Mask blank substrate and manufacturing method thereof
By using local processing and fine polishing steps, the flatness of the mask preform substrate is predicted and corrected, solving the problem of insufficient flatness in high-NA exposure in extreme ultraviolet lithography, and realizing the manufacturing of mask preform substrates with high transfer accuracy and high productivity.
Patent Information
- Application Number
- CN202410653073.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies struggle to achieve high transfer accuracy during high-NA exposure in extreme ultraviolet lithography (EUVL), primarily due to insufficient flatness of the glass substrate, especially the measurement difficulties and excessively high flatness requirements caused by the refractive index distribution of multi-component glass substrates.
By using local processing and fine polishing steps, the flatness of the mask substrate is predicted and evaluated to ensure that TTV1 in the simulated TTV diagram is below 35nm and TTV2 is below 25nm. A 152mm×152mm square main surface and a 6.35mm thick substrate are used. By combining local processing and fine polishing steps, the shape changes of the main surface are predicted and corrected to achieve the predetermined flatness.
It achieves high transfer accuracy and high productivity during high NA EUVL exposure, and provides a mask preform substrate with good exposure performance, suitable for next-generation high NA EUV exposure apparatus.
Smart Images

Figure CN119024637A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a mask blank substrate for photolithography and a method for manufacturing the same, and more particularly to a mask blank substrate suitable for manufacturing a transfer mask for photolithography using extreme ultraviolet (EUV) light for exposure light and a method for manufacturing the same. Background Art
[0002] In recent years, as AI and IoT have attracted attention, arithmetic processing of large amounts of data has become necessary, and therefore speeding up arithmetic processing and energy saving are required. In order to meet these requirements, it is necessary to improve the performance of IC chips, and miniaturization of electrical wiring is generally adopted as an effective method. For miniaturization of wiring, high NA, exposure light with a short wavelength, etc. are mainly used, but in recent years, extreme ultraviolet (EUV) lithography (EUVL) using EUV light has been put into practical use.
[0003] In EUVL, the exposure mask is one of the important elements, and in order to achieve accurate exposure, it is extremely important to improve the flatness of the glass substrate of the original plate (mask blank) of the exposure mask. As a common manufacturing method of a glass substrate, double-sided simultaneous polishing is mainly used, but the flatness good enough for EUVL cannot be obtained only by double-sided simultaneous polishing. In order to achieve high flatness, it is necessary to improve the flatness according to the surface shape by polishing one side at a time, and local processing techniques such as local etching or local polishing are used for this purpose. These are methods of making the entire substrate almost flat by removing relatively protruding areas on the main surface of the substrate. In addition, the surface shape of the exposure mask can be optically corrected using the wavefront correction function of the exposure device, and the exposure mask can have high flatness optically.
[0004] With the trend of miniaturization in recent years, EUVL is also required to have a high NA, and the flatness requirements are becoming more and more stringent. The flatness requirements have reached a range that cannot be achieved by pursuing polishing technology alone, and it has been required to selectively manufacture a glass substrate with a shape that can be used for exposure rather than just using flatness as an indicator.
[0005] Examples of indicators closely related to such performance include TTV of a glass substrate. TTV has been used for performance evaluation of a single-component glass substrate. A transmission optical system is suitable for measuring substrate thickness distribution (TTV diagram), and it is easy to measure the TTV diagram of a single-component glass. However, in a multi-component glass substrate used for EUVL, a refractive index distribution caused by fluctuations in the concentration of the glass components occurs, and it is difficult to measure the TTV diagram in an optically accurate manner. Therefore, it is necessary to use a simulated TTV diagram (hereinafter referred to as a pseudo-TTV diagram) obtained by adding the surface shapes of the first main surface and the second main surface, respectively.
[0006] For example, in WO 2016 / 098452 (Patent Document 1), when a reflective mask prepared by using a substrate having both a front main surface and a rear main surface that have undergone conventional double-sided polishing and local processing is adsorbed to an exposure device for exposure transfer, in order to obtain high transfer accuracy, if during electrostatic adsorption the shape of the front main surface of the substrate is made close to a shape defined by a Zernike polynomial that can be corrected by the wavefront correction function of the exposure device (virtual surface shape), then even if the substrate has a substrate thickness fluctuation that affects changes in the shape of the front main surface, it may tend to be easy to correct the substrate thickness fluctuation by the wavefront correction function of the exposure device, and using a transfer mask having such a substrate, the transfer pattern can be exposed and transferred to the transfer object in a highly precise manner.
[0007] Reference List
[0008] Patent Document 1: WO 2016 / 098452
[0009] Patent Document 2: JP-A 2010-194705 Summary of the invention
[0010] The method described in WO 2016 / 098452 (Patent Document 1) includes a process of calculating a composite plane of the front main surface and the rear main surface during adsorption to an exposure device, a process of fitting the composite plane with a Zernike polynomial, and a process of subtracting the fitted shape from the composite plane to predict the surface shape after optical correction. However, this method defines the flatness in a circular area with a diameter of 104 mm, which is insufficient for the area actually used for exposure (132 mm×104 mm square). In addition, the steep shape of the outermost circumference tends to be corrected more strongly by excluding higher-order terms from the fourth to sixth terms of the Legendre polynomial. In this case, correction is applied to a shape that would adversely affect exposure if not corrected, so that TTV is evaluated as good.
[0011] The present invention is proposed in view of the above situation, and its purpose is to provide a mask blank substrate and a method for manufacturing such a mask blank substrate with high productivity. The mask blank substrate provides an exposure mask that can achieve transfer accuracy that is extremely advantageous for next-generation high-NA EUV exposure during exposure using the exposure mask, especially during exposure using EUVL.
[0012] As a result of intensive studies to solve the above-mentioned problems, the present inventors have found that a mask blank substrate having two main surfaces of a first main surface and a second main surface of a square shape of 152 mm×152 mm and a thickness of 6.35 mm becomes sufficiently flat during electrostatic attraction of an exposure machine, and an exposure mask having good transfer performance can be provided, wherein when a cross-shaped area is set, the cross-shaped area is formed in the case of creating a pseudo-TTV map by adding height maps of the first main surface and the second main surface, and in the pseudo-TTV map, a first rectangular area of 132 mm×104 mm coincides with a second rectangular area of 104 mm×132 mm, and the first rectangular area The four sides are parallel to the main surface and are centered on the intersection of the diagonals of the main surface. The second rectangular area is orthogonal to the first rectangular area and is parallel to the four sides of the main surface and is centered on the intersection of the diagonals of the main surface. In the cross-shaped area, in the fitting of the pseudo-TTV diagram, when a plane function approximated by a first-order polynomial is derived, the difference between the highest and lowest heights of the TTV1 diagram excluding the first-order component (TTV1) is less than 35nm, and in the fitting of the pseudo-TTV diagram, when a surface function approximated by a highest second-order polynomial is derived, the difference between the highest and lowest heights of the TTV2 diagram excluding the first-order and second-order components (TTV2) is less than 25nm.
[0013] Furthermore, the present inventors have found that a mask blank substrate that is sufficiently flat during electrostatic adsorption of an exposure machine and provides an exposure mask with good transfer performance can be reliably and efficiently manufactured by manufacturing a mask blank substrate by the following method, the method including a local processing step and a fine polishing step after the local processing step, predicting the shape of the main surface after the fine polishing step by applying a change in the shape of the main surface after the fine polishing step grasped in advance to the shape of the main surface before the fine polishing step in the local processing step after the local processing step, and evaluating whether the predicted shape of the main surface is a shape imparting a predetermined flatness, and have completed the present invention.
[0014] Therefore, the present invention provides the following mask blank substrate and a method for manufacturing the mask blank substrate.
[0015] 1. A mask blank substrate having two main surfaces, a first main surface and a second main surface, of a 152 mm×152 mm square and a thickness of 6.35 mm, wherein
[0016] In the pseudo-TTV map obtained by adding the height map of the first main surface and the height map of the second main surface based on the position of each of the first main surface and the second main surface on the respective least squares planes,
[0017] In the fitting of the pseudo-TTV graph, when a plane function approximated by a first-order polynomial is derived, the difference between the highest height and the lowest height of the TTV1 graph excluding the first-order component (TTV1) is 35 nm or less, and in the fitting of the pseudo-TTV graph, when a surface function approximated by a highest second-order polynomial is derived, the difference between the highest height and the lowest height of the TTV2 graph excluding the first-order component and the second-order component (TTV2) is 25 nm or less,
[0018] In the cross-shaped area formed when the first rectangular area of 132mm×104mm overlaps with the second rectangular area of 104mm×132mm, the first rectangular area is parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate, and the second rectangular area is orthogonal to the first rectangular area and parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate.
[0019] 2. The mask blank substrate according to 1, wherein the flatness of the first main surface in the cross-shaped region is 35 nm or less.
[0020] 3. A method for manufacturing a mask blank substrate, the mask blank substrate having two main surfaces, a first main surface and a second main surface, of a square shape of 152 mm×152 mm and a thickness of 6.35 mm, the manufacturing method comprising:
[0021] a local processing step of at least one of the first main surface and the second main surface and a fine polishing step after the local processing step, wherein
[0022] The local processing steps include:
[0023] (A) a step of locally processing at least one of the first main surface and the second main surface;
[0024] (B) a step of measuring the shape of the main surface partially processed after the step (A) as the shape of the main surface before the finish polishing step;
[0025] (C) a step of predicting the shape of the locally processed main surface after the finish polishing step by applying the change in the surface shape in the finish polishing step grasped in advance to the shape of the main surface before the finish polishing step obtained in step (B); and
[0026] (D) A step of evaluating whether the shape after the fine polishing step predicted in step (C) is a shape that produces a predetermined TTV.
[0027] 4. The manufacturing method according to 3, wherein the shape of the predetermined TTV generated in step (D) is a shape in a predicted pseudo-TTV map within a cross-shaped region formed in the following case:
[0028] (1) The first main surface and the second main surface of the substrate are arranged in a substantially vertical direction, and a calculation area of a square tubular shape is set, the calculation area extending in the horizontal direction through four sides of a square of 132 mm×132 mm along four sides of the first main surface and the second main surface at the central part of the first main surface and the second main surface;
[0029] (2) cutting out a portion of the first main surface within the calculation area while facing the first main surface as the first area surface;
[0030] (3) setting a vertical plane that passes through a reference point that is an arbitrary point on the central axis of the square prism in the calculation area and is orthogonal to the central axis as a reference plane, setting a rotation axis that passes through the reference point and is parallel to any one of the four sides of a square that is an intersection line between the square prism in the calculation area and the vertical plane, and, by rotating the substrate 180 degrees along the rotation axis from a state facing the first main surface, cutting out a portion of the second main surface in the calculation area in a state facing the second main surface as a second area surface;
[0031] (4) calculating a least squares plane in each of the first area surface and the second area surface;
[0032] (5) converting the first area surface and the second area surface into a height map of the first area surface and a height map of the second area surface based on a position of each of the first area surface and the second area surface on a respective least squares plane;
[0033] (6) setting the height map of the second region surface as an inverted height map of the second region surface by moving the height map symmetrically relative to a vertical plane passing through the rotation axis and along the 90 degree direction of the rotation;
[0034] (7) creating a predicted pseudo-TTV map by adding the height of the height map of the first regional surface and the height of the inverted height map of the second regional surface at their respective positions (X coordinate, Y coordinate) on the reference plane; and
[0035] (8) In the predicted pseudo-TTV diagram, a first rectangular area of 132 mm×104 mm overlaps with a second rectangular area of 104 mm×132 mm, the first rectangular area is parallel to the four sides of the main surface of the substrate and is centered at the intersection of the diagonals of the main surface of the substrate, and the second rectangular area is orthogonal to the first rectangular area and is parallel to the four sides of the main surface of the substrate and is centered at the intersection of the diagonals of the main surface of the substrate.
[0036] In the fitting of the predicted pseudo-TTV diagram, when a plane function approximated by a first-order polynomial is derived, the difference between the highest and lowest heights of the TTV1' diagram excluding the primary component (TTV1') is less than 35nm, and, in the fitting of the predicted pseudo-TTV diagram, when a surface function approximated by a second-order polynomial is derived, the difference between the highest and lowest heights of the TTV2' diagram excluding the primary and secondary components (TTV2') is less than 25nm.
[0037] Beneficial Effects of the Invention
[0038] The mask blank substrate of the present invention can provide an exposure mask having a highly flat shape when the exposure mask is electrostatically adsorbed to an exposure device during exposure using an exposure mask, particularly during exposure using a high NA EUVL. In addition, according to the method for manufacturing a mask blank substrate of the present invention, such a mask blank substrate can be reliably manufactured with high productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1A and 1B 1 is a view for explaining the state of the mask blank substrate of the present invention, wherein Figure 1A is a side view of a state in which the first main surface and the second main surface of the mask blank substrate are arranged in a vertical direction, Figure 1B is located in Figure 1A A front view of the first main surface on the right side of the middle;
[0040] Figure 2A and 2B 1 is a view for explaining the state of the mask blank substrate of the present invention, wherein Figure 2A is a side view of the mask blank substrate after being rotated 180 degrees, Figure 2B is located after rotation Figure 2A A front view of the second main surface on the right side of the center;
[0041] Figures 3A to 3C 1 is a view for explaining the state of the mask blank substrate of the present invention, wherein Figure 3A is the height map of the first region surface, Figure 3B is the height map of the second region surface, Figure 3C is the inverted height map of the second region surface;
[0042] Figure 4 is a view for explaining the state of the mask blank substrate of the present invention, and is a pseudo-TTV map (map of the Z coordinate) obtained from the height map of the first region surface and the inverted height map of the second region surface; and
[0043] Figures 5A to 5C 1 is a view for explaining the state of the mask blank substrate of the present invention, wherein Figure 5Ais a diagram showing a cross-shaped area as an object area for evaluation in a pseudo-TTV diagram, Figure 5B is a view showing a first rectangular region (vertical long region) constituting a cross-shaped region, Figure 5C : is a view showing a second rectangular region (horizontally long region) constituting the cross-shaped region. DETAILED DESCRIPTION
[0044] The present invention is described in detail below.
[0045] The mask blank substrate of the present invention has two main surfaces, the first main surface and the second main surface, which are 152 mm×152 mm square and a thickness of 6.35 mm. A substrate of this size is called a so-called 6025 substrate, and is a substrate having two main surfaces, the first main surface and the second main surface, which are 6 inches×6 inches square and a thickness of 0.25 inches.
[0046] The material of the mask blank substrate of the present invention may be a conventionally used material and is not particularly limited. However, when drawing a fine pattern, the substrate is exposed to high-energy exposure light, and thus TiO2-doped quartz glass containing 3 to 10 wt% of TiO2 having very high dimensional stability at high temperatures is suitably used. As a raw material substrate of the mask blank substrate, a substrate synthesized, molded, and processed according to a conventional method can be used.
[0047] The mask blank substrate is required to have high flatness. This is because the higher the flatness, the easier it is to achieve the target exposure, and it can be said that a substrate with higher flatness is a mask blank substrate suitable for drawing fine patterns. The mask blank substrate has a first main surface on which an exposure pattern (such as a wiring pattern) is formed after film formation and a second main surface on which no exposure pattern is formed, and the second main surface is adsorbed and held by an exposure machine. Among them, in the most advanced applications, since a reflective mask is mainly used, the flatness of the first main surface is required to be at an extremely high level. Therefore, in order to improve the flatness of the first main surface, various studies have been conducted on flattening based on local processing technology.
[0048] On the other hand, there is a wavefront correction function as a function on the exposure machine side. This is a function for optically correcting the surface shape even for a substrate with low flatness, so that even a substrate with low flatness actually obtains an exposure result equivalent to that of a substrate with high flatness.
[0049] In a pseudo-TTV map obtained by adding a height map of the first main surface and a height map of the second main surface based on the position of each of the first main surface and the second main surface on their respective least squares planes, the mask blank substrate of the present invention has a difference between the highest and lowest heights of the TTV map excluding the primary component (TTV1) of less than 35 nm and a difference between the highest and lowest heights of the TTV map excluding the primary component and the secondary component (TTV2) of less than 25 nm in a cross-shaped area formed when a first rectangular area of 132 mm×104 mm and a second rectangular area of 104 mm×132 mm overlap, the first rectangular area is parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate, and the second rectangular area is orthogonal to the first rectangular area and parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate.
[0050] In particular, it is preferred that in the mask blank substrate of the present invention,
[0051] In the pseudo-TTV map within the cross-shaped region, the difference between the highest height and the lowest height of the TTV1 map excluding the primary component (TTV1) is 35 nm or less, and the difference between the highest height and the lowest height of the TTV2 map excluding the primary component and the secondary component (TTV2) is 25 nm or less, and the cross-shaped region is formed under the following conditions:
[0052] (1) The first main surface and the second main surface of the substrate are arranged in a substantially vertical direction, and a calculation area of a square tubular shape is set, the calculation area extending in the horizontal direction through four sides of a square of 132 mm×132 mm along four sides of the first main surface and the second main surface at the central part of the first main surface and the second main surface;
[0053] (2) in a state facing the first main surface, cutting out a portion of the first main surface within the calculation area as a first area surface;
[0054] (3) setting a vertical plane that passes through a reference point that is an arbitrary point on the central axis of the square prism in the calculation area and is orthogonal to the central axis as a reference plane, setting a rotation axis that passes through the reference point and is parallel to any one of four sides of a square that is an intersection line between the square prism in the calculation area and the vertical plane, and cutting out a portion of the second main surface in the calculation area in a state facing the second main surface as a second area surface by rotating the substrate 180 degrees along the rotation axis from a state facing the first main surface;
[0055] (4) calculating a least squares plane in each of the first area surface and the second area surface;
[0056] (5) converting the first area surface and the second area surface into a height map of the first area surface and a height map of the second area surface based on a position of each of the first area surface and the second area surface on a respective least squares plane;
[0057] (6) setting the height map of the second region surface as an inverted height map of the second region surface by symmetrically moving the height map relative to a vertical plane passing through the rotation axis in (3) and along a 90 degree direction of the rotation in (3);
[0058] (7) creating a pseudo-TTV map by adding the height of the height map of the first regional surface and the height of the inverted height map of the second regional surface at their respective positions (X coordinate, Y coordinate) on the reference plane; and
[0059] (8) In the pseudo-TTV diagram, a first rectangular area of 132 mm × 104 mm overlaps with a second rectangular area of 104 mm × 132 mm, the first rectangular area is parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate, and the second rectangular area is orthogonal to the first rectangular area and is parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate.
[0060] refer to Figure 1A and Figures 1B to 4 The above (1) to (8) are specifically described to explain the state of the mask blank substrate of the present invention. Figure 1A and Figure 1B middle, Figure 1A is a side view of a state in which the first main surface and the second main surface of the mask blank substrate are arranged in a vertical direction, Figure 1B is located in Figure 1A A front view of the first main surface on the right side of FIG. In (1), as Figure 1A As shown in the figure, the 152mm×152mm square first main surface 1 and the second main surface 2 of the substrate 500 are basically arranged in the vertical direction, and a calculation area C of a square tubular shape is set, which extends in the horizontal direction along the four sides of the first main surface 1 and the second main surface 2 in the central part of the first main surface 1 and the second main surface 2 through the four sides of the 132mm×132mm square.
[0061] Next, in (2), if Figure 1B As shown in FIG. 1 , in a state facing the first main surface 1, a portion of the first main surface 1 in the calculation area C is cut out as the first area surface 11. For convenience, it is assumed that there is a convex portion 11a on the first main surface 1, and as will be described below Figure 2B As shown in FIG. 2 , there are also protrusions 21 a on the second major surface 2 .
[0062] Next, in (3), if Figure 1A and 1B As shown in , a vertical plane passing through a reference point P which is an arbitrary point on the central axis CA of the square prism in the calculation area C and which is orthogonal to the central axis CA is set as a reference plane S (here, the reference plane S is a plane extending in the depth direction of the figure), and a rotation axis RA is set which passes through the reference point P and is parallel to any one of the four sides of a square which is an intersection line between the square prism in the calculation area C and the vertical plane. Then, the substrate 500 is rotated 180 degrees along the rotation axis RA (about the rotation axis RA) from the state facing the first main surface 1.
[0063] On the other hand, Figure 2A and Figure 2B middle, Figure 2A is a side view of the mask blank substrate after being rotated 180 degrees. Figure 2B After rotation, it is located Figure 2A After the substrate 500 is rotated, as shown in FIG. Figure 2B As shown in , in a state facing the second main surface 2 , a portion of the second main surface 2 within the calculation area C is cut as a second area surface 21 .
[0064] Next, in (4), a least square plane is calculated in each of the first area plane 11 and the second area plane 21, and, in (5), the first area plane 11 and the second area plane 21 are converted into a plane having a least square plane as a reference based on the position of each of the first area plane 11 and the second area plane 21 on the respective least square planes. Figure 3A The height map 111 of the first area surface shown in FIG. Figure 3B The height map 211 of the second region surface shown in FIG. In addition, in (6), as Figure 3B As shown in FIG. 2 , the height map 211 of the second region surface is symmetrically moved relative to the vertical plane V (here, the vertical plane V is a plane extending in the depth direction of the figure) and as shown in FIG. Figure 3C The vertical plane V shown in FIG. 211 is set as the inverted height map 211R of the second region surface, and passes through the rotation axis RA in (3) and is along the 90-degree rotation direction in (3). Note that due to Figure 3C The inverted height map 211R of the second region surface shown in is obtained by symmetrically moving the height map 211, so 21aR in the inverted height map 211R is not inverted in the height direction and is a convexity similar to 21a.
[0065] Next, in (7), Figure 3A The height map 111 of the first area surface shown in FIG. Figure 3C The inverted height map 211R of the second region surface shown in FIG. 211 coincides, and Figure 1AFor each position (X coordinate, Y coordinate) on the reference plane S shown in FIG. 1 , the height of the height map 111 of the first area surface and the height of the inverted height map 211R of the second area surface are added to create a Figure 4 The pseudo-TTV map (map of the Z coordinate) shown in 3.
[0066] Next, in (8), in the pseudo-TTV graph obtained in (7), cut out Figure 5A The cross-shaped area 31 shown in FIG. 1 is formed when a first rectangular area (vertical long area) 31a of 132 mm×104 mm and a second rectangular area (horizontal long area) 31b of 104 mm×132 mm overlap to evaluate the parameters (TTV1 and TTV2) obtained by numerically processing the pseudo-TTV of the pseudo-TTV diagram within the cross-shaped area 31. Figure 5B As shown in , the first rectangular region is parallel to the four sides of the main surface (first main surface or second main surface) 10 of the substrate 500, with the intersection of the diagonal lines of the main surface of the substrate as the center, as shown in Figure 5C As shown in , the second rectangular region is orthogonal to the first rectangular region 31 a and parallel to four sides of the main surface (the same main surface) 10 of the substrate 500 , centered at the intersection of the diagonal lines of the main surface of the substrate.
[0067] The minimum area on the main surface of the substrate that can be used for exposure is a first rectangular area of 132 mm × 104 mm with four sides parallel to the main surface of the substrate and centered at the intersection of the diagonal lines of the main surface, and a second rectangular area of 104 mm × 132 mm with four sides parallel to the main surface of the substrate and centered at the intersection of the diagonal lines of the main surface of the substrate. For the pseudo-TTV diagram, a cross-shaped area where the two rectangular areas overlap with each other is effective as the object. Therefore, in the present invention, the cross-shaped area is set as the object area for evaluation.
[0068] In the present invention, TTV is used as an index of the shape of a mask blank substrate that can be effectively used for exposure in a multi-component glass substrate for EUVL. In the pseudo-TTV diagram, TTV1 calculated from the TTV1 diagram excluding the primary component as a simple component and TTV2 calculated from the TTV2 diagram excluding the primary component and the secondary component as slightly complex components are important indicators that greatly affect the exposure performance. In the fitting of the pseudo-TTV diagram, when a plane function approximated by a first-order polynomial (specifically, a function represented by the following expression (1)) or a surface function approximated by a highest second-order polynomial (specifically, a function represented by the following expression (2)) is derived, the linear function component is the primary component and the quadratic function component is the quadratic component.
[0069] Here, the method for calculating TTV1 and TTV2 is described. First, a pseudo TTV map (S) is created with the center of the substrate as the origin, the horizontal axis as x [mm], the vertical axis as y [mm], and the height direction as z [nm]. TTV ). Next, the pseudo-TTV graph is approximated by the following expressions (1) and (2).
[0070] S′ TTV1 =a1x+a2y (1)
[0071] S′ TTV2 =b1x+b2y+b3x 2 +b4xy+b5y 2 (2)
[0072] In the expressions, a1, a2, b1, b2, b3, b4 and b5 are all constants. As shown in the following expressions (3) and (4), from the pseudo-TTV diagram (S TTV ) minus the approximate expression S'(S' TTV1 and S' TTV2 ), as TTV1 map (S TTV1 ) and TTV2 graph (S TTV2 ).
[0073] S TTV1 =S TTV -S′ TTV1 (3)
[0074] S TTV2 =S TTV -S′ TTV2 (4)
[0075] Then, the TTV1 map (S TTV1 The difference between the highest and lowest heights of the graph (S) is defined as TTV1, and the TTV2 graph (S TTV2 ) is defined as the difference between the highest altitude and the lowest altitude.
[0076] The steeper the shape of the periphery, the more likely it is to have a negative impact on exposure. Such a shape can be considered to be composed mainly of secondary or higher-order components. Therefore, by excluding only the primary component and evaluating TTV1 in which the secondary or higher-order components are retained, exposure failure due to the steep shape of the periphery can be avoided. In addition, the wavefront correction function of the exposure machine is usually well approximated by the highest secondary component. In other words, a substrate with a poor pseudo-TTV calculated by excluding the component of the highest secondary component can be designated as a substrate that is difficult to correct by the wavefront correction function, and a substrate that is easy to correct by the wavefront correction function can be selected by evaluating TTV2 excluding the primary and secondary components.
[0077] The measurement of the main surface shape of the mask blank substrate is not particularly limited, but a laser interferometer can be used, for example. The shape that can be measured by the laser interferometer is the raw data of the height map of the main surface of the substrate, and, in this case, the height reference is the platform on which the substrate is placed during measurement. In the present invention, for the height map of the main surface of the substrate, the least square plane of the main surface (the least square plane of the surface or the height map) is calculated and corrected to the height map based on the least square plane, thereby eliminating the influence due to the shape of the platform on which the substrate is placed.
[0078] In the height map corrected in this manner, the inverted height map of the second region surface obtained by symmetrically moving the height map of the second region surface with respect to the plane passing through the rotation axis in (3) and along the 90-degree rotation direction in (3) as a reference has both sides inverted in the direction orthogonal to the rotation axis in (3), although the positive and negative sides in the height direction remain unchanged. The pseudo-TTV map can be calculated by adding the inverted height maps of the first main surface and the second main surface, thereby obtaining the substrate thickness distribution of the mask blank substrate. Here, the pseudo-TTV is the difference between the highest value (highest height) and the lowest value (lowest height) within a predetermined range.
[0079] For the pseudo-TTV of the mask blank substrate of the present invention, the difference (TTV1) between the highest height and the lowest height of the TTV1 figure (pseudo-TTV1 figure) excluding the primary component is 35 nm or less, preferably 30 nm or less, and more preferably 25 nm or less. If TTV1 is 35 nm or less, such a mask blank substrate is a mask blank substrate that can advantageously achieve exposure with good transfer accuracy during exposure using an exposure mask obtained from the mask blank substrate through the mask blank. On the other hand, if TTV1 is greater than 35 nm, such a mask blank substrate is disadvantageous in terms of transfer accuracy.
[0080] Furthermore, for the pseudo-TTV of the mask blank substrate of the present invention, the difference (TTV2) between the highest height and the lowest height of the TTV2 graph (pseudo-TTV2 graph) excluding the primary component and the secondary component is 25 nm or less, preferably 20 nm or less, and more preferably 18 nm or less. Such a mask blank substrate is a mask blank substrate that can advantageously achieve exposure with good transfer accuracy during exposure using an exposure mask obtained from the mask blank substrate through the mask blank.
[0081] TTV1 is calculated from the TTV1 graph excluding the primary component in the pseudo-TTV graph, and TTV1 can be said to be similar to flatness. However, in the present invention, the upper limit (threshold) of TTV2 calculated from the TTV2 graph excluding (relaxing) the primary component and the secondary component in the pseudo-TTV graph is 25 nm or less. TTV2 reflects the actual flatness during exposure more than TTV1, and a mask blank substrate having TTV1 and TTV2 within a predetermined range is a mask blank substrate that can achieve good exposure when actually subjected to exposure, and can provide a photomask blank having high exposure performance.
[0082] Conventionally, for example, a range of 138 mm × 138 mm parallel to the four sides of the main surface of the substrate, centered at the intersection of the diagonal lines of the main surface, has been evaluated, but this range extends to include not only the range of the area used for exposure, but also the range of the portion of the main surface on the side that is vacuum-adsorbed to the exposure device, which is vacuum-adsorbed to the exposure device. In the present invention, a cross-shaped area obtained by overlapping the above two areas of 132 mm × 104 mm is set as a target for evaluation. This cross-shaped area is a range narrower than the conventional range, but the range outside the cross-shaped area is a range that is not usually used for exposure and tends to have a high flatness.
[0083] Although the mask blank substrate of the present invention has a TTV1 below 35nm and a TTV2 below 25nm in the above-mentioned cross-shaped area, the mask blank substrate of the present invention can be applied not only to the traditional NA0.33 generation, but also to the NA0.55 generation which requires more stringent flatness, and can be suitable for application as a mask blank substrate for the next generation EUV exposure device.
[0084] Furthermore, when the side on which the optical film is formed is set as the first main surface and the side to be vacuum-drawn to the exposure device is set as the second main surface, at least one of the flatness of the first main surface in the cross-shaped region and the flatness of the second main surface in the cross-shaped region of the mask blank substrate of the present invention, preferably the flatness of the first main surface in the cross-shaped region, is preferably 35 nm or less, more preferably 20 nm or less, and still more preferably 18 nm or less. Such a mask blank substrate is a mask blank substrate that can more favorably achieve exposure with good transfer accuracy during exposure using an exposure mask obtained from the mask blank substrate through the mask blank.
[0085] Next, a method for manufacturing the mask blank substrate of the present invention is described.
[0086] The method for manufacturing a mask blank substrate of the present invention includes a local processing step of at least one of a first main surface and a second main surface of the mask blank substrate, and a finish polishing step after the local processing step.
[0087] In the manufacture of the mask blank substrate, the raw material substrate for the mask blank substrate is prepared from a glass ingot before the local processing step, but the raw material substrate for the mask blank substrate can be prepared by first cutting the glass ingot into a predetermined shape, performing profile processing, and then polishing the main surface and the end surface. Polishing can be performed in several stages, such as rough polishing, precision polishing, and ultra-precision polishing. The polishing can be performed by using a polishing cloth and a polishing agent. The polishing agent is not particularly limited, but for example, an aqueous dispersion of cerium oxide having an average primary particle size of 10 to 100 nm, an aqueous dispersion of silicon dioxide nanoparticles having an average primary particle size of 10 to 100 nm (colloidal silica aqueous dispersion), etc. can be used.
[0088] Each of the surface shapes obtained only by local processing is not flat, and is generally a shape that cancels out the surface shape change in the fine polishing performed thereafter (generally an intermediate convex shape (a shape with the center portion of each main surface protruding), an intermediate concave shape (a shape with the center portion of each main surface concave), etc.). Even if the flatness of each surface shape obtained only by local processing is evaluated, the evaluation only deviates from the evaluation result of the shape of the main surface of the mask blank substrate finally obtained. After local processing, the change in the main surface shape caused by the fine polishing performed under predetermined polishing conditions has reproducibility. By understanding the change in the main surface shape after fine polishing under predetermined polishing conditions, applying the change to the shape of the main surface after local processing to predict the surface shape after fine polishing under predetermined polishing conditions, the surface shape obtained after fine polishing can be evaluated at the local processing stage before fine polishing to evaluate the quality of the shape of the main surface obtained by fine polishing. Note that the local processing step can be repeated until the predetermined shape is obtained.
[0089] In the manufacture of the mask blank substrate of the present invention, the local processing step preferably includes:
[0090] (A) a step of locally processing at least one of the first main surface and the second main surface;
[0091] (B) a step of measuring the shape of the locally processed main surface after the step (A) as the shape of the main surface before the finish polishing step;
[0092] (C) a step of predicting the shape of the locally processed main surface after the finish polishing step by applying the change in the surface shape in the finish polishing step grasped in advance to the shape of the main surface before the finish polishing step obtained in step (B); and
[0093] (D) A step of evaluating whether the shape after the fine polishing step predicted in step (C) is a shape that produces a predetermined TTV.
[0094] In step (A), the main surface is partially processed, but in the partial processing, the predetermined processing conditions in the partial processing are set in consideration of the shape of the main surface before the partial processing and the change in the shape of the main surface in the fine polishing step so that the main surface has a predetermined shape. Specifically, for example, in the case where the main surface is to be convex by fine polishing, the main surface preferably has a shape that offsets the change in consideration of the change (for example, a low convex or concave shape), and in the case where the main surface is to be concave by fine polishing, the main surface preferably has a shape that offsets the change in consideration of the change (for example, a shallow concave or convex shape). Before the partial processing, the shape of the main surface is appropriately measured, but there is no particular limitation on the measurement, and for example, a laser interferometer can be used.
[0095] In the local processing, processing for selectively removing relatively protruding portions is performed on the main surface of the mask blank substrate. The local processing can be performed by polishing with a polishing cloth and a polishing agent. There is no particular limitation on the polishing agent, but for example, an aqueous dispersion of cerium oxide having an average primary particle size of 10 to 100 nm, an aqueous dispersion of silicon dioxide nanoparticles having an average primary particle size of 10 to 100 nm (colloidal silicon dioxide aqueous dispersion), etc. can be used. In addition, in the local processing, a method such as magnetorheological finishing (MRF) can also be applied.
[0096] In step (B), the shape of the main surface after step (A), that is, actually after partial processing, is measured as the shape of the main surface before the fine polishing step, but there is no particular limitation on the measurement, for example, a laser interferometer may be used.
[0097] In step (C), the change in surface shape in the finish polishing step grasped in advance is applied to the shape of the main surface before the finish polishing step obtained in step (B) to predict the shape of the locally processed main surface after the finish polishing step.
[0098] Specifically, the change in the surface shape of the main surface before and after the fine polishing step (the change in the surface shape after the fine polishing step relative to the surface shape after the local processing step) is grasped, but the change can be grasped, for example, from the shape of the main surface obtained by selecting another mask blank substrate having a main surface of a similar shape from the mask blank substrate that has been partially processed and performing a predetermined fine polishing on the other mask blank substrate. In addition, the change in the surface shape can also be grasped by simulation. In this case, as another mask blank substrate, a main surface having a central concave shape as a target shape in the local processing step is suitable, and a main surface having a flatness of less than 300nm is suitable. The change in the surface shape in the fine polishing step grasped in advance is selected according to the shape of the main surface after the local processing obtained in step (B).
[0099] Here, for example, when the shape of the pseudo-TTV diagram of the main surface after the local processing step of the main surface is set to S1 and when the change in the shape of the pseudo-TTV diagram of the main surface when the predetermined finish polishing is performed is set to ΔS, according to the following expression
[0100] S1+ΔS=S2,
[0101] The shape of the locally processed main surface after the finish polishing step can be predicted as the shape of the pseudo-TTV map (predicted pseudo-TTV map) of the main surface after the finish polishing step (S2).
[0102] In step (D), it is evaluated whether the shape after the fine polishing step predicted in step (C) is a shape that imparts a predetermined flatness, specifically, a shape that produces a predetermined TTV. As an evaluation method, a method of measuring the shape of the main surface and evaluating a predetermined value calculated from the measured shape or a predetermined value obtained by mathematically processing the measured shape can be used.
[0103] In step (D), for example, in a pseudo-TTV map obtained by adding a height map of the first main surface and a height map of the second main surface based on the position of each of the first main surface and the second main surface of the mask blank substrate on the respective least squares planes, it can be evaluated whether the difference (TTV1) between the highest height and the lowest height of the TTV1 map excluding the primary component (pseudo-TTV1 map) is 35 nm or less, and whether the difference (TTV2) between the highest height and the lowest height of the TTV2 map excluding the primary component and the secondary component (pseudo-TTV2 map) is 25 nm or less in a cross-shaped area formed when a first rectangular area of 132 mm×104 mm coincides with a second rectangular area of 104 mm×132 mm, the first rectangular area being parallel to four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate, and the second rectangular area being orthogonal to the first rectangular area and parallel to four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate.
[0104] Specifically, in step (D):
[0105] In the cross-shaped region, it can be evaluated whether the difference (TTV1') between the highest height and the lowest height of the TTV1' graph excluding the primary component (predicted pseudo-TTV1' graph) is 35 nm or less, and whether the difference (TTV2') between the highest height and the lowest height of the TTV2' graph excluding the primary component and the secondary component (predicted pseudo-TTV2' graph) is 25 nm or less. The cross-shaped region is formed under the following conditions:
[0106] (1) The first main surface and the second main surface of the substrate are arranged in a substantially vertical direction, and a calculation area of a square tubular shape is set, the calculation area extending in the horizontal direction through four sides of a square of 132 mm×132 mm along four sides of the first main surface and the second main surface at the central part of the first main surface and the second main surface;
[0107] (2) in a state facing the first main surface, cutting out a portion of the first main surface within the calculation area as a first area surface;
[0108] (3) setting a vertical plane that passes through a reference point that is an arbitrary point on the central axis of the square prism in the calculation area and is orthogonal to the central axis as a reference plane, setting a rotation axis that passes through the reference point and is parallel to any one of four sides of a square that is an intersection line between the square prism in the calculation area and the vertical plane, and cutting out a portion of the second main surface in the calculation area in a state facing the second main surface as a second area surface by rotating the substrate 180 degrees along the rotation axis from a state facing the first main surface;
[0109] (4) calculating a least squares plane in each of the first area surface and the second area surface;
[0110] (5) converting the first area surface and the second area surface into a height map of the first area surface and a height map of the second area surface based on a position of each of the first area surface and the second area surface on a respective least squares plane;
[0111] (6) setting the height map of the second regional surface as an inverted height map of the second regional surface by symmetrically moving the height map relative to a vertical plane passing through the rotation axis in (3) and along the 90 degree direction of the rotation described in (3);
[0112] (7) creating a predicted pseudo-TTV map by adding the height of the height map of the first regional surface and the height of the inverted height map of the second regional surface at their respective positions (X coordinate, Y coordinate) on the reference plane; and
[0113] (8) In the predicted pseudo-TTV diagram, a first rectangular area of 132 mm × 104 mm overlaps with a second rectangular area of 104 mm × 132 mm, the first rectangular area is parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate, and the second rectangular area is orthogonal to the first rectangular area and is parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate.
[0114] In step (D), in the case where the shape of the main surface predicted in step (C) is a shape having a predetermined flatness, a fine polishing step may be performed. On the other hand, in step (D), in the case where the shape does not have the predetermined flatness, a local processing step, specifically including the local processing steps of steps (A) to (D), may be performed again, and the local processing step, specifically including the local processing steps of steps (A) to (D), may be repeated until the shape of the main surface predicted in step (C) is evaluated to have the predetermined flatness in step (D).
[0115] The defect level of the surface obtained only by local processing may be insufficient particularly in mask blank substrates for state-of-the-art products, and, in the manufacture of the mask blank substrate, the fine polishing step is generally performed after the local processing step. In addition, in the method for manufacturing the mask blank substrate of the present invention, the fine polishing step is performed after the local processing step. There is no particular limitation on the measurement of the shape of the main surface of the mask blank substrate obtained after the fine polishing step, but, for example, a laser interferometer can be used. Regarding the shape of the main surface of the mask blank substrate obtained after the fine polishing, a pseudo-TTV diagram can be created as needed to evaluate the difference between the highest height and the lowest height of the TTV1 diagram (TTV1) and the difference between the highest height and the lowest height of the TTV2 diagram (TTV2).
[0116] For example, if local processing is generally repeated about twice, it is relatively easy to obtain a mask blank substrate having a TTV1 of about 100 nm, but in conventional methods, it is difficult to set TTV1 to 35 nm or less and TTV2 to 25 nm or less in the above-mentioned cross-shaped region.
[0117] According to the present invention, a mask blank substrate having high flatness can be provided during exposure of an exposure mask obtained by film formation and pattern formation on a mask blank substrate, and such a mask blank substrate can be manufactured with high productivity by evaluating TTV using a pseudo-TTV map. In addition, by evaluating TTV using a pseudo-TTV map, the flatness of the mask blank substrate after fine polishing can be estimated as a predicted pseudo-TTV map, and therefore, the pseudo-TTV map of the mask blank substrate after fine polishing can be evaluated by the predicted pseudo-TTV map to provide a mask blank substrate having good flatness.
[0118] According to the present invention, whether the flatness of an exposure mask obtained by film formation and pattern formation on a mask blank substrate during exposure is good can also be evaluated through a pseudo TTV plot of the mask blank substrate after finish polishing.
[0119] Example
[0120] The present invention is specifically described below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0121] Example 1
[0122] Six glass substrates (the size of the first main surface and the second main surface is 152 mm×152 mm square and the thickness is 6.35 mm) made of SiO2 and TiO2 (TiO2 concentration is about 7 wt%) were prepared. The end faces (four faces except the main surface) of each glass substrate were chamfered and ground, and the two main surfaces were also rough-polished and precision-polished using a polishing solution containing cerium oxide abrasives. Thereafter, the six glass substrates (substrates 1-1 to 1-6) were set on a bracket of a double-sided polishing device, a suede-type soft polishing cloth was applied to the double-sided polishing device, and the first main surface and the second main surface were ultra-precision polished by a polishing solution using colloidal silica abrasives. After ultra-precision polishing, the silica nanoparticles were removed by washing the main surface with a washing solution containing KOH, and after drying, the shapes of the first main surface and the second main surface were measured using a surface shape measuring device (UltraFlat, manufactured by Tropel Corporation).
[0123] Next, the local processing step is carried out. First, the processing conditions for local processing are determined based on the shape of the main surface obtained, and based on the determined processing conditions, the first main surface and the second main surface of the glass substrate are locally processed by a local processing device (step (A)). The local processing device described in JP-A 2010-194705 (patent document 2) is used as a local processing device. The local processing using this device polishes all surfaces of the substrate while controlling the moving speed of the fine polishing tool, and the target shape can be obtained by slowly moving the polishing tool on the relatively convex part and quickly moving the polishing tool on the relatively concave part. Wool polishing felt is used as the processing tool of the local processing device, and silicon dioxide nanoparticles (AJ-3540, manufactured by Nissan Chemical Corporation) mixed with a small amount of defoamer (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.) are used as polishing slurry.
[0124] The glass substrate after the partial processing was washed with a washing solution containing KOH to remove silica nanoparticles, dried, and then the shapes of the first main surface and the second main surface were measured with a surface shape measuring device (UltraFlat, manufactured by Tropel Corporation) (step (B)).
[0125] Here, in order to grasp the change in the shape of the main surface after the fine polishing relative to the surface after the local processing, another glass substrate is used, similarly, the local processing is performed, and the fine polishing similar to the fine polishing to be described below is also performed to grasp the change in the shape of the surface before and after the fine polishing step in advance. Thereafter, for the 6 glass substrates after the local processing (substrate 1-1 to substrate 1-6), the shape of the surface after the fine processing is predicted by applying the grasped change in the shape of the main surface to the shape of the main surface of the glass substrate after the local processing (step (C)).
[0126] Next, it is evaluated whether the predicted shape after the fine polishing step is a shape that produces a predetermined TTV (step (D)). The shape of the surface of the glass substrate after local processing and the predicted shape of the surface after fine polishing are evaluated in a cross-shaped area formed when a first rectangular area of 132 mm×104 mm overlaps with a second rectangular area of 104 mm×132 mm, the first rectangular area being parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonals of the main surface of the substrate, and the second rectangular area being orthogonal to the first rectangular area and parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonals of the main surface of the substrate.
[0127] Here, it is assessed whether a shape produces a predetermined TTV based on the following facts:
[0128] In the cross-shaped region, in the predicted pseudo-TTV map, whether the difference between the highest height and the lowest height of the TTV1' map excluding the primary component (TTV1') is less than 35nm, and whether the difference between the highest height and the lowest height of the TTV2' map excluding the primary component and the secondary component (TTV2') is less than 25nm, the cross-shaped region is formed in the following cases:
[0129] (1) The first main surface and the second main surface of the substrate are arranged in a substantially vertical direction, and a calculation area of a square tubular shape is set, the calculation area extending in the horizontal direction through four sides of a square of 132 mm×132 mm along four sides of the first main surface and the second main surface at the central part of the first main surface and the second main surface;
[0130] (2) in a state facing the first main surface, cutting out a portion of the first main surface within the calculation area as a first area surface;
[0131] (3) setting a vertical plane that passes through a reference point that is an arbitrary point on the central axis of the square prism in the calculation area and is orthogonal to the central axis as a reference plane, setting a rotation axis that passes through the reference point and is parallel to any one of four sides of a square that is an intersection line between the square prism in the calculation area and the vertical plane, and cutting out a portion of the second main surface in the calculation area in a state facing the second main surface as a second area surface by rotating the substrate 180 degrees along the rotation axis from a state facing the first main surface;
[0132] (4) calculating a least squares plane in each of the first area surface and the second area surface;
[0133] (5) converting the first area surface and the second area surface into a height map of the first area surface and a height map of the second area surface based on a position of each of the first area surface and the second area surface on a respective least squares plane;
[0134] (6) setting the height map of the second regional surface as an inverted height map of the second regional surface by symmetrically moving the height map relative to a vertical plane passing through the rotation axis in (3) and along the 90 degree direction of the rotation described in (3);
[0135] (7) creating a predicted pseudo-TTV map by adding the height of the height map of the first regional surface and the height of the inverted height map of the second regional surface at their respective positions (X coordinate, Y coordinate) on the reference plane; and
[0136] (8) In the predicted pseudo-TTV diagram, a first rectangular area of 132 mm × 104 mm overlaps with a second rectangular area of 104 mm × 132 mm, the first rectangular area is parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate, and the second rectangular area is orthogonal to the first rectangular area and is parallel to the four sides of the main surface of the substrate and is centered on the intersection of the diagonals of the main surface of the substrate.
[0137] For the surface shape after the first local processing step, a predicted shape of the main surface of each glass substrate after fine polishing (predicted pseudo-TTV diagram) was created, and the results of evaluating TTV1' in the predicted pseudo-TTV1' diagram and TTV2' in the predicted pseudo-TTV2' diagram are shown in Table 1.
[0138] In any of the substrates, TTV1' and TTV2' were not equal to or less than the predetermined value in the first processing. Therefore, local processing was performed by repeating steps (A) to (D) until TTV1' and TTV2' were equal to or less than the predetermined value. The values of TTV1' and TTV2' that were equal to or less than the predetermined value, and the number of steps (A) to (D) performed until TTV1' and TTV2' were equal to or less than the predetermined value are shown in Table 1. As a result, in any of the glass substrates, TTV1' was 35 nm or less, and TTV2' was 25 nm or less, so it was evaluated that the shape of the main surface having a predetermined flatness was obtained, and the fine polishing step was performed.
[0139] The glass substrate was set on a holder of a polishing device to which a suede-type soft polishing cloth was applied, polished by using a polishing solution of colloidal silica, washed with a washing solution containing KOH after polishing to remove the colloidal silica, and dried to obtain a mask blank substrate. The shapes of the first and second main surfaces of the obtained mask blank substrate were measured with a surface shape measuring device (UltraFlat, manufactured by Tropel Corporation) to create a pseudo-TTV map, and TTV1, TTV2, and flatness of the first main surface were evaluated. The results are shown in Table 1.
[0140] Table 1
[0141]
[0142] Comparative Example 1
[0143] 15 glass substrates (the size of the first main surface and the second main surface is 152 mm×152 mm square and the thickness is 6.35 mm) made of SiO2 and TiO2 (TiO2 concentration is about 7 wt%) were prepared. The end faces (four faces other than the main surface) of each glass substrate were chamfered and ground, and the two main surfaces were also rough-polished and precision-polished using a polishing solution containing cerium oxide abrasives. Thereafter, the 15 glass substrates (substrates C1-1 to C1-15) were set on a bracket of a double-sided polishing device, a suede-type soft polishing cloth was applied to the double-sided polishing device, and the first main surface and the second main surface were ultra-precision polished by a polishing solution using colloidal silica abrasives. After ultra-precision polishing, the silica nanoparticles were removed by washing the main surface with a washing solution containing KOH, and after drying, the shapes of the first main surface and the second main surface were measured using a surface shape measuring device (UltraFlat, manufactured by Tropel Corporation).
[0144] Next, the local processing step is carried out. First, the processing conditions for local processing are determined based on the shape of the main surface obtained, and, based on the determined processing conditions, the first main surface and the second main surface of the glass substrate are locally processed by a local processing device. The local processing device described in JP-A 2010-194705 (patent document 2) is used as a local processing device. The local processing using this device polishes all surfaces of the substrate while controlling the moving speed of the fine polishing tool, and the target shape can be obtained by slowly moving the polishing tool on the relatively convex part and quickly moving the polishing tool on the relatively concave part. Wool polishing felt is used as the processing tool of the local processing device, and silicon dioxide nanoparticles (AJ-3540, manufactured by Nissan Chemical Corporation) mixed with a small amount of defoamer (Shin-Etsu Silicone KS-537, manufactured by Shin-Etsu Chemical Co., Ltd.) are used as polishing slurry.
[0145] The glass substrate after the partial processing was washed with a washing solution containing KOH to remove silica nanoparticles, dried, and then the shapes of the first major surface and the second major surface were measured with a surface shape measuring device (UltraFlat, manufactured by Tropel Corporation).
[0146] Here, in order to grasp the change in the shape of the main surface after the fine polishing relative to the surface after the local processing, another glass substrate is used, similarly, the local processing is performed, and the fine polishing similar to the fine polishing to be described below is performed to grasp the change in the shape of the surface before and after the fine polishing step in advance. Thereafter, for 15 glass substrates after the local processing (substrates C1-1 to C1-15), the shape of the surface after the fine processing is predicted by applying the grasped change in the shape of the main surface to the shape of the main surface of the glass substrate after the local processing.
[0147] Next, it is evaluated whether the shape predicted after the fine polishing step is a shape that produces a predetermined TTV. The shape of the surface of the glass substrate after local processing and the shape of the surface predicted after fine polishing are evaluated in a cross-shaped area formed when a first rectangular area of 132 mm×104 mm coincides with a second rectangular area of 104 mm×132 mm, the first rectangular area being parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonal lines of the main surface of the substrate, and the second rectangular area being orthogonal to the first rectangular area and parallel to the four sides of the main surface of the substrate and centered at the intersection of the diagonal lines of the main surface of the substrate. Whether the shape produces a predetermined TTV is evaluated in a manner similar to that in Example 1.
[0148] For the surface shape after the first local processing step, a predicted shape of the main surface of each glass substrate after fine polishing (predicted pseudo-TTV diagram) was created, and the results of evaluating TTV1' in the predicted pseudo-TTV1' diagram and TTV2' in the predicted pseudo-TTV2' diagram are shown in Table 2.
[0149] In any of the substrates, TTV1' and TTV2' are not equal to or less than the predetermined value in the first process, but the finish polishing step is performed without change.
[0150] The glass substrate was set on a holder of a polishing device to which a suede-type soft polishing cloth was applied, polished by using a polishing solution of colloidal silica, washed with a washing solution containing KOH after polishing to remove the colloidal silica, and dried to obtain a mask blank substrate. The shapes of the first and second main surfaces of the obtained mask blank substrate were measured with a surface shape measuring device (UltraFlat, manufactured by Tropel Corporation) to create a pseudo TTV map, and TTV1 and TTV2 were evaluated. The results are shown in Table 2.
[0151] Table 2
[0152]
[0153] The mask blank substrate obtained in the embodiment has TTV1 below 35nm and TTV2 below 25nm, and an exposure mask having excellent flatness when adsorbed to an exposure machine can be obtained from such a mask blank substrate, and it can be expected that good exposure results can be obtained as an exposure mask for a next-generation high-NA exposure machine.
Claims
1. A mask blank substrate having two main surfaces, a first main surface and a second main surface, of a 152 mm×152 mm square and a thickness of 6.35 mm, wherein In a pseudo-TTV map obtained by adding a height map of the first main surface and a height map of the second main surface based on the position of each of the first main surface and the second main surface on the respective least squares planes, In the fitting of the pseudo-TTV graph, when a plane function approximated by a first-order polynomial is derived, the difference between the highest height and the lowest height of the TTV1 graph excluding the first-order component (TTV1) is 35 nm or less, and, in the fitting of the pseudo-TTV graph, when a surface function approximated by a highest quadratic polynomial is derived, the difference between the highest height and the lowest height of the TTV2 graph excluding the first-order component and the second-order component (TTV2) is 25 nm or less, In the cross-shaped area formed when a first rectangular area of 132mm×104mm overlaps with a second rectangular area of 104mm×132mm, the first rectangular area is parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate, and the second rectangular area is orthogonal to the first rectangular area and parallel to the four sides of the main surface of the substrate and centered on the intersection of the diagonals of the main surface of the substrate.
2. The mask blank substrate according to claim 1, wherein: The flatness of the first main surface within the cross-shaped region is 35 nm or less.
3. A method for manufacturing a mask blank substrate, the mask blank substrate having two main surfaces, a first main surface and a second main surface, of a square shape of 152 mm×152 mm and a thickness of 6.35 mm, the manufacturing method comprising: a local processing step of at least one of the first main surface and the second main surface and a fine polishing step after the local processing step, wherein The local processing steps include: (A) a step of locally processing at least one of the first main surface and the second main surface; (B) a step of measuring the shape of the locally processed main surface after the step (A) as the shape of the main surface before the finish polishing step; (C) a step of predicting the shape of the locally processed main surface after the finish polishing step by applying the change in the surface shape in the finish polishing step grasped in advance to the shape of the main surface before the finish polishing step obtained in step (B); and (D) A step of evaluating whether the shape after the fine polishing step predicted in step (C) is a shape that produces a predetermined TTV.
4. The manufacturing method according to claim 3, wherein: The shape of the predetermined TTV generated in step (D) is a shape in the predicted pseudo-TTV map within the cross-shaped region formed in the following cases: (1) The first main surface and the second main surface of the substrate are arranged in a substantially vertical direction, and a calculation area of a square tubular shape is set, the calculation area extending in a horizontal direction through four sides of a square of 132 mm×132 mm along four sides of the first main surface and the second main surface at the center portion of the first main surface and the second main surface; (2) in a state facing the first main surface, cutting out a portion of the first main surface within the calculation area as a first area surface; (3) setting a vertical plane that passes through a reference point that is an arbitrary point on the central axis of the square prism in the calculation area and is orthogonal to the central axis as a reference plane, setting a rotation axis that passes through the reference point and is parallel to any one of four sides of a square that is an intersection line between the square prism in the calculation area and the vertical plane, and cutting out a portion of the second main surface in the calculation area in a state facing the second main surface as a second area surface by rotating the substrate 180 degrees along the rotation axis from a state facing the first main surface; (4) calculating a least squares plane in each of the first area surface and the second area surface; (5) converting the first area surface and the second area surface into a height map of the first area surface and a height map of the second area surface based on a position of each of the first area surface and the second area surface on a respective least squares plane; (6) setting the height map of the second region surface as an inverted height map of the second region surface by moving the height map symmetrically relative to a vertical plane passing through the rotation axis and along the 90 degree direction of the rotation; (7) creating a predicted pseudo-TTV map by adding the height of the height map of the first regional surface and the height of the inverted height map of the second regional surface at their respective positions (X coordinate, Y coordinate) on the reference plane; and (8) In the predicted pseudo-TTV diagram, a first rectangular area of 132 mm×104 mm overlaps with a second rectangular area of 104 mm×132 mm. The first rectangular area is parallel to the four sides of the main surface of the substrate and is centered at the intersection of the diagonals of the main surface of the substrate. The second rectangular area is orthogonal to the first rectangular area and is parallel to the four sides of the main surface of the substrate and is centered at the intersection of the diagonals of the main surface of the substrate. In the fitting of the predicted pseudo-TTV diagram, when a plane function approximated by a first-order polynomial is derived, the difference between the highest and lowest heights of the TTV1' diagram excluding the primary component (TTV1') is less than 35nm, and, in the fitting of the predicted pseudo-TTV diagram, when a surface function approximated by a second-order polynomial is derived, the difference between the highest and lowest heights of the TTV2' diagram excluding the primary and secondary components (TTV2') is less than 25nm.