Production process of 750kV extra-high voltage cross-linked polyethylene smooth aluminum sheath cable

By adopting circular conductor compression and Z-type wire twisting technology in the production of 750kV ultra-high voltage cables, combining electromagnetic induction preheating and multi-stage cooling crosslinking, thermal convection degassing and smooth aluminum sleeves, the conductor core wire circle is solved The thermal stress problems of cross-linking of flatness and insulating layers reduce cable weight and ablation risks, and improve cable stability and production efficiency.

CN119028664AActive Publication Date: 2024-11-26NINGBO ORIENT WIRES & CABLES CO LTD

Patent Information

Application Number
CN202411181133.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

In the production of 750kV ultra-high voltage cables, the circularity of the conductor core wire is difficult to control, the thermal stress of the cross-linking of the insulating layer is high, the weight of the cable is increased, and the ablation problem of the semiconductor buffer layer is serious, resulting in cable failure or shutdown.

Method used

The inner core of the circular conductor is adopted, and the Z-type wire twist is synthesized into the outer core of the ring conductor. Through electromagnetic induction preheating and multi-stage cooling cross-linking technology, the internal stress of cross-linking is reduced, and the thermal convection type dryer is used to accelerate the degassing. , a smooth aluminum sleeve is formed to avoid ablation risks, and the stability and performance of the cable are improved by multiple roller sets and hot melt adhesive spraying.

Benefits of technology

The circularity control of the conductor core wire is realized, the thermal stress of the cross-linking of the insulating layer is reduced, the weight of the cable is reduced, the ablation of the semiconducting buffer layer is avoided, and the safety and production efficiency of the cable are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028664A_ABST
    Figure CN119028664A_ABST
Patent Text Reader

Abstract

The invention discloses a production process of a 750kV extra-high voltage cross-linked polyethylene smooth aluminum sleeve cable, which comprises the following steps: compressing a circular conductor to form a conductor inner core, twisting a Z-shaped molded line conductor to form a conductor outer core, enabling a formed conductor core wire to pass through a front preheater to form an insulated core wire, enabling the conductor core wire to pass through a rear preheater, and carrying out multi-section cooling cross-linking and degassing, thereby obtaining the 750kV extra-high voltage cross-linked polyethylene smooth aluminum sleeve cable. Longitudinally wrapping an aluminum strip to form a smooth aluminum sleeve, reducing the diameter of the smooth aluminum sleeve, spraying a hot melt adhesive, extruding an outer sheath, cooling and taking up. According to the production process of the 750kV extra-high voltage cross-linked polyethylene smooth aluminum sleeve cable, the roundness of the conductor core wire is guaranteed, the cross-linking thermal stress of the insulating layer is reduced, and the buffer layer is prevented from being ablated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of cables, in particular to a production process for a 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable. Background Art

[0002] With the continuous growth of global energy demand and the large-scale development and utilization of renewable energy, the market demand for UHV cables, as a key technology for long-distance, large-capacity power transmission, is expected to continue to expand. In particular, UHV cables play an irreplaceable role in connecting remote renewable energy bases (such as wind and solar power stations) with load centers.

[0003] In the process of manufacturing 750kV power cables, there are currently some technical difficulties, such as the difficulty in controlling the roundness of large-section conductors, the thick insulation layer resulting in large cross-linking thermal stress, the heavy cable weight, and the easy flattening of the sheath during production. At the same time, in recent years, high-voltage cable failures or shutdowns due to the ablation of the semi-conductive buffer layer of the cable have occurred frequently at home and abroad. The small contact area between the corrugated aluminum sheath of the cable and the semi-conductive buffer layer, and uneven contact are important factors leading to the ablation of the buffer layer. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a production process for a 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable which ensures the roundness of the conductor core wire, reduces the cross-linking thermal stress of the insulation layer, and avoids the ablation of the buffer layer.

[0005] The technical solution adopted by the present invention to solve the above problem is a production process of a 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable, comprising the following steps:

[0006] S1: Use round conductor to compress and form the conductor core;

[0007] S2: Use Z-shaped wire conductors to twist into a ring-shaped conductor outer core and wrap the conductor inner core;

[0008] S3: passing the conductor core wire composed of the conductor inner core and the conductor outer core through the preheater to perform electromagnetic induction preheating on the conductor core wire;

[0009] S4: Co-extrude the inner shielding layer, the insulating layer and the outer shielding layer on the surface of the conductor core wire to form an insulated core wire;

[0010] S5: passing through the post-preheater, the conductor core wire inside the insulated core wire is subjected to electromagnetic induction heating to reduce the cross-linking internal stress;

[0011] S6: The insulated core wire passes through the cross-linking tube, which is heated and cross-linked at the inlet end, and then cross-linked by multi-stage cooling;

[0012] S7: The insulated core wire is placed in a hot convection drying room for degassing;

[0013] S8: wrap a layer of semi-conductive butyl tape, two layers of semi-conductive water-resistant tape and a layer of semi-conductive water-resistant copper wire shielding tape around the outer layer of the insulated core wire in sequence to form a tape-wrapped core wire;

[0014] S9: longitudinally wrap aluminum tape on the surface of the tape-wrapped core wire;

[0015] S10: Perform argon arc welding on the longitudinal connection of the aluminum strip to form a smooth aluminum sleeve;

[0016] S11: Online eddy current testing of the weld of the smooth aluminum sleeve;

[0017] S12: reducing the diameter of the smooth aluminum sheath so that the smooth aluminum sheath and the insulated core wire are pressed together to form an aluminum sheath core wire;

[0018] S13: spraying hot melt adhesive on the surface of the smooth aluminum sleeve;

[0019] S14: extruded outer sheath;

[0020] S15: Cooling;

[0021] S16: Reel in the line.

[0022] Compared with the prior art, the advantages of the present invention are as follows: the conventional conductor core wire is a circular compact structure, which is formed by twisting a number of circular conductor monofilaments of the same diameter, and there are gaps between the conductor monofilaments of the outermost layer. During the cross-linking process, the inner shielding layer material is easily randomly embedded under the high pressure of extrusion, resulting in uneven thickness and waste of inner shielding layer material. At the same time, compared with the profile wire, the compaction coefficient is low and the amount of copper used is increased. Through the steps of S1 and S2, a mixed conductor production process is adopted, the center adopts a circular compaction to form a conductor inner core, and the outer layer uses a Z-shaped profile wire to twist into a ring-shaped conductor outer core, wherein the Z-shaped profile wire twisting does not require mold cold drawing, and the heat generated during twisting is small, which greatly reduces the increase in the resistivity of the conductor due to lattice distortion, thereby meeting the electrical requirements. Under the premise of meeting the resistance requirements, the copper section can be reduced. The copper consumption of the conductor outer core structure can save 1% to 2.5% compared with the conventional circular compact structure. At the same time, the outer Z-shaped wires are closely connected, the contact area between each other is large, the contact resistance is reduced, and the gap between each other is small. In the three-layer co-extrusion process, the extrusion pressure can make the Z-shaped wires more closely connected when under pressure like the wedge-shaped wires, and it is not easy to loosen, thereby solving the problem of embedded inner shielding layer materials. Compared with the traditional circular compact structure, the inner shielding layer material can be saved by 1%-5%, and the outer diameter of the conductor core wire is stable, the surface is smooth and round, the bending radius is also smaller than that of the full-shaped wire conductor, and the structure is stable and reliable. This structure takes into account the advantages of circular single-wire compaction and wire twisting;

[0023] In steps S3-S6, through step S3, the conductor core wire can be heated to increase the temperature of the conductor core wire, which is helpful to improve the cross-linking efficiency, and can also increase the adhesion between the conductor and the inner shielding layer, and can also play a role in drying and dehumidification. Through the design of step S5, the conductor core wire can continue to be heated after the three-layer co-extrusion, and the heat can be transferred from the conductor core wire to the three-layer co-extrusion, reducing the temperature difference between the inner and outer circles of the three-layer co-extrusion, and improving the uniformity and sufficiency of the cross-linking. Then in step S6, the cross-linking heat of the three-layer co-extrusion can be transferred from the inner layer and the outer layer in two directions, thereby improving the cross-linking efficiency. The temperature of the conductor core wire and the cross-linking tube is calculated and set by the software. The absorbed heat is enough to make the cross-linking reaction fully proceed, shortening the cross-linking time. The multi-stage cooling cross-linking design along the cross-linking tube can reduce the surface temperature of the insulating core wire, so that the insulating core wire can enter the cooling section at a lower temperature, shortening the cooling time. Since the surface temperature difference between the conductor core wire and the insulating core wire is reduced, the thermal stress and uneven crystallization phenomenon in the three-layer co-extrusion are also improved. In the process of three-layer co-extrusion cross-linking, the heat is transferred from the outer layer to the inner layer, which not only ensures that the inner circle of the insulating layer is in good cross-linking condition, but also prevents the outer circle of the insulating layer from over-cross-linking.

[0024] In step S7, according to the XLPE insulation manufacturing principle, after XLPE is chemically cross-linked, small molecular byproducts such as methane, water, cumyl alcohol, and acetophenone will be produced, which will remain in the insulation layer and affect the product performance of the high-voltage cable. In addition, the insulation layer of the 750kV ultra-high voltage cable is thick, so it is necessary to adopt a reasonable degassing method to eliminate internal gas byproducts, reduce and redistribute solid byproducts, reach a degassing equilibrium point, and thus ensure that the cable performance is not affected; the traditional heat conduction system uses electric heating equipment around the turntable for heat conduction, and hot air is naturally transmitted from the outside to the inside, and the heat transfer efficiency is low, resulting in the cable in the inner circle of the drying room being difficult to heat and slow to heat up, and the degassing time is too long, affecting the production efficiency and product delivery cycle; in response to the above problems, on the basis of the traditional degassing equipment, the heat transfer function of thermal convection is added, thereby increasing the heat transfer efficiency, reducing the degassing time, and improving the production efficiency;

[0025] Through the design of step S8, after the subsequent smooth aluminum sleeve is formed, the smooth aluminum sleeve is fully pressed and compacted with a layer of semi-conductive butyl tape, two layers of semi-conductive water-blocking tape and a layer of semi-conductive water-blocking copper wire shielding tape to form a negative gap to ensure good conductivity and reliable electrical connection, thereby avoiding the risk of suspended discharge and ablation caused by poor contact caused by the gap between the wrinkled aluminum sleeve and the water-blocking tape;

[0026] The S9-S12 design can form a high-quality smooth aluminum sheath to ensure the safe use of UHV cables and avoid the risk of ablation.

[0027] As an improvement of the present invention, in step S3, the preheating temperature of the front preheater is set at 80-100°C; in step S5, the preheating temperature of the rear preheater is set at 140-160°C; in step S6, the multi-stage cooling cross-linking process is seven stages, and the temperatures are 280°C, 270°C, 265°C, 260°C, 255°C, 250°C, and 240°C, respectively. Through the improvement, the front preheater and the rear preheater are used to reduce the temperature difference between the inner ring and the outer ring of the three-layer co-extrusion, improve the uniformity and sufficiency of the cross-linking, and through the VCV special calculation software TCC precise calculation, the cross-linked tube adopts seven heating sections, the temperature is reduced section by section, the front preheater and the rear preheater are enabled, and the internal and external heating methods are used to reduce the temperature of the cross-linked tube. The temperature gradient of the three-layer co-extrusion cross-linking is reduced to keep the heating uniform while maintaining a good degree of cross-linking. During the heating process, the temperature of the outer ring of the insulation layer rises rapidly to 230°C, so that the outer ring of the insulation layer is quickly cross-linked, and the melting sag of the polyethylene melt under gravity is reduced. As the insulation layer moves in the cross-linked tube, the middle layer area of ​​the insulation layer slowly rises from 135°C to 195°C, and the temperature of the inner ring of the insulation layer slowly rises to 163°C. At 60 meters, the degree of cross-linking of the insulation layer reaches more than 93%, and at 80 meters, the degree of cross-linking reaches more than 98%. In addition, the temperature is reduced step by step. After the insulation core wire leaves the heating section and enters the cooling section at 20 meters, the surface temperature drops to 45°C. The cooling is timely and sufficient, and the generation of cross-linking internal stress is reduced.

[0028] As an improvement of the present invention, after step S6 is completed, the insulating core wires are layered and raised when winding the wires to increase the gap between each layer of the insulating core wires. The raising is performed by hollow pads. Through the improvement, the gap between each layer of cables is increased, which is conducive to faster and more uniform transfer of heat to the surface of each layer of cables when hot air convection is formed, thereby accelerating the degassing efficiency.

[0029] As an improvement of the present invention, a heating tube for heating the convection drying room is provided on the inner wall of the convection drying room, a support frame for supporting the insulating core wire is provided on the axis of the convection drying room, the support frame is rotatably connected in the convection drying room, the insulating core wire is spirally stacked on the support frame, the support frame includes an air transfer tube arranged on the axis, the air transfer tube is connected to a supporting square tube in the circumferential direction, the supporting square tube is evenly arrayed with air outlet holes, the connection between the air transfer tube and the supporting square tube is provided with air transfer holes, an exhaust fan is provided below the air transfer tube, and an air outlet is provided above the air transfer tube. Valve, through the improvement, there are two main ways to form air convection phenomenon, one is to use increased air pressure to send air to achieve convection, the other is to use reduced air pressure to gather wind to achieve convection, and the convection drying room is large in size. If the convection is formed by increasing the air pressure, the requirements for the booster fan are high. It is necessary to ensure the compatibility between the booster fan and the convection drying room, and to ensure the sufficiency and integrity of the convection, which will cause a substantial increase in the degassing cost. By reducing the air pressure to gather wind, it is only necessary to ensure the centrality of the gathering position to ensure the uniformity of the convection. , and can ensure the comprehensiveness of convection. The convection drying room has lower requirements for its adaptability. Therefore, the method of forming convection by negative pressure wind gathering is more valuable in the convection drying room than the method of forming convection by increasing air supply. The setting of the rotating connection of the support frame can enhance the air flow in the convection drying room, which is conducive to the transmission of high temperature and improves the degassing efficiency. The design of the air transfer duct and the exhaust fan can form an axial air flow area on the axis of the convection drying room. In addition to the air flow moving along the axial direction, a negative pressure area will be formed in the air transfer duct, and the heating tube on the inner wall is heated to form a negative pressure area on the inner wall. A high-pressure area is formed, so that heat can be quickly transferred from the inner wall area to the axial area, thereby improving the degassing efficiency. The traditional structural design, in which the heating tube is heated in the inner wall area, has a heat transfer efficiency that is much lower than the transfer efficiency of the negative pressure area designed on the axis. The design of the air outlet and the air transfer hole is to ensure the high pressure of the inner wall and the low pressure of the axis. The air flow is fluid, and the heat is transferred quickly. The supporting square tube is a hollow pad. As the heat passes through the air outlet, the cable on the supporting square tube can be driven to heat up. Compared with the traditional heat transfer method, the temperature rises faster.

[0030] As an improvement of the present invention, an air inlet is provided on the outside of the convection drying room, and the direction of the air inlet of the air inlet is arranged along the tangent direction of the convection drying room, and the heating tube is extended and spirally ascended along the direction of the air inlet, and the spiral ascending rotation direction of the heating tube is the same as the rotation direction of the support frame, and the inner side of the top surface of the convection drying room is in an inverted cone shape. Through the improvement, through the design of the air inlet and the heating tube, a spiral upward airflow can be formed on the inner wall of the convection drying room, and when the airflow contacts the top surface of the convection drying room, it will converge to the center, and then because the heat of the spiral ascending airflow is higher than that of the air transfer pipe, the spiral ascending airflow will move spirally downward along the air transfer pipe to realize heat transfer on the axis, so as to accelerate the heating speed of the cable in the inner circle of the spiral, thereby accelerating the heating speed of the cable as a whole, so as to improve the degassing efficiency of the cable, wherein the spiral ascending rotation direction of the heating tube is the same as the rotation direction of the support frame, so that the rotation of the support frame can enhance the spiral ascending speed of the airflow on the heating tube.

[0031] As an improvement of the present invention, a ventilation duct is provided between the air outlet valve and the air inlet fan. Through the improvement, the air flow in the convection drying room forms a closed-loop reflux, thereby preventing the air pressure in the convection drying room from rising with the operation of the air inlet fan during the flow of the air flow. In actual operation, if the air inlet fan always draws external gas and transports it into the convection drying room, on the one hand, it will bring in colder air into the convection drying room, thereby affecting the heating efficiency of the convection drying room, and on the other hand, it will cause the air pressure in the convection drying room to rise rapidly. In order to ensure the safety of the use of the convection drying room, it is necessary to release the pressure in time, which can easily increase the operating cost of the convection drying room. At the same time, in the process of negative pressure gathering wind forming in the air transfer duct, the air inlet fan can strengthen the negative pressure of the air transfer duct, use an exhaust fan at one end to supply air, and use an air inlet fan at the other end to exhaust air, so as to achieve the smooth flow of negative pressure airflow in the air transfer duct.

[0032] As an improvement of the present invention, in step S9, during the longitudinal wrapping process of the aluminum strip, it passes through a forming wheel, four to six horn dies, and a sizing die in sequence and then converges into a circle. The sizing die adopts a nano-diamond coated sizing die. Through the improvement, the diameter reduction of the multi-channel horn die can better align the two sides of the aluminum strip during the longitudinal wrapping process, reduce the high and low misalignment, and enhance the welding reliability of the weld. The sizing die adopts a nano-diamond coated sizing die design, which can reduce traction resistance and ensure that the surface of the formed aluminum sleeve is bright, which helps to improve the quality of the weld.

[0033] As an improvement of the present invention, in step S11, when a leaky weld or a cold weld is detected, a cold welding machine is used for online repair welding. Through the improvement, the cold welding machine adopts the principle of capacitor energy storage to instantly release current between the tungsten electrode and the workpiece in the form of a high-frequency pulse arc. It only takes a dozen milliseconds to complete the welding of a weld. The heat input is concentrated, and the time for arcing and arcing is fast. There is no continuous heating of the workpiece, thereby achieving a cold welding effect, which can effectively ensure the quality of the repair welding. At the same time, after the repair welding is completed, it is necessary to ensure that the inner surface of the aluminum sleeve is not deformed.

[0034] As an improvement of the present invention, in step S12, multiple groups of roller groups are used for rolling to perform gradual diameter reduction, the roller group includes four rollers, the four rollers are arranged in the center along the circumferential direction to form a diameter reduction hole for diameter reduction, the diameters of the diameter reduction holes of the multiple groups of roller groups are reduced successively, during the diameter reduction process, the rollers rotate, and a rotating connecting buckle is provided at the connection of the two connected rollers, the rotating connecting buckle includes a matching parallel groove and a parallel block, the parallel block is provided on one roller, the parallel groove is provided on the other roller, the parallel block is provided along the radial direction of one roller, and the parallel groove is provided along the axial direction of the other roller, the rollers are made of MC nylon, Through the improvement, through the design of multiple roller groups, the cable can be reduced in diameter, and the cable diameter can be reduced, which can not only make the aluminum tape and the semi-conductive butyl tape, semi-conductive water-resistant tape, and semi-conductive water-resistant copper wire shielding tape fit more closely, but also reduce the overall diameter of the cable, thereby reducing the use of the outer sheath of the outer layer of the aluminum tape, reducing the weight of the cable, and reducing the cable production cost. The connection design of the rollers between each roller group can ensure the rotation stability of the rollers and avoid the phenomenon of connection and separation between the rollers. The rollers are made of MC nylon, because MC nylon has high strength, can bear loads for a long time, has strong wear resistance and self-lubrication, and can absorb noise and impact. Roller molding is free of lubricating oil, which is convenient for the subsequent hot melt adhesive process.

[0035] As an improvement of the present invention, in step S13, before spraying the hot melt adhesive, the smooth aluminum sleeve is preheated, the core wire of the aluminum sleeve is passed through an embracing heating device, and infrared heating is used to raise the surface temperature of the smooth aluminum sleeve to 60 degrees, and then a plurality of atomizing spray guns evenly distributed along the circumference are used for spraying. Through the improvement, preheating the smooth aluminum sleeve is not only beneficial to the adhesion between the smooth aluminum sleeve and the hot melt adhesive, but also helps to prolong the solidification time of the hot melt adhesive. In S14, the bonding strength between the outer sheath and the hot melt adhesive after extrusion is enhanced, so that the smooth aluminum sleeve, the hot melt adhesive and the outer sheath are tightly bonded. The design of multiple atomizing spray guns helps to control the spraying thickness and spraying uniformity of the hot melt adhesive, thereby improving the spraying quality of the spray adhesive. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a schematic diagram of the cross-sectional structure of the cable of the present invention.

[0037] Figure 2 It is a schematic diagram of the structure of the three-layer co-extrusion process of the conductor core wire of the present invention.

[0038] Figure 3 It is a schematic diagram of the cross-linking degree and temperature curve of the three-layer co-extrusion of the insulated core wire of the present invention.

[0039] Figure 4 It is a schematic diagram of the internal structure of the convection drying room of the present invention.

[0040] Figure 5 It is a schematic diagram of the connection structure between the supporting square tube and the air transmission tube of the present invention.

[0041] Figure 6 It is a schematic diagram of the top view structure of the support frame of the present invention.

[0042] Figure 7 It is a schematic diagram of airflow in a convection drying room of the present invention.

[0043] Figure 8 It is a schematic diagram of the structure of the smooth aluminum sleeve forming process of the present invention.

[0044] Fig. 9 It is a schematic diagram of the structure of the aluminum strip longitudinal wrapping process of the present invention.

[0045] Fig.10 It is a schematic diagram of the structure of the roller group of the present invention.

[0046] As shown in the figure: 1. Conductor core wire, 1.1. Conductor inner core, 1.2. Conductor outer core, 2. Pre-preheater, 3. Insulation core wire, 3.1. Inner shielding layer, 3.2. Insulation layer, 3.3. Outer shielding layer, 4. Three-layer co-extrusion extruder, 5. Post-preheater, 6. Cross-linking tube, 6.1. Heating section, 6.2. Cooling section, 7. Convection drying room, 7.1. Heating tube, 7.2. Support frame, 7.2.1. Air transfer tube, 7.2.2. Support square tube, 7.2.3. Air outlet, 7.2.4. Air outlet, 7.2.5. Exhaust fan, 7.2.6. Air outlet valve, 8. Air inlet fan, 8.1, ventilation duct, 9, semi-conductive buffer layer, 10, aluminum strip, 11, smooth aluminum sleeve, 12, aluminum sleeve core wire, 13, outer sheath, 14, forming wheel, 15, horn mold, 16, sizing mold, 17, roller set, 17.1, reducing hole, 17.2, rotating connecting buckle, 17.2.1, parallel groove, 17.2.2, parallel block, 18, atomizing spray gun, 19, insulated core wire pay-off rack, 20, aluminum strip pay-off rack, 21, argon arc welding gun, 22, online eddy current flaw detector, 23, aluminum sleeve preheating machine, 24, outer sheath extruder, 25, cooling water tank, 26, cable take-up rack. DETAILED DESCRIPTION

[0047] The embodiments of the present invention are further described below in conjunction with the accompanying drawings.

[0048] like Figure 1 As shown, a production process of a 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable comprises the following steps:

[0049] S1: A round conductor is pressed to form a conductor core 1.1;

[0050] S2: A Z-shaped conductor is twisted into a ring-shaped conductor outer core 1.2 and is fitted to wrap the conductor inner core 1.1;

[0051] S3: passing the conductor core wire 1 composed of the conductor inner core 1.1 and the conductor outer core 1.2 through the preheater 2 to perform electromagnetic induction preheating on the conductor core wire 1;

[0052] S4: co-extruding the inner shielding layer 3.1, the insulating layer 3.2 and the outer shielding layer 3.3 on the surface of the conductor core wire 1 to form an insulating core wire 3;

[0053] S5: passing through the post-preheater 5, electromagnetic induction heating is performed on the conductor core wire 1 inside the insulated core wire 3 to reduce the cross-linking internal stress;

[0054] S6: the insulated core wire 3 passes through the cross-linking tube 6, the cross-linking tube 6 starts to be heated and cross-linked at the inlet end, and then cross-linked by multi-stage cooling;

[0055] S7: The insulated core wire 3 is placed in a hot convection drying room 7 for degassing;

[0056] S8: wrapping a layer of semi-conductive butyl tape, two layers of semi-conductive water-resistant tape and a layer of semi-conductive water-resistant copper wire shielding tape around the outer layer of the insulated core wire 3 in sequence to form a tape-wrapped core wire;

[0057] S9: longitudinally wrap an aluminum tape 10 on the surface of the tape-wrapped core wire;

[0058] S10: performing argon arc welding on the longitudinal connection of the aluminum strip 10 to form a smooth aluminum sleeve 11;

[0059] S11: Performing online eddy current flaw detection on the weld of the smooth aluminum sleeve 11;

[0060] S12: reducing the diameter of the smooth aluminum sheath 11 so that the smooth aluminum sheath 11 and the taped core wire are pressed together to form the aluminum sheath core wire 12;

[0061] S13: spraying hot melt adhesive on the surface of the smooth aluminum sleeve 11;

[0062] S14: extruded outer sheath 13;

[0063] S15: Cooling;

[0064] S16: Reel in the line.

[0065] like Figure 2 , Figure 3 As shown, the conductor core wire 1 passes through the pre-preheater 2, the three-layer co-extrusion extruder 4, the post-preheater 5 and the cross-linking tube 6 in sequence to complete cross-linking. In step S3, the preheating temperature of the pre-preheater 2 is set at 100°C; in step S5, the preheating temperature of the post-preheater 5 is set at 140°C. In step S6, the multi-stage cooling cross-linking process is seven stages, and the temperatures are 280°C, 270°C, 265°C, 260°C, 255°C, 250°C, and 240°C in sequence; the cross-linking tube 6 includes a heating The multi-stage cooling cross-linking process takes place in the heating section 6.1, and the cross-linking tube 6 is a nitrogen-sealed space. Through the VCV special calculation software TCC, the cross-linking tube 6 adopts seven-stage heating, and the heating temperature is gradually reduced. The front preheater 2 and the rear preheater 5 are activated, and the internal and external heating methods are used. As the heating temperature of the heating section 6.1 decreases, the temperature gradient formed in the insulating core wire 3 is reduced to keep it heated evenly, while maintaining a good degree of cross-linking. Figure 3 In the figure, green (Cure) is the cross-linking degree curve, blue (Zone Temp) is the multi-segment zone temperature curve, and red (Surface Temp) is the outer ring temperature curve of the insulating layer 3.2, and pink (Conductor) is the conductor core temperature curve. During the heating process, under the action of 280°C in the first section of the heating section 6.1, the outer ring temperature of the insulating layer 3.2 rises rapidly to 230°C, and the outer ring of the insulating layer 3.2 is rapidly cross-linked, reducing the melting sag of the polyethylene solution under the action of gravity. The middle layer area of ​​the insulating layer 3.2 slowly rises from 135°C to 195°C as it moves in the cross-linked tube 6, and the inner ring temperature of the insulating layer 3.2 slowly rises to 163°C. At 60 meters, the cross-linking degree of the insulating layer 3.2 reaches more than 93%, and at 80 meters, the cross-linking degree reaches more than 98%. In addition, the temperature is reduced step by step. After the insulating core 3 leaves the heating section 6.1 of the cross-linked tube 6 and enters the cooling section 6.2 at 20 meters, the surface temperature of the insulating core 3 drops to 45°C. The cooling is timely and sufficient, and the generation of cross-linking internal stress is reduced.

[0066] like Figure 4-6As shown, after step S6 is completed, the insulating core wires 3 are layered and raised when the wires are taken up to increase the gap between each layer of the insulating core wires 3. The raising is performed by hollow pads. A heating tube 7.1 for heating the convection drying room 7 is provided on the inner wall of the convection drying room 7. A support frame 7.2 for supporting the insulating core wires 3 is provided on the axis of the convection drying room 7. The support frame 7.2 is rotatably connected in the convection drying room 7. The insulating core wires 3 are spirally stacked on the support frame 7.2. The support frame 7.2 includes an air transfer tube 7.2.1 arranged on the axis. A supporting square tube 7.2.2 is connected to the circumference of the air transfer tube 7.2.1. The supporting square tube 7.2.2 is a hollow pad. The supporting square tube 7.2.2 is evenly arrayed with air outlet holes 7.2.3, and the left and right sides and the upper and lower sides of the supporting square tube 7.2.2 are provided with air outlet holes. 7.2.3, an air transmission hole 7.2.4 is provided at the connection between the air transmission pipe 7.2.1 and the supporting square pipe 7.2.2, an exhaust fan 7.2.5 is provided below the air transmission pipe 7.2.1, an air outlet valve 7.2.7 is provided above the air transmission pipe 7.2.1, an air inlet fan 8 is provided on the outside of the convection drying room 7, the air inlet direction of the air inlet fan 8 is arranged along the tangent direction of the convection drying room 7, the heating pipe 7.1 is extended and spirally ascended along the direction of the air inlet, the heating pipe 7.1 in the figure is a schematic distribution curve, in actual production, the heating pipe 7.1 is distributed throughout the inner wall of the convection drying room 7, the spiral ascending rotation direction of the heating pipe 7.1 is the same as the rotation direction of the supporting frame 7.2, the inner side of the top surface of the convection drying room 7 is inverted cone shape, and a ventilation duct 8.1 is provided between the air outlet valve 7.2.7 and the air inlet fan 8.

[0067] like Figure 7 As shown, four airflows are finally formed in the convection drying room 7, including an airflow spiraling upward along the outer circle, an airflow spiraling downward along the outer wall of the air transfer tube 7.2.1, an airflow vertically upward inside the air transfer tube 7.2.1, and a pressure difference airflow flowing in the opposite direction along the radial direction, thereby achieving rapid diffusion of heat in the convection drying room 7, achieving overall rapid heating and degassing of the insulating core wire 3, and improving the degassing efficiency.

[0068] like Figure 8 As shown, after the insulating core wire 3 is degassed, the insulating core wire 3 needs to start from the insulating core wire pay-off frame 19, and be wrapped with a layer of semi-conductive butyl tape, two layers of semi-conductive water-resistant tape and a layer of semi-conductive water-resistant copper wire shielding tape. The combination of a layer of semi-conductive butyl tape, two layers of semi-conductive water-resistant tape and a layer of semi-conductive water-resistant copper wire shielding tape is called a semi-conductive buffer layer 9, and then pass through the aluminum strip pay-off frame 20, the forming wheel 14, the horn mold 15, the sizing mold 16, the argon arc welding gun 21, the online eddy current flaw detector 22, the roller group 17, the aluminum sleeve preheating machine 23, the atomizing spray gun 18, the outer sheath extruder 24, and the cooling water tank 25 in sequence, and arrive at the cable take-up frame 26 to complete the storage of the formed cable.

[0069] During the winding process of the semi-conductive buffer layer 9, the semi-conductive water-blocking copper wire shielding tape has a thickness of 0.5 mm, a width of 80 mm, no less than 20 copper wires, a copper wire diameter of no less than 0.2 mm, a tinned surface of the copper wire, and is woven longitudinally in an up-and-down wave-like manner. The volume resistivity is less than 500Ω·cm, and the surface resistance is less than 100Ω. The good electrical conductivity enables it to maintain a more reliable electrical connection with the smooth aluminum sleeve 11. Subsequently, the smooth aluminum sleeve 11 will be reduced in diameter by multiple groups of rollers 17, so that the semi-conductive buffer layer 9 reserves a buffer space. After the smooth aluminum sleeve 11 is reduced in diameter, it is in close surface contact with the semi-conductive buffer layer 9, maintaining reliable and good electrical performance, and avoiding the risk of suspended discharge caused by poor contact due to the gap between the wrinkled aluminum sleeve and the water-blocking tape.

[0070] like Fig. 9 As shown, in step S9, when the insulated core wire 3 passes through the aluminum strip pay-off frame 20, it will be placed on the center line of the aluminum strip 10, and then the aluminum strip 10 is longitudinally wrapped to form a smooth aluminum sleeve 11 under the action of the forming wheel 14, the horn mold 15, the sizing mold 16, and the argon arc welding gun 21. During the longitudinal wrapping process of the aluminum strip 10, two forming wheels 14 are provided. The forming wheel 14 arranged upstream is used to first lift the two side edges of the aluminum strip 10, and the forming wheel 14 arranged downstream is used to directionally bend the aluminum strip 10 and form an arc as a whole. When the aluminum strip 10 enters the horn mold 15 again, the convergence direction of the aluminum strip 10 can be guaranteed, thereby ensuring the forming quality and uniformity of the aluminum strip 10. Then, the insulating core wire 3 and the semi-circular aluminum strip 10 pass through the six-channel horn mold 15 in turn, so that the arc diameter of the aluminum strip 10 is gradually reduced, and finally passes through the sizing mold 16, and the aluminum strip 10 converges into a circle to form a smooth aluminum sleeve 11, which wraps the insulating core wire 3. The sizing die 16 will make the aluminum strip 10 in close contact with the semi-conductive buffer layer 9, and the sizing die 16 will be in close contact with the aluminum strip 10 accordingly. To ensure the quality of the aluminum strip 10, the sizing die 16 adopts a nano-diamond coating sizing die, which can reduce traction resistance and ensure that the surface of the formed smooth aluminum sleeve 11 is bright, which helps to improve the quality of the weld.

[0071] A brush may be added above the horn mold 15 to filter out debris and impurities generated by friction between the aluminum strip 10 and various molds after trimming and during the molding process, thereby increasing welding reliability.

[0072] The argon arc welding torch 21 cannot be stopped due to the operating state of the outer sheath extruder 24. The smooth aluminum sleeve 11 cannot be stopped to replace the tungsten electrode or the gas cylinder during production. Therefore, it is necessary to introduce double welding gun technology in the argon arc welding process to avoid leaking and repairing caused by replacing the tungsten electrode. The protective gas cylinders are connected in series to ensure the production needs of large lengths. During the online eddy current flaw detection process, the weld seam automatic tracking system is used to automatically identify the initial point of the weld seam and automatically track and control the weld seam through visual guidance. At the same time, horizontal and vertical two-dimensional tracking information can be obtained, which greatly reduces the requirements for environmental conditions, improves anti-interference performance, sensitivity and measurement accuracy, greatly reduces leaking welding, cold welding and other phenomena during welding, and ensures the welding quality of the smooth aluminum sleeve 11.

[0073] like Figure 8 As shown, a repair welding space is provided between the online eddy current flaw detector 22 and the roller group 17. In step S11, when leaking welding or cold welding is detected, a cold welding machine is used for online repair welding. The cold welding machine adopts the principle of capacitor energy storage to release current between the tungsten electrode and the workpiece in the form of a high-frequency pulse arc in an instant. It only takes a dozen milliseconds to complete the welding of a weld point. The heat input is concentrated, and the time for arcing and arcing is fast. There is no continuous heating of the workpiece, thereby achieving a cold welding effect, which can effectively ensure the quality of repair welding. At the same time, after the repair welding is completed, it is necessary to ensure that the inner surface of the smooth aluminum sleeve 11 is not deformed.

[0074] like Figure 8 , Fig.10 As shown, after the welding of the smooth aluminum sleeve 11 is completed, in step S12, multiple groups of roller groups 17 are used for rolling to perform gradual diameter reduction, so that the smooth aluminum sleeve 11 and the semi-conductive buffer layer 9 are more closely fitted, while improving the compactness of the cable and reducing the cable diameter. The roller group 17 includes four rollers, and the four rollers are arranged in the center along the circumference to form a diameter reduction hole 17.1 for diameter reduction. The diameters of the diameter reduction holes 17.1 of the multiple groups of roller groups 17 are reduced successively. During the diameter reduction process, the rollers rotate, and a rotating connecting buckle 17.2 is provided at the connection of the two connected rollers. The rotating connecting buckle 17.2 includes a matching parallel groove 17.2.1 and a parallel block 17.2.2. The parallel block 17.2.2 is provided on one roller, and the parallel groove 17.2.1 is provided on the other roller. The parallel block 17.2.2 is provided along the radial direction of one roller, and the parallel groove 17.2.1 is provided along the axial direction of the other roller. Each roller group 17 controls the reduction ratio to be 2-3%, and finally realizes the reduction ratio of the outer diameter of the smooth aluminum sleeve 11 to be 8-17 mm, and controls the roundness of the smooth aluminum sleeve 11 to be ≥99%. The rollers are made of MC nylon, because MC nylon has high strength, can bear load for a long time, has strong wear resistance and self-lubricating properties, can absorb noise and absorb impact. At the same time, the roller forming process has no lubricating oil pollution, which is convenient for the subsequent hot melt adhesive process.

[0075] In step S13, before the hot melt adhesive is sprayed, the smooth aluminum sleeve 11 is preheated; and the spraying is performed using a plurality of atomizing spray guns 18 evenly distributed along the circumference. In the selection of the hot melt adhesive, it is necessary to ensure that the hot melt adhesive is non-toxic and odorless, has long-term chemical stability and environmental protection, and cannot chemically react with aluminum metal and plastic molecules during repeated heating. In addition, it is also necessary to ensure that the softening point temperature of the hot melt adhesive is higher than the most demanding temperature of the cable operation to ensure the normal operation of the cable.

[0076] During the extrusion process of the outer sheath 13, the outer sheath 13 of different thicknesses has an influence on the bending performance of the cable, as shown in Table 1.

[0077] Table 1 Influence of outer sheath thickness on cable bending performance

[0078] Outer sheath thickness / mm Is the smooth aluminum sleeve wrinkled? Maximum equivalent plastic strain of smooth aluminum sleeve 0 yes 0.211 1.0 yes 0.088 2.0 yes 0.082 3.0 yes 0.080 4.0 no 0.075 5.0 no 0.073

[0079] Through experiments, it is found that in actual production, the thicker the non-metallic outer sheath 13 is, the stronger the bending resistance of the smooth aluminum sheath cable is, and the maximum equivalent plastic strain on the bending compression side continues to decrease. It is recommended that 750kV ultra-high voltage cross-linked polyethylene smooth aluminum cable use an outer sheath 13 of more than 5mm.

[0080] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. All changes made within the scope of protection of the independent claims of the present invention are within the scope of protection of the present invention.

Claims

1. A production process for 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable, It is characterized in that The following steps are involved: S1: A round conductor is pressed to form a conductor core (1.1); S2: A Z-shaped conductor is twisted into a ring-shaped conductor outer core (1.2) and is tightly wrapped around a conductor inner core (1.1); S3: passing a conductor core wire (1) composed of a conductor inner core (1.1) and a conductor outer core (1.2) through a preheater (2) to perform electromagnetic induction preheating on the conductor core wire (1); S4: co-extruding an inner shielding layer (3.1), an insulating layer (3.2) and an outer shielding layer (3.3) on the surface of the conductor core wire (1) to form an insulating core wire (3); S5: passing through a post-preheater (5) to perform electromagnetic induction heating on the conductor core wire (1) inside the insulating core wire (3) to reduce cross-linking internal stress; S6: the insulated core wire (3) passes through the cross-linking tube (6), the cross-linking tube (6) starts to be heated and cross-linked at the inlet end, and then cross-linked by multi-stage cooling; S7: The insulated core wire (3) is placed in a hot convection drying room (7) for degassing; S8: wrapping a layer of semi-conductive butyl tape, two layers of semi-conductive water-repellent tape and a layer of semi-conductive water-repellent copper wire shielding tape around the outer layer of the insulated core wire (3) in sequence to form a tape-wrapped core wire; S9: longitudinally wrapping an aluminum tape (10) on the surface of the tape-wrapped core wire; S10: performing argon arc welding on the longitudinal connection of the aluminum strip (10) to form a smooth aluminum sleeve (11); S11: Performing online eddy current flaw detection on the weld of the smooth aluminum sleeve (11); S12: reducing the diameter of the smooth aluminum sheath (11) so that the smooth aluminum sheath (11) and the taped core wire are pressed together to form an aluminum sheath core wire (12); S13: spraying hot melt adhesive on the surface of the smooth aluminum sleeve (11); S14: extruded outer sheath (13); S15: Cooling; S16: Reel in the line.

2. According to the production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable described in claim 1, Features: In step S3, the preheating temperature of the preheater (2) is set at 80-100°C; In step S5, the preheating temperature of the post-preheater (5) is set at 140-160°C; In step S6, the multi-stage cooling and cross-linking process consists of seven stages, and the temperatures are 280°C, 270°C, 265°C, 260°C, 255°C, 250°C, and 240°C respectively.

3. According to the production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable described in claim 1, Features: After step S6 is completed, the insulating core wires (3) are layered and raised when the wires are collected, so as to increase the gap between each layer of the insulating core wires (3), and hollow pads are used for the raising.

4. According to the production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable as described in claim 3, Features: A heating tube (7.1) for heating the convection drying room (7) is provided on the inner wall of the convection drying room (7); a support frame (7.2) for supporting the insulating core wire (3) is provided on the axis of the convection drying room (7); the support frame (7.2) is rotatably connected in the convection drying room (7); the insulating core wire (3) is spirally stacked on the support frame (7.2); the support frame (7.2) includes an air transmission pipe (7.2.1) provided on the axis; The air transfer pipe (7.2.1) is connected to a supporting square pipe (7.2.2) in the circumferential direction, the supporting square pipe (7.2.2) is provided with air outlet holes (7.2.3) in a uniform array, the connection between the air transfer pipe (7.2.1) and the supporting square pipe (7.2.2) is provided with air transfer holes (7.2.4), an exhaust fan (7.2.5) is provided below the air transfer pipe (7.2.1), and an air outlet valve (7.2.7) is provided above the air transfer pipe (7.2.1).

5. According to the production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable as described in claim 4, Features: An air inlet fan (8) is arranged on the outside of the convection drying room (7); the air inlet of the air inlet fan (8) is arranged along the tangent direction of the convection drying room (7); the heating tube (6.1) is arranged to extend in a spiral upward direction along the direction of the air inlet; the spiral upward rotation direction of the heating tube (6.1) is the same as the rotation direction of the support frame (6.2); and the inner side of the top surface of the convection drying room (7) is in an inverted cone shape.

6. The production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable according to claim 5, Features: A ventilation duct (8.1) is provided between the air outlet valve (6.2.6) and the air inlet fan (8).

7. According to the production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable described in claim 1, Features: In step S9, during the longitudinal wrapping process of the aluminum strip (10), the aluminum strip (10) passes through the forming wheel (14), the four to six-lane horn mold (15), and the sizing mold (16) in sequence, and then converges into a circle. The sizing mold (16) is a nano-diamond coated sizing mold.

8. According to the production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable described in claim 1, Features: In step S11, when leaky welding or cold welding is detected, a cold welding machine is used to perform online repair welding.

9. The production process of the 750kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable according to claim 1, Features: In step S12, multiple groups of roller groups (17) are used for rolling to perform gradual diameter reduction. The roller group (17) includes four rollers, and the four rollers are arranged in the center along the circumferential direction to form a diameter reduction hole (17.1) for diameter reduction. The diameters of the diameter reduction holes (17.1) of the multiple groups of roller groups (17) are reduced in sequence. During the diameter reduction process, the rollers rotate. A rotating connecting buckle (17.2) is provided at the connection of two connected rollers. The rotating connecting buckle (17.2) includes a matching parallel groove (17.2.1) and a parallel block (17.2.2). The parallel block (17.2.2) is provided on one roller, and the parallel groove (17.2.1) is provided on the other roller. The parallel block (17.2.2) is provided along the radial direction of one roller, and the parallel groove (17.2.1) is provided along the axial direction of the other roller. The rollers are made of MC nylon.

10. The production process of the 750 kV ultra-high voltage cross-linked polyethylene smooth aluminum sheathed cable according to claim 1, Features: In step S13, before the hot melt adhesive is sprayed, the smooth aluminum sleeve (11) is preheated, and the aluminum sleeve core wire (12) passes through the embracing heating device. The surface temperature of the smooth aluminum sleeve (9) is raised to 60 degrees by infrared heating, and then a plurality of atomizing spray guns (18) evenly distributed along the circumference are used for spraying.

Citation Information

Patent Citations

  • The device is suitable for cable core drying devices

    CN212724845U

  • Improvements in and relating to tanks for drying, vulcanizing, accommodating, or impregnating electric cables

    GB346704A

Cited By

  • Compression conductor cable and compression molding system for production thereof

    CN119207866A

  • Cross-linked polyethylene insulated composite cable based on skin effect technology

    CN120496926A