiated by an initiator (or catalyst) of an azo compound (e.g., azo-bisisobutyronitrile (AIBN), azobiscyanovaleric acid (ACVA), and 2,2'-azobis-(2,4-dimethyl) valeronitrile (ABVN), etc.) or an organic peroxide (e.g., dilauroyl peroxide (LPO), di-tert-butyl peroxide (TBPO), diisopropyl peroxydicarbonate (IPP), etc.). Once polymerization is complete, unreacted AN monomer is stripped off (e.g., by degassing under high vacuum), and the resulting PAN polymer solution is cooled. At this stage, the PAN polymer is in the form of a solution or stock solution ready for spinning. Preferably, the PAN polymer is prepared by solution polymerization.
[0031] PAN polymers can also be made by suspension polymerization. To prepare a spinning solution by this method, the obtained PAN can be dissolved in a solvent such as dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), ethylene carbonate (EC), zinc chloride (ZnCl2) / water and sodium thiocyanate (NaSCN) / water to form a spinning solution.
[0032] According to a preferred embodiment, PAN polymerization is carried out based on the following formulation (by weight %): >90% AN monomer; <5% comonomer; <1% initiator, based on the total weight of these components; and a sufficient amount of solvent to form a solution containing 16 wt% to 28 wt%, preferably 19 wt% to 24 wt% of the final PAN polymer. Spinning
[0033] To make PAN precursor fibers, after removing bubbles by vacuum, the PAN polymer solution (i.e., spinning "dope") is subjected to conventional wet spinning and / or air gap spinning. The spinning dope can have a polymer concentration of from about 16% to about 28%, preferably from about 19wt% to about 24wt%, by weight based on the total weight of the solution. In wet spinning, the dope is filtered and squeezed into a liquid coagulation bath for the polymer through the holes of a spinneret (typically made of metal) to form filaments. The spinneret holes determine the desired filament count of the PAN fiber (e.g., 3,000 holes for 3K carbon fiber). In air gap spinning, a vertical air gap of 1 to 50 mm, preferably 2 to 10 mm, is provided between the spinneret and the coagulation bath. In this spinning method, the polymer solution is filtered and extruded from the spinneret in air, and the extruded filaments are then coagulated in a coagulation bath. Air gap spinning is preferred.
[0034] The coagulation liquid used in the method is a mixture of a solvent and a non-solvent. Water or alcohol is typically used as a non-solvent. Suitable solvents include dimethyl sulfoxide, dimethylformamide, dimethylacetamide, sodium thiocyanate and zinc chloride. Dimethyl sulfoxide, dimethylformamide and dimethylacetamide are preferred, with dimethyl sulfoxide being particularly preferred. The ratio of solvent to non-solvent and the bath temperature are used to adjust the coagulation rate of the newly grown filaments extruded during coagulation.
[0035] Coagulation conditions can have a great influence on the structure and tensile properties of precursor fibers and carbon fibers. According to the present invention, in order to obtain dense coagulated fibers with smaller pores, the precursor fibers are coagulated with a coagulation bath concentration of about 70 wt% solvent or higher and up to about 30 wt% water. Preferably, the coagulation bath concentration is about 70 wt% to about 85 wt% solvent and about 15 wt% to about 30 wt% water. More preferably, the coagulation bath concentration is about 75 wt% to about 85 wt% solvent and about 15 wt% to about 25 wt% water. The temperature of the coagulation bath is from about 0°C to about 10°C.
[0036] As a first step to control the fiber diameter, the spun filaments are then taken out of the coagulation bath via rollers through one or more washing baths to remove excess solvent and stretched in a hot (e.g., 40° C. to 100° C.) water bath to impart molecular orientation to the filaments. The stretched filaments are then dried, for example, on drying rollers. These drying rollers may consist of a plurality of rotatable rollers arranged in series and in a serpentine configuration, over which the filaments pass sequentially from roller to roller and under sufficient tension to provide stretching or relaxation of the filaments on these rollers. At least some of the rollers are heated by pressurized steam that circulates internally or through rollers or electrical heating elements within the rollers. Before drying, a finishing oil may be applied to the stretched fibers to prevent the filaments from sticking to each other in downstream processes.
[0037] Processing conditions, including the composition of the spinning solution and coagulation bath, total bath volume, drawing, temperature, and filament speed, are correlated to provide filaments having the desired structure and denier. Oxidation
[0038] To convert the PAN precursor fibers into carbon fibers, the PAN precursor fibers are subjected to oxidation and carbonization. During the oxidation stage, the PAN fibers are fed under tension through one or more specialized ovens into which heated air is fed. The oxidation can be performed at an oven temperature of from about 200°C to about 300°C. The oxidation process combines oxygen molecules from the air with the PAN fibers and begins to crosslink the polymer chains, thereby increasing the fiber density to 1.3 g / cm 3 Up to 1.4g / cm 3 During the oxidation process, the tension applied to the fiber generally controls the fiber to be stretched or contracted at a stretch ratio of 0.8 to 1.35, preferably 1.0 to 1.2. When the stretch ratio is 1, there is no stretching. And when the stretch ratio is greater than 1, the applied tension causes the fiber to be stretched. This oxidized PAN fiber has an infusible trapezoidal aromatic molecular structure and is ready for carbonization treatment. Carbonization
[0039] Carbonization occurs in an inert (oxygen-free) atmosphere in one or more specially designed furnaces. In a preferred embodiment, carbonization can be performed in two steps. Here, the oxidized fiber first passes through a pre-carbonization furnace that subjects the fiber to a heating temperature from about 300°C to about 800°C while being exposed to an inert gas (e.g., nitrogen). The pre-carbonization is then followed by carbonization by passing the fiber through a furnace heated to a higher temperature from about 700°C to about 1500°C while being exposed to an inert gas. The highest carbonization temperature is from 1100°C to 1500°C. Preferably, fiber tension is increased throughout the pre-carbonization and carbonization process. In pre-carbonization, the fiber tension applied is sufficient to control the draw ratio within the range of 0.9 to 1.2. In carbonization, the tension used is sufficient to provide a draw ratio of 0.9 to 1.05. Carbonization causes crystallization of carbon molecules and thus produces a finished carbon fiber having a carbon content greater than 90%.
[0040] Adhesion between the matrix resin and the carbon fibers is an important criterion in carbon fiber reinforced polymer composites. Since the precursor fibers produced according to the method of the present invention are very dense, carbonization can be performed at lower temperatures. This is advantageous because less graphitization occurs, resulting in carbon fibers with more surface functional groups that react with the matrix resin. Surface treatment
[0041] During the manufacture of carbon fibers, surface treatment may be performed after oxidation and carbonization to further enhance adhesion between the resin matrix and the carbon fibers. The surface treatment may include pulling the carbonized fibers through an electrolytic bath containing an electrolyte such as ammonium bicarbonate or sulfuric acid. The chemicals of the electrolytic bath add reactive chemical groups on the fiber surface that improve interfacial fiber / matrix bonding and also remove weakly bonded crystallites for better mechanical bonding properties.
[0042] Next, the carbon fibers may be subjected to sizing, wherein a sizing coating (e.g., an epoxy coating) is applied to the fibers. Sizing may be performed by passing the fibers through a sizing bath containing a liquid coating material. Sizing protects the carbon fibers during handling and processing into intermediate forms such as dry fabrics and prepregs. Sizing also holds the filaments together in individual tows to reduce fuzz, improves processability, and increases interfacial shear strength between the fibers and the matrix resin.
[0043] After sizing, the coated carbon fiber is dried and then wound onto a bobbin.
[0044] Carbon fibers produced from the above PAN polymers have been found to have the following mechanical properties: a tensile strength greater than 700 Ksi (4826 MPa) and a tensile initial modulus greater than 38 Msi (262 GPa) according to the ASTM D 4018 test method.
[0045] The following examples are provided to illustrate aspects of the present invention, and these examples should not be construed as limiting the present invention. Unless otherwise indicated, all elastic modulus measurements cited in the examples were performed in accordance with ASTM D4018. The fiber modulus values refer to the tensile chord modulus of the resin-impregnated tow line determined between the lower and upper strain limits of 0.1% and 0.6%, respectively. In addition, tensile strength was measured in accordance with ASTM D 4018. Example - Example 1 - Synthesis of dope for spinning
[0046] PAN polymers were prepared according to the formulations for PAN polymerization shown in Table 1. DMSO and AIBN were used for solution polymerization solvent and catalyst, respectively. Table 1 - Formulations for PAN polymerization
[0047] During solution polymerization, DMSO and AN are metered into the reactor. Under nitrogen purge, comonomers (ITA or MAA) and AIBN are added to the reactor at the desired temperature of 40°C-85°C. The reaction takes about 8-24 hours. After the reaction, the reactants are then cooled and discharged. After the bubbles are removed by vacuum, the polymer solution (or spinning "dope") is pumped for spinning. Example 2 - Fabrication of PAN Precursor Fibers
[0048] Carbon fiber precursors (or white fibers) were formed by air-gap spinning using PAN polymers produced from Formulations 1-3 as described in Table 1 above, with air gap spacing ranging from 2 to 10 mm. Coagulation bath parameters were varied for each run as indicated in Table 2 below. Table 2 - Coagulation bath composition and coagulated fiber density results
[0049] The properties of the white precursor fibers were determined as follows. Porosity determination
[0050] The fiber samples leaving the coagulation bath were freeze dried at -60 °C and the freeze dried samples were tested by mercury intrusion porosimetry for porosity and porous structure analysis. Mercury intrusion porosimetry characterizes the porosity of a material by applying various levels of pressure to a sample immersed in mercury. It can measure pore sizes ranging from 500 μm to 35 nm. It is based on the physical principle that a non-reactive, non-wetting liquid will not penetrate a pore until sufficient pressure is applied to force it in. In this case, mercury is a non-wetting liquid for almost all substances and has a high contact angle for most solids. Mercury will not penetrate the pores by capillary action and requires a force to enter the pore space. Considering the Washburn equation, entering the pore space requires the application of a pressure that is inversely proportional to the size of the pore opening. When mercury comes into contact with a pore opening having a circular cross section, the surface tension of the mercury acts along the contact circle for a length equal to the circumference of the circle. This assumes a cylindrical pore. Based on this assumption, the force with which mercury resists entering the pore is equal to -πDγcosθ, where D is the pore diameter, γ is the surface tension, and θ is the contact angle. (Since θ>90°, the minus sign is introduced and the term is inherently negative.) The force acts on the area of the contact circle (hole) due to the externally applied pressure and is expressed as πD 2 P / 4, where P is the applied pressure. At equilibrium, the following equation holds:
[0051] A simplified version of this equation is called the Washburn equation:
[0052] Based on this, the volume of mercury forced into the pores (and void space) increases directly with increasing pressure. By increasing the applied pressure over a set range, a unique pressure-volume curve can be plotted. The pore size distribution is then readily obtained. Incremental and cumulative pore volumes compared to pore size can also be calculated.
[0053] For this measurement, a freeze-dried sample with a known weight is placed in a penetrometer assembly with a known weight and sealed. A "powder" sample bottle is used to prevent fibers from entering the rod. The sample is placed in the low-pressure port of the porosimeter, where a vacuum is applied to remove air and residual moisture. The sample cell is then filled with mercury and a pressure of 0.54psia is obtained. The bulk density measurement is calculated at this time. The penetrometer is then returned to atmospheric pressure and removed and placed in the high-pressure port to complete the test. In the high-pressure port, the sample cell is surrounded by hydraulic fluid and the pressure is gradually increased to up to 60,000psia. At each pressure point, the volume of intruded mercury is measured by the change in capacitance between the mercury column in the dilatometer rod and the coaxial metal sheet around the rod of the penetrometer assembly. Once the final pressure is reached, the skeletal density is calculated. A report showing the pressure-volume curve and pore size distribution is then generated. Once the pore size distribution data is obtained, several data modifications are performed to calculate the most relevant and accurate data. The first modification is to exclude pores larger than 5μm. Based on the logarithmic differential intrusion volume curve for pore size, there are characteristic regions above 5 μm that are interpreted as inter-filament pores / spacing and do not reflect the internal pore structure. These measurements were removed to obtain only inter-filament / internal pores. The second modification was a recalculation of the percent porosity based on the intrusion volume below 5 μm and a set skeletal density of 1.17 g / cc. Swelling degree
[0054] For swelling, the sample removed from the coagulation bath was first centrifuged at 3000 rpm for 15 minutes to remove the adhering liquid from the filament surface. The collected sample was then immersed in a glass beaker / flask containing deionized water (DIW) and "washed" for a minimum of 15 minutes. This washing step was then repeated twice more with fresh DIW to ensure complete coagulation of the sample and removal of the solvent. Once the final wash was completed, the sample was centrifuged again at 3,000 rpm for 15 minutes and weighed to obtain W a The sample was then placed in an air circulating oven at 110°C for 3 hours. After drying, the sample was removed from the oven and placed in a desiccator for a minimum of 10 minutes. The dried and desiccated sample was reweighed and the final weight was recorded as W. f The swelling degree was then calculated using the following formula: Swelling degree (%) = (W a –W f )x(100 / W f )
[0055] The PAN fibers based on Runs 4-6 from Table 2 were found to have good structures with low porosity and no macropores as measured by swelling tests and mercury intrusion porosimetry. As a result, subsequent carbon fibers from these low porosity precursors produced tensile strengths ranging from 778 to 829 ksi. Transforming white fibers into carbon fibers
[0056] The carbon fiber precursors produced by runs 1-6 were oxidized using a multi-stage oven. The total stretch was <10%. The oven temperature was in the range of 200°C-300°C. The total residence time was <150 minutes. The oxidized fibers were carbonized in a multi-stage furnace. The low temperature furnace (called the pre-carbonization furnace) operated in the temperature range of 300°C-800°C. The total stretch was <10%. The high temperature furnace (called the carbonization furnace) operated in the temperature range of 700°C-1500°C. The maximum carbonization temperature was from 1100°C to 1500°C. The total relaxation was <5%. The carbonized fibers were then surface treated and sized with an epoxy resin compatible sizing compound.
[0057] The tensile strength and tensile modulus of the obtained carbon fibers were determined and are shown in Table 3. Table 3 - Carbon fiber properties
[0058] Carbon fiber tensile strength and initial tensile modulus were determined according to ASTM D4018 and SRM 16. Density testing was based on ASTM D3800 and SRM 15.
[0059] Although the present invention has been described with reference to preferred embodiments, it will be appreciated by those skilled in the art that various changes may be made and elements thereof may be replaced by equivalents without departing from the scope of the present invention. In addition, many modifications may be made to adapt specific situations or materials to the teachings of the present invention without departing from its basic scope. Therefore, the present invention is intended not to be limited to the specific embodiments disclosed as the best mode contemplated for carrying out the present invention, but the present invention will include all embodiments falling within the scope of the appended claims.
Claims
1. A method for producing carbon fiber, the method include: forming a polyacrylonitrile polymer solution having a polyacrylonitrile (PAN) polymer concentration of about 19% to about 24%; Spinning the polyacrylonitrile polymer solution by air-gap spinning, wherein the polyacrylonitrile polymer solution is extruded from a spinneret in air to form filaments, and then coagulating the extruded filaments in a coagulation bath, wherein the coagulation bath contains about 70% to about 85% by weight of dimethyl sulfoxide and about 15% to about 30% by weight of water, thereby forming carbon fiber precursor fibers; drawing the carbon fiber precursor fibers through one or more drawing and washing baths, wherein after the step of drawing the carbon fiber precursor fibers, the carbon fiber precursor fibers are substantially free of solvent; and stabilizing and carbonizing the carbon fiber precursor fibers; The polyacrylonitrile polymer is a copolymer obtained by polymerizing acrylonitrile monomer and itaconic acid and / or methacrylic acid as the only comonomers in the presence of an initiator at a temperature of 40°C to 85°C; The temperature of the coagulation bath is in the range of 40°C to 85°C; The carbon fiber precursor fibers from the coagulation bath have a swelling degree from about 80% to about 120%, an average pore size from about 0.01 μm to about 0.03 μm, and a porosity from about 30% to about 70%, and The carbon fiber precursor fibers are carbonized at a temperature ranging from about 1100°C to about 1500°C.
2. The method of claim 1, wherein the polyacrylonitrile polymer has a weight average molecular weight (MW) of about 120,000 to about 180,000. w ).
3. The method of claim 1, wherein the air gap spacing from the face of the spinneret to the surface of the coagulation bath is about 2.0 to about 10.0 mm.
4. The method of claim 1, wherein the bath temperature of the one or more drawing and washing baths is from about 40°C to about 100°C.
5. The method of claim 1, further comprising stretching the carbon fiber precursor fiber in the drawing step.
6. The method of claim 1, further comprising drawing the carbon fiber precursor fiber at a speed of about 100 to about 400 meters per minute.
7. The method of claim 1, further comprising stabilizing the carbon fiber precursor fibers in air at an oxidation temperature of about 200°C to about 300°C at a draw ratio of about 0.80 to about 1.
35.
8. The method of claim 1, wherein the polyacrylonitrile-based polymer has a copolymer content of up to about 4% and an acrylonitrile content of about 96% or greater.
9. The method of claim 1, wherein after carbonization, the polyacrylonitrile-based polymer has a tensile strength of about 800 ksi or greater and an elastic modulus of about 40 Msi or greater.
10. The method of claim 1, wherein The coagulation bath contains 82.3 wt% to 84.02 wt% of dimethyl sulfoxide, and the temperature of the coagulation bath is 4.5° C. to 8.5° C.; and The carbon fiber precursor fibers from the coagulation bath have a swelling degree from 98% to 110%, an average pore diameter from 0.0125 μm to 0.0145 μm, and a porosity from 48.08% to 56.01%.
11. The method of claim 1, wherein the initiator is an azo compound or an organic peroxide.