Round stranded wire roundness control method

By using nylon paint to replace lubricant in the production of round strands and combined with the molding mold to process, the roundness problem caused by lubricant inhomogeneity is solved, the performance of the wire and the uniformity of the round strands are improved, and the coil is ensured. quality.

CN119028668APending Publication Date: 2024-11-26GUANGDONG SUNTEK WIRE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411057810.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the production process of round strands, the volatile and uneven coating of lubricating oil leads to inconsistent lubrication of wires, affecting the uniformity of roundness, and thus reducing the quality of the extrusion line.

Method used

Nylon paint is used instead of lubricating oil to form a lubricating paint film, and the multiple strands of enameled single wires are extruded and smoothly formed through a constant tension lay-up frame and a shaping mold to ensure the consistency of the roundness and size of the wire harness.

Benefits of technology

The insulation, wear resistance, heat resistance and moisture resistance of the wire are improved, and the stability prevents defects caused by uneven lubrication, ensuring the uniformity of the roundness of the round stranded wire and the quality of the coil finished product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for controlling roundness of a round stranded wire, which comprises the following steps of: manufacturing a plurality of strands of enameled single wires, and coating nylon paint on the peripheries of the enameled single wires to form a lubricating paint film; conveying the enameled single wires by using a constant-tension pay-off rack to maintain the tension of the enameled single wires, averagely dividing the plurality of strands of enameled single wires into five groups of wire harnesses, and enabling the five groups of wire harnesses to respectively penetrate through a wire inlet mesh plate to enter a shaping mold; wherein five threading holes which are circumferentially and uniformly distributed around the center of the wire inlet mesh plate are formed in the wire inlet mesh plate, each group of wire harnesses correspond to one threading hole for threading, and the center of the wire inlet mesh plate and the axis of a wire passing channel of the shaping mold are located on the same axis; then, the five groups of wire harnesses are extruded and smoothly shaped through a shaping mold, so that a plurality of strands of enameled single wires are ensured to be straightly led out; and finally, stranding the plurality of enameled single wires leaving the shaping mold to form the round stranded wire. According to the invention, the uniformity of the overall roundness of the wire rod can be improved, so that the quality of a coil finished product manufactured subsequently is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wire production, and in particular relates to a roundness control method for round stranded wires. Background Art

[0002] Extruded wire is a stranded wire made of multiple strands of enameled single wires, and then an insulating layer or sheath is injected on the surface of the stranded wire through an extruder to improve insulation and mechanical properties. It can be widely used in transformers or inductors in high-frequency and high-voltage working environments, such as antenna inductors, LCD TVs, LED energy-saving lamps, etc. Since the advent of silk-covered wire products in the 1980s, its market size and application areas have been expanding year by year, especially in recent years, the demand for extruded wires for high-power electrical equipment has been gradually increasing.

[0003] The roundness uniformity of the extruded wire is an important quality indicator that needs to be strictly controlled during the design and manufacturing process of the wire, and has a direct impact on the overall performance and application effect of the wire. As a semi-finished product of the extruded wire, the roundness control of the round stranded wire after twisting directly affects the roundness uniformity of the extruded wire. During the production process, the enameled single wire is generally lubricated with lubricating oil on its surface, which can reduce the friction and wear of the wire harness during the twisting process. However, since too much or too little lubricating oil will affect the production environment and the performance of the wire, the lubricating oil needs to be controlled in an appropriate amount during the coating process. However, the lubricating oil itself is volatile, and its concentration will change with the ambient temperature and humidity. It is also easy to be touched and fall off, causing local changes in the thickness of the lubricating oil, making the overall lubrication of the wire inconsistent, affecting the subsequent twisting process, thereby reducing the uniformity of the roundness of the round stranded wire, resulting in uneven roundness of the extruded wire, causing irregular deformation of the extruded wire during the coil making process, affecting the quality of the finished coil. Summary of the invention

[0004] The object of the present invention is to provide a round stranded wire roundness control method capable of improving the uniformity of the overall roundness of the wire.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A method for controlling the roundness of a round stranded wire comprises the following steps:

[0007] Step 1: preparing a plurality of enameled single wires, and coating the outer circumference of the enameled single wires with nylon paint to form a lubricating paint film;

[0008] Step 2: Use a constant tension pay-off rack to convey the enameled single wire to maintain the tension of the enameled single wire, and evenly divide the multiple strands of enameled single wire into 5 groups of wire bundles, and the 5 groups of wire bundles respectively pass through the wire inlet mesh plate into the shaping mold; wherein, the wire inlet mesh plate is provided with 5 threading holes evenly distributed around the center of the wire inlet mesh plate, each group of wire bundles corresponds to a threading hole for threading, and the center of the wire inlet mesh plate and the axis of the wire passage of the shaping mold are located on the same axis;

[0009] Step 3: Use a shaping die to extrude and shape the 5 sets of wire harnesses smoothly to ensure that the multiple enameled single wires are straight out;

[0010] Step 4: Twisting the multiple strands of enameled single wires after leaving the shaping die to form round stranded wires.

[0011] As a preferred embodiment of the present invention, in the step 1, the thickness of the nylon paint is 0.8 μm to 1.2 μm.

[0012] As a preferred embodiment of the present invention, in the step 1, the thickness of the nylon paint is 1 μm.

[0013] As a preferred solution of the present invention, in step three, the relative deformation rate of the five groups of wire harnesses when passing through the shaping die is 4% to 6%.

[0014] As a preferred solution of the present invention, in step three, the relative deformation rate of the five groups of wire harnesses when passing through the shaping die is 5%.

[0015] As a preferred embodiment of the present invention, the cross-sectional shape of the wire passage of the shaping die is circular.

[0016] As a preferred solution of the present invention, the wire inlet of the wire passage of the shaping die is provided with a trumpet-shaped guiding arc surface.

[0017] The roundness control method of a round stranded wire provided by the embodiment of the present invention has the following beneficial effects compared with the prior art:

[0018] The roundness control method of the round stranded wire of the present invention adopts nylon paint instead of lubricating oil, so that a lubricating paint film is formed on the periphery of the enameled single wire. Nylon paint is a material with good insulation performance. The enameled single wire coated with nylon paint has good wear resistance, flexibility and adhesion, a small surface friction coefficient, and good lubrication, which can reduce the friction and wear of the wire harness during the twisting process, thereby improving the twisting efficiency and the quality of the finished cable; at the same time, nylon paint as a lubricating paint film can also improve the heat resistance, chemical resistance and moisture resistance of the enameled single wire. In the production process of the round stranded wire, nylon paint The performance of Longqi is stable and will not change with changes in ambient temperature and humidity, ensuring the uniformity of the overall lubrication of the enameled single wire, thereby effectively preventing uneven lubrication from causing defects in the wire harness during the twisting process, such as wire breakage, deformation or damage; in addition, the multiple strands of enameled single wire are squeezed and smoothly shaped through the shaping mold to ensure that the wire harness remains straight when leaving the mold. At the same time, the use of the shaping mold helps to improve the roundness of the wire harness, ensuring that any cross-section of the wire harness is close to a perfect circle and the required size, improving the uniformity of the roundness of the round stranded wire, and facilitating the subsequent use of the wire for coil winding. DETAILED DESCRIPTION

[0019] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0020] A preferred embodiment of the present invention provides a method for controlling the roundness of a round stranded wire, which comprises the following steps:

[0021] Step 1: preparing a plurality of enameled single wires, and coating the outer circumference of the enameled single wires with nylon paint to form a lubricating paint film;

[0022] Step 2: Use a constant tension pay-off rack to convey the enameled single wire to maintain the tension of the enameled single wire, and evenly divide the multiple strands of enameled single wire into 5 groups of wire bundles, and the 5 groups of wire bundles respectively pass through the wire inlet mesh plate into the shaping mold; wherein, the wire inlet mesh plate is provided with 5 threading holes evenly distributed around the center of the wire inlet mesh plate, each group of wire bundles corresponds to a threading hole for threading, and the center of the wire inlet mesh plate and the axis of the wire passage of the shaping mold are located on the same axis;

[0023] Step 3: Use a shaping die to extrude and shape the 5 sets of wire harnesses smoothly to ensure that the multiple enameled single wires are straight out;

[0024] Step 4: Twisting the multiple strands of enameled single wires after leaving the shaping die to form round stranded wires.

[0025] According to a round stranded wire roundness control method of an embodiment of the present invention, nylon paint is used instead of lubricating oil to form a lubricating paint film on the periphery of the enameled single wire. Nylon paint is a material with good insulation performance. The enameled single wire coated with nylon paint has good wear resistance, flexibility and adhesion, a small surface friction coefficient, and good lubrication, which can reduce the friction and wear of the wire harness during the twisting process, thereby improving the twisting efficiency and the quality of the finished cable. At the same time, nylon paint as a lubricating paint film can also improve the heat resistance, chemical resistance and moisture resistance of the enameled single wire, which is very important in the production of round stranded wires. During the process, the performance of nylon paint is stable and will not change with changes in ambient temperature and humidity, ensuring the uniformity of the overall lubrication of the enameled single wire, thereby effectively preventing uneven lubrication from causing defects in the wire harness during the twisting process, such as wire breakage, deformation or damage; in addition, the multiple strands of enameled single wire are squeezed and smoothly shaped through the shaping mold to ensure that the wire harness remains straight when leaving the mold. At the same time, the use of the shaping mold helps to improve the roundness of the wire harness, ensuring that any cross-section of the wire harness is close to a perfect circle and the required size, improving the uniformity of the roundness of the round stranded wire, and facilitating the subsequent use of the wire for coil winding.

[0026] Exemplarily, in step one, the thickness of the nylon paint is 0.8 μm to 1.2 μm, preferably 1 μm, to ensure that the nylon paint forms an effective lubricating paint film while preventing the nylon paint from being too thick and affecting the performance of the original wire.

[0027] Exemplarily, in step three, the relative deformation rate of the five groups of wiring harnesses when passing through the molding die is 4% to 6%, preferably 5%, to ensure that the wiring harnesses can achieve the desired shape and size during the extrusion molding process, while avoiding excessive deformation that causes damage to the nylon paint and affects the uniformity of the lubrication effect.

[0028] Exemplarily, the cross-sectional shape of the wire passage of the shaping mold is circular, so that the wire harness is squeezed into a circle when passing through the wire passage of the shaping mold.

[0029] Exemplarily, the wire inlet of the wire passage of the shaping mold is provided with a trumpet-shaped guiding arc surface. The trumpet-shaped guiding arc surface gradually widens at one end to form a smooth transition area, so that each group of wire harnesses can be smoothly gathered and merged into the shaping mold.

[0030] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A method for controlling the roundness of a round stranded wire, characterized in that: The steps include: Step 1: preparing a plurality of enameled single wires, and coating the outer circumference of the enameled single wires with nylon paint to form a lubricating paint film; Step 2: Use a constant tension pay-off rack to convey the enameled single wire to maintain the tension of the enameled single wire, and evenly divide the multiple strands of enameled single wire into 5 groups of wire bundles, and the 5 groups of wire bundles respectively pass through the wire inlet mesh plate into the shaping mold; wherein, the wire inlet mesh plate is provided with 5 threading holes evenly distributed around the center of the wire inlet mesh plate, each group of wire bundles corresponds to a threading hole for threading, and the center of the wire inlet mesh plate and the axis of the wire passage of the shaping mold are located on the same axis; Step 3: Use a shaping die to extrude and shape the 5 sets of wire harnesses smoothly to ensure that the multiple enameled single wires are straight out; Step 4: Twisting the multiple strands of enameled single wires after leaving the shaping die to form round stranded wires.

2. The round stranded wire roundness control method according to claim 1, characterized in that: In the step 1, the thickness of the nylon paint is 0.8 μm to 1.2 μm.

3. The roundness control method of round stranded wire according to claim 1, characterized in that: In the step 1, the thickness of the nylon paint is 1 μm.

4. The roundness control method of round stranded wire according to claim 1, characterized in that: In the step three, the relative deformation rate of the five wire harnesses when passing through the shaping die is 4% to 6%.

5. The round stranded wire roundness control method according to claim 4, characterized in that: In the step three, the relative deformation rate of the five wire harnesses when passing through the shaping die is 5%.

6. The roundness control method of round stranded wire according to claim 1, characterized in that: The cross-sectional shape of the wire passage of the shaping die is circular.

7. The round stranded wire roundness control method according to claim 6, characterized in that: The wire inlet of the wire passage of the shaping die is provided with a horn-shaped guiding arc surface.