Method for measuring average density of powder in Bi-series wire
By dissolving Bi-based wire powder and combining it with metallographic analysis, the problem of measuring the average density of powder in Bi-based wires was solved, improving testing efficiency and accuracy, and guiding the optimization of processing technology and the uniformity of engineering current density.
Patent Information
- Application Number
- CN202411132541.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies make it difficult to quickly and effectively measure the average density of powder in Bi-based wires, which affects the engineering current density and processing optimization of superconducting wires and strips.
The average density of the powder was obtained by dissolving the powder in Bi-based wire using glacial acetic acid under high-temperature reflux conditions, and then calculating the mass and volume of the powder using metallographic analysis.
It enables rapid and accurate measurement of the average density of powder in Bi-based wires, guiding the adjustment of processing technology and improving the uniformity of engineering current density.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-temperature superconducting wire strip performance testing and characterization, and in particular relates to a method for measuring the average density of powder in a Bi-based wire. Background Art
[0002] Bi-based superconducting materials are a very important branch of high-temperature superconducting materials, mainly including Bi2Sr2CaCu2O x (referred to as Bi2212) wire and Bi2Sr2Ca2Cu3O x (Abbreviated as Bi2223) strip, powder in tube method (PIT) is the mainstream technology for preparing Bi-based wire. At present, the wire strips prepared by this technology have met the practical needs.
[0003] The size and uniformity of the engineering current density (Je) of Bi-based wires are key parameters in practical applications. The density of superconducting powder in wire strips directly affects the Je of superconducting wire strips, so how to quickly and effectively evaluate the density of superconducting powder in the core wire is an urgent problem to be solved. At the same time, by measuring the density of the core wire powder in the wire, it can provide data support for the study of the deformation of the Ag / powder composite, and can also provide certain help for the optimization of the processing technology of the wire strip. The greater the density of the core wire powder prepared by different processing technologies, the more effectively Je can be improved.
[0004] In order to solve the problem of measuring the average density of powder in Bi-based wires, it is necessary to provide a method for measuring the average density of powder in Bi-based wires. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for measuring the average density of powder in Bi-based wires in view of the deficiencies of the above-mentioned prior art. The method dissolves the powder in the Bi-based wire, obtains the mass of the powder by calculating the mass difference before and after dissolution, and obtains the volume of the powder by metallographic analysis and combining the length, thereby quickly obtaining the average density of the powder in the Bi-based wire, judging whether the Bi-based wire is synchronously deformed during the deformation process, and also providing data support for subsequent process adjustment and processing optimization.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for measuring the average density of powder in Bi-based wire, characterized in that the method comprises the following steps:
[0007] Step 1: Clean and dry the Bi series wire in sequence, then cut it and perform metallographic analysis on the cut part to obtain a metallographic diagram;
[0008] Step 2: Cut the Bi series wire after drying in step 1, and then process the cut part to obtain a short sample of standard columnar shape, and then weigh the short sample to obtain the original mass;
[0009] Step 3, placing the short sample weighed in step 2 into a container filled with glacial acetic acid, and then heating and refluxing in an oil bath with stirring, and then taking out the remaining solid and sequentially deacidifying, dehydrating and drying to obtain a remaining sample;
[0010] Step 4: weigh the remaining sample obtained in step 4 to obtain the remaining mass, and then subtract the remaining mass from the original mass obtained in step 1 to obtain the actual mass of the powder in the short sample;
[0011] Step 5: Analyze the metallographic image obtained in step 1 to obtain the area of the powder in the Bi-based wire, then calculate the volume of the powder in the short sample based on the length of the short sample, and then divide the actual mass of the powder by the volume of the powder in the short sample to obtain the average density of the powder in the Bi-based wire.
[0012] The above-mentioned method for measuring the average density of powder in Bi-based wire is characterized in that the total number of core wires of the Bi-based wire in step 1 is not more than 990, and the core wire size is not less than 100 μm. The present invention controls the total number of core wires and the core wire size of the Bi-based wire to prevent the deficiency of too many core wires and too small core wire size reducing the efficiency and accuracy of the test.
[0013] The above method for measuring the average density of powder in Bi-based wire is characterized in that the length of the short sample in step 2 is 3 mm to 10 mm. The present invention improves the test efficiency while ensuring the accuracy of the test results by controlling the length of the short sample.
[0014] The above method for measuring the average density of powder in Bi-based wire is characterized in that the temperature of the heating reflux in step 3 is 120°C to 140°C and the time is 12h to 24h. The present invention controls the temperature and time of the heating reflux so that the powder in the short sample is fully dissolved by glacial acetic acid, thereby improving the accuracy of the calculation of the average density of powder in Bi-based wire.
[0015] The above method for measuring the average density of powder in Bi-based wire is characterized in that the accuracy of the original mass in step 2 and the residual mass in step 4 is better than 0.001 g. The present invention improves the accuracy of the average density of powder in Bi-based wire by controlling the accuracy of the mass.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] 1. The present invention uses glacial acetic acid as an etchant, and slowly dissolves the powder in the Bi-based wire under stirring and high-temperature reflux conditions. After the reaction is completed, the mass of the powder in the Bi-based wire is obtained by calculating the mass difference before and after dissolution. The metallographic diagram is used for analysis to confirm the area of the powder in the wire. Combined with the length, shape and other information of the Bi-based wire, the volume occupied by the powder in the Bi-based wire is calculated. Finally, the powder mass is divided by the powder volume to obtain the average density of the powder in the Bi-based wire. The average density of the powder in the Bi-based wire is quickly obtained to guide the processing technology.
[0018] 2. The present invention studies whether the Ag / powder complex deforms synchronously during the deformation process and the corresponding deformation law by measuring the average density of powders in different sizes and different parts of the wire.
[0019] 3. The present invention improves the test efficiency while ensuring the accuracy of the test results by controlling the length of the short sample; by controlling the temperature and time of heating reflux, the powder in the short sample is fully dissolved by glacial acetic acid, thereby improving the accuracy of the calculation of the average density of the powder in the Bi-based wire.
[0020] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION
[0021] Example 1
[0022] This embodiment includes the following steps:
[0023] Step 1: Clean the surface of the Bi2223 wire with a diameter of 3.50 mm and remove surface impurities and oil stains, dry it at 80°C, then cut off 1.5 cm and perform metallographic analysis to obtain a metallographic diagram;
[0024] Step 2: Cut the Bi2223 wire after drying in step 1, and then process the cut part to obtain a short sample of a standard column with a length of 9.04 mm, and then weigh the short sample to obtain an original mass of 0.845 g;
[0025] Step 3: Place the short sample weighed in step 2 into a round-bottom flask filled with glacial acetic acid, and then heat to 120° C. in an oil bath and reflux for 24 h with stirring. Then take out the remaining solid and perform deacidification, dehydration and drying at 100° C. in sequence to obtain a remaining sample;
[0026] Step 4: weigh the remaining sample obtained in step 4 to obtain a remaining mass of 0.706 g, and then subtract the remaining mass from the original mass obtained in step 1 to obtain an actual mass of the powder in the short sample of 0.139 g;
[0027] Step 5: Analyze the metallographic image obtained in step 1 using ImageJ image analysis software to obtain the area of the powder in the Bi2223 wire, and then calculate the volume of the powder in the short sample based on the length of the short sample to be 25.965mm 3 , and then the actual mass of the powder is divided by the volume of the powder in the short sample, and the average density of the powder in the Bi2223 wire is 5.353 g / cm 3 .
[0028] Example 2
[0029] This embodiment includes the following steps:
[0030] Step 1: Clean the surface of the Bi2212 wire with a core diameter of 990 and a diameter of 10.00 mm to remove surface impurities and oil stains, dry it at 100°C, then cut off 1.0 cm and perform metallographic analysis to obtain a metallographic diagram;
[0031] Step 2: Cut the Bi2212 wire after drying in step 1, and then process the cut part to obtain a short sample of a standard column with a length of 5.12 mm, and then weigh the short sample to obtain an original mass of 3.640 g;
[0032] Step 3: Place the short sample weighed in step 2 into a round-bottom flask filled with glacial acetic acid, and then heat to 140°C in an oil bath and reflux for 12 hours with stirring, then take out the remaining solid and perform deacidification, dehydration and drying at 80°C in sequence to obtain the remaining sample;
[0033] Step 4: weigh the remaining sample obtained in step 4 to obtain a remaining mass of 3.259 g, and then subtract the remaining mass from the original mass obtained in step 1 to obtain an actual mass of 0.381 g of the powder in the short sample;
[0034] Step 5: Analyze the metallographic image obtained in step 1 using ImageJ image analysis software to obtain the area of the powder in the Bi2212 wire, and then calculate the volume of the powder in the short sample based on the length of the short sample to be 67.126 mm 3 , and then the actual mass of the powder is divided by the volume of the powder in the short sample, and the average density of the powder in the Bi2212 wire is 5.676 g / cm 3 .
[0035] Example 3
[0036] This embodiment includes the following steps:
[0037] Step 1: Clean the surface of the Bi2212 wire with a core diameter of 990 mm and a diameter of 10.00 mm to remove surface impurities and oil stains, dry it at 90°C, then cut off 1.2 cm and perform metallographic analysis to obtain a metallographic diagram;
[0038] Step 2: Cut the Bi2212 wire after drying in step 1, and then process the cut part to obtain a short sample of a standard column with a length of 3.15 mm, and then weigh the short sample to obtain an original mass of 2.244 g;
[0039] Step 3: Place the short sample weighed in step 2 into a round-bottom flask filled with glacial acetic acid, and then heat to 130° C. in an oil bath and reflux for 18 h with stirring. Then take out the remaining solid and perform deacidification, dehydration and drying at 90° C. in sequence to obtain a remaining sample;
[0040] Step 4: weigh the remaining sample obtained in step 4 to obtain a remaining mass of 2.012 g, and then subtract the remaining mass from the original mass obtained in step 1 to obtain an actual mass of the powder in the short sample of 0.232 g;
[0041] Step 5: Analyze the metallographic image obtained in step 1 using ImageJ image analysis software to obtain the area of the powder in the Bi2212 wire, and then calculate the volume of the powder in the short sample based on the length of the short sample to be 41.295 mm 3 , and then the actual mass of the powder is divided by the volume of the powder in the short sample, and the average density of the powder in the Bi2212 wire is 5.618 g / cm 3 .
[0042] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for measuring the average density of powder in Bi-based wire, characterized in that: The method comprises the following steps: Step 1: Clean and dry the Bi series wire in sequence, then cut it and perform metallographic analysis on the cut part to obtain a metallographic diagram; Step 2: Cut the Bi series wire after drying in step 1, and then process the cut part to obtain a short sample of standard columnar shape, and then weigh the short sample to obtain the original mass; Step 3, placing the short sample weighed in step 2 into a container filled with glacial acetic acid, and then heating and refluxing in an oil bath with stirring, and then taking out the remaining solid and sequentially deacidifying, dehydrating and drying to obtain a remaining sample; Step 4: weigh the remaining sample obtained in step 4 to obtain the remaining mass, and then subtract the remaining mass from the original mass obtained in step 1 to obtain the actual mass of the powder in the short sample; Step 5: Analyze the metallographic image obtained in step 1 to obtain the area of the powder in the Bi-based wire, then calculate the volume of the powder in the short sample based on the length of the short sample, and then divide the actual mass of the powder by the volume of the powder in the short sample to obtain the average density of the powder in the Bi-based wire.
2. A method for measuring the average density of powder in Bi-based wire according to claim 1, characterized in that: The total number of core wires of the Bi-based wire in step 1 is not greater than 990, and the size of the core wire is not less than 100 μm.
3. A method for measuring the average density of powder in Bi-based wire according to claim 1, characterized in that: The length of the short sample in step 2 is 3 mm to 10 mm.
4. A method for measuring the average density of powder in Bi-based wire according to claim 1, characterized in that: The heating reflux temperature in step 3 is 120° C. to 140° C., and the time is 12 h to 24 h.
5. The method for measuring the average density of powder in Bi-based wire according to claim 1, characterized in that: The accuracy of the original mass described in step 2 and the residual mass described in step 4 is better than 0.001 g.