Semiconductor film layer etching method and semiconductor process equipment

Through the atomic layer etching process, the problem of lateral erosion of the side wall of the electrode contact layer in the traditional method is solved, and the yield and performance of GaN HEMT devices are improved.

CN119028821APending Publication Date: 2024-11-26BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411111106.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the etching process of GaN HEMT devices, traditional methods cause lateral erosion of the side walls of the electrode contact layer, affecting the device conductivity and contact resistance, especially in high integration and small-size chips.

Method used

The GaN cap layer and the AlGaN layer interface are etched by atomic layer etching process. Through gas adsorption, atomic layer reaction and cycle etching steps, the GaN cap layer is gradually removed until the AlGaN layer is reached, avoiding the transverse direction of the side wall of the electrode contact layer. Side erosion.

Benefits of technology

It effectively improves the yield of the device, avoids lateral erosion of the side walls of the TiN electrode contact layer, and ensures the device's conductivity and stability of the contact resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028821A_ABST
    Figure CN119028821A_ABST
Patent Text Reader

Abstract

The invention discloses an etching method of a semiconductor film layer and semiconductor process equipment, and the etching method comprises the steps: etching an electrode contact layer in a preset region until a GaN cap layer is exposed, and forming an electrode contact layer pattern; etching the exposed GaN cap layer to a set depth; and continuously etching the residual GaN cap layer by adopting an atomic layer etching process until the AlGaN layer is etched. According to the invention, the lateral erosion of the side wall of the electrode contact layer can be avoided in the interface etching process of the GaN cap layer and the AlGaN layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor device manufacturing, and more specifically, to an etching method for a semiconductor film layer and semiconductor process equipment. Background Art

[0002] Normally-off GaN high electron mobility transistors (HEMTs) devices usually include the following material structures: Figure 1 The film structure shown is: SiO2 mask layer, TiN ohmic contact layer, p-GaN cap layer, AlGaN functional layer, intrinsic GaN layer and Si or SiC substrate layer. In order to ensure the performance of subsequent devices, the upper metal material of p-GaN material usually uses TiN as the conductor material. By utilizing its dense structure and pores, the GaN HEMT normally-off device can reduce the metal interconnection on-resistance in the subsequent process and avoid the atomic pinning problem introduced by metal atom diffusion. Therefore, the TiN conductive metal material layer has a crucial impact on the device performance.

[0003] Traditional GaN HEMT device etching usually adopts step-by-step etching, etching the mask layer, electrode contact layer, p-GaN cap layer and finally stopping at the AlGaN layer. However, as the device integration requirements become higher and higher, the chip size becomes smaller and smaller, and the corresponding gate line width (CD) becomes narrower and narrower (usually below 0.5um), and the corresponding etching loading effect becomes more and more obvious. In order to ensure the yield level of the whole chip, the normally-off GaN HEMTs device will increase the over-etching ratio to ensure performance; secondly, in order to ensure the conduction performance of the two-dimensional electron gas, the over-etching amount of the AlGaN film layer must be guaranteed. Therefore, the etching process from p-GaN to AlGaN in the subsequent process technology usually requires a formula system with a high selectivity ratio for AlGaN. The corresponding gas formula generally adopts a Cl-based or F-based mixed gas system, and this gas system will produce obvious side etching on the TiN sidewall material, affecting the device conduction performance and contact resistance. Summary of the invention

[0004] The purpose of the present invention is to provide a semiconductor film etching method and semiconductor process equipment, so as to avoid lateral side etching of the electrode contact layer side wall during the etching process of the interface between the GaN cap layer and the AlGaN layer.

[0005] To achieve the above object, the present invention provides an etching method for a semiconductor film layer, wherein the semiconductor film layer structure comprises an AlGaN layer, a GaN cap layer and an electrode contact layer stacked in sequence from bottom to top; the etching method comprises:

[0006] Etching the electrode contact layer in a preset area until the GaN cap layer is exposed to form an electrode contact layer pattern;

[0007] Etching the exposed GaN cap layer to a set depth;

[0008] The remaining GaN cap layer is continuously etched using an atomic layer etching process until the AlGaN layer is etched.

[0009] Optionally, the atomic layer etching process includes:

[0010] Gas adsorption step: introducing a first process gas into the process chamber so that the first process gas is adsorbed on the surface of the GaN cap layer;

[0011] Atomic layer reaction step: continue to introduce the first process gas into the process chamber and load RF power, so that the first process gas reacts with the surface atomic layer of the GaN cap layer to form a transition layer;

[0012] Atomic layer etching step: introducing a second process gas into the process chamber, and sequentially loading upper RF power and lower RF power to remove the transition layer;

[0013] The gas adsorption step-the atomic layer etching step is cyclically executed for a set number of times until the AlGaN layer is etched.

[0014] Optionally, the atomic layer etching process further includes:

[0015] After the atomic layer reaction step, a first purge step is performed: introducing a purge gas into the process chamber to remove the residual first process gas and byproducts in the process chamber;

[0016] A second purge step is performed after the atomic layer etching step: a purge gas is introduced into the process chamber to remove residual etching byproducts in the process chamber.

[0017] Optionally, the first process gas includes at least one of Cl2, BCl3, and HBr.

[0018] Optionally, the second process gas includes at least one of Ar, N2, O2, Kr, Xe, and Ne.

[0019] Optionally, the purge gas is the same as the second process gas.

[0020] Optionally, the first process gas includes Cl2, and the process parameters used in the gas adsorption step include:

[0021] Cl2 flow rate range: 20sccm~200sccm;

[0022] The chamber pressure range is: 3mt~10m.

[0023] Optionally, the process parameters used in the atomic layer reaction step include:

[0024] The upper RF power range is: 50W~200W;

[0025] Cl2 flow rate range: 20sccm~200sccm;

[0026] The chamber pressure range is: 3mt~10mt.

[0027] Optionally, the second process gas includes Ar, and the process parameters used in the atomic layer etching step include:

[0028] Ar flow range: 20sccm~200sccm;

[0029] The chamber pressure range is 3mt to 10mt;

[0030] The upper RF power range is 50W to 200W;

[0031] The lower RF power range is 3W to 15W.

[0032] Optionally, the purge gas includes Ar, and the process parameters used in the first purge step and the second purge step include:

[0033] The Ar flow rate range is: 100 sccm~1000 sccm.

[0034] Optionally, the process parameters used in the atomic layer etching process also include:

[0035] The process temperature range is: -20℃~40℃.

[0036] Optionally, the set depth is 1 / 2 to 2 / 3 of the thickness of the GaN cap layer.

[0037] The present invention also proposes a semiconductor process equipment, including a process chamber, an air intake assembly, an upper electrode assembly, a lower electrode assembly and a controller, wherein the controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the above-mentioned semiconductor film layer etching method is implemented.

[0038] The beneficial effects of the present invention are:

[0039] The semiconductor film layer etching method of the present invention, for the semiconductor film layer structure, first etches the electrode contact layer in a preset area until the GaN cap layer is exposed to form an electrode contact layer pattern, then etches the exposed GaN cap layer to a set depth, and then uses an atomic layer etching process to continue etching the remaining GaN cap layer until the AlGaN layer is etched. The method etches the remaining GaN cap layer through the atomic layer etching process, and can avoid lateral side etching of the side wall of the electrode contact layer during the etching process of the GaN cap layer-AlGaN layer interface, thereby improving the device yield.

[0040] The system of the present invention has other characteristics and advantages, which will be apparent from the drawings incorporated herein and the following detailed description, or will be described in detail in the drawings incorporated herein and the following detailed description, which together serve to explain the specific principles of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, in which like reference numerals generally represent like components.

[0042] Figure 1 The film structure of the normally-off GaN HEMT device is shown.

[0043] Figure 2 A schematic diagram of the etching process of a GaN HEMTs device using a conventional step-by-step etching process in prior art 1 is shown.

[0044] Figure 3 The cross-sectional view of conventional GaN HEMTs in prior art 1 after each etching step is shown.

[0045] Figure 4 A schematic diagram of the etching process of a GaN HEMTs device using a spacer-added process according to prior art 2 is shown.

[0046] Figure 5 A flowchart showing a method for etching a semiconductor film layer according to an embodiment of the present invention is shown.

[0047] Figure 6 A film layer structure diagram corresponding to each step of a semiconductor film layer etching method according to an embodiment of the present invention is shown.

[0048] Figure 7 A flow chart of an atomic layer etching process in a semiconductor film etching method according to an embodiment of the present invention is shown.

[0049] Figure 8The cross-sectional views after etching at each step of a semiconductor film etching method according to an embodiment of the present invention are shown.

[0050] Fig. 9 A structural diagram of a semiconductor process equipment according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0051] Prior art 1 uses a traditional step-by-step etching scheme to Figure 1 The film structure shown is etched to complete the etching of GaN HEMTs device, such as Figure 2 As shown, the mask layer (SiO2), TiN layer and p-GaN layer are etched step by step and stopped at the AlGaN layer (a small amount of over-etching of AlGaN is allowed due to contact resistance).

[0052] The typical etching recipe of GaN HEMTs is shown in Table 1. The etching results are as follows: Figure 3 As shown, the CD size of the chip is less than 1um.

[0053] Table 1: Commonly used process menu for traditional step-by-step etching scheme

[0054]

[0055] (Pressure value unit: mt; Power value unit: Watt; Gas flow value: sccm)

[0056] The recipe in the prior art 1 is used for etching. As the film layer is etched to the bottom p-GaN and AlGaN interface, in order to ensure a high p-GaN / AlGaN material selectivity (usually the p-GaN / AlGaN selectivity needs to be above 15, otherwise the AlGaN film layer is easily etched through), the gas system in this scheme adopts a conventional Cl and F-based gas system; and as the etching process reaches the AlGaN interface, the p-GaN on the interface is gradually consumed. At this time, the plasma in the chamber is mainly used to react with AlGaN, but because the etching rate of the bottom AlGaN surface is slow, the concentration of Cl-based and F-based plasmas in the chamber rises sharply and scatters when reaching the wafer surface, resulting in a significant enhancement of lateral chemical etching, and lateral side etching of TiN material, such as Figure 3 As shown in the morphology; and with the extension of the over-etching time, the lateral side etching of the TiN side wall will continue to deteriorate, and the window time is small, so the etching morphology cannot meet the requirements, affecting the electrical performance of the device.

[0057] The present invention provides a semiconductor film layer etching method and semiconductor process equipment, which can be applied to the preparation of normally-off GaN HEMTs devices. In the conventional step-by-step etching scheme of GaN HEMTs, the present invention solves the lateral undercut problem of the TiN electrode contact layer in the p-GaN and AlGaN interface etching process by combining a multi-step cycle ALE mode etching scheme in the step-by-step etching steps.

[0058] The present invention will be described in more detail below with reference to the accompanying drawings. Although preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0059] Example 1

[0060] This embodiment provides a method for etching a semiconductor film layer. The semiconductor film layer structure etched in this embodiment includes an AlGaN layer, a GaN cap layer and an electrode contact layer stacked in sequence from bottom to top, and the semiconductor film layer structure also includes a mask layer and a patterned photoresist layer (PR) located on the electrode contact layer, and an intrinsic GaN layer and a substrate layer located below the AlGaN layer. The material of the electrode contact layer can be a metal material, such as TiN, Wu, etc., the material of the GaN cap layer is P-type GaN, the material of the mask layer is SiO2, and the substrate layer is a silicon substrate.

[0061] The specific process flow of the semiconductor film etching method of this embodiment is as follows: Figure 5 As shown, the film structure corresponding to each step is as follows Figure 6 As shown, the specific etching process steps are as follows:

[0062] S1: etching the electrode contact layer in a preset area until the GaN cap layer is exposed to form an electrode contact layer pattern;

[0063] This step specifically includes:

[0064] S101: etching the mask layer to form an opening exposing the electrode contact layer;

[0065] It should be noted that the following embodiments of the present application are illustrated by taking the electrode contact layer as a TiN layer as an example.

[0066] In this step, F-based gas is used to perform opening etching on the mask layer using the patterned photoresist layer, and the etching stop surface stops at the underlying TiN layer. The F-based gas used in this embodiment is preferably CF4 gas.

[0067] The specific implementation process of this step is: pass the wafer to be etched into the process chamber and introduce CF4 gas, wherein the CF4 gas is 20 to 200 sccm; maintain a certain chamber pressure, and the pressure range is preferably a fixed value between 3mt and 15mt. By applying a certain upper electrode power, the gas in the chamber is ionized to generate plasma, and the upper RF power range is preferably 100-800W; then apply a certain lower electrode power to accelerate the plasma downward to bombard the surface of the mask layer for etching, and the lower RF power range is preferably 10 to 150W; introduce a certain pressure of He gas under the wafer to cool the wafer, reduce the surface temperature of the wafer, and control the surface temperature of the wafer in the range of 50 to 110°C; the etching time is preferably 40 to 100s. The chemical reaction formula involved in the process of etching the SiO2 mask layer in this step is as follows:

[0068] CF4→CF3 + +F*+e

[0069] SiO2+CF3 + +F*+e→SiF4↑+CO2↑

[0070] This step is to make mask openings for subsequent etching of the electrode contact layer and the GaN cap layer. The thickness of the mask layer needs to ensure that the mask material can meet the etching requirements of the subsequent film layers.

[0071] S102: etching the electrode contact layer until the GaN cap layer is exposed;

[0072] In this step, a F-based gas system is used to etch the TiN film layer, and the etching stop layer stops on the GaN cap layer (EPD can be used to capture the end point). In this embodiment, the etching gas is preferably SF6 and Ar.

[0073] The specific implementation process of this step is: first, N2 is purged in the process chamber to remove the chamber by-products, and the purging time is preferably 30 to 120 seconds; after completion, SF6 and Ar gas are introduced into the chamber, wherein the ratio of Ar:SF6 gas is 1:1 to 1:6; a certain chamber pressure is maintained, and the preferred pressure range is a fixed value between 1.5mt and 8mt. By applying a certain upper electrode power, the gas in the chamber is ionized to generate plasma, and the upper RF power is preferably in the range of 100-800W; then a certain lower electrode power is applied to accelerate the plasma downward to bombard the material surface for etching, and the lower RF power is preferably in the range of 10-150W; a certain pressure of He gas is introduced under the wafer to cool the wafer, reduce the surface temperature of the wafer, and control the surface temperature of the wafer at 70 to 110°C; the etching time is preferably 50 to 150s; the chemical reaction formula involved in the etching of the TiN layer in this step is as follows:

[0074] SF6→SF5 + +F*+e

[0075] Ar→Ar + +e

[0076] TiN+SF x + +yF*+Ar + +2e→TiF4↑+Ar↑+N2↑+SF6↑

[0077] It should be noted that the etching angle in this step needs to be as large as possible to avoid side etching during the subsequent etching of the GaN cap layer, which may cause serious lateral CD shrinkage of the TiN layer.

[0078] S2: Etching the exposed GaN cap layer to a set depth;

[0079] In this step, the GaN cap layer is etched to a certain depth using a Cl2+Ar or Cl2+BCl3 gas system (usually the etching depth is required to be more than half of the thickness of the GaN cap layer to ensure the overall bottom roughness). In this embodiment, the GaN cap layer is mainly etched using a Cl2+Ar gas system, and the set etching depth is 1 / 2 to 2 / 3 of the thickness of the GaN cap layer.

[0080] The specific implementation process of this step is: first, N2 is purged in the chamber to remove the etching by-products in the process chamber, and the purging time is preferably 30 to 120 seconds; after completion, Cl2 and Ar gases are introduced into the chamber, wherein the Cl:Ar gas ratio range is preferably 10:1 to 20:1; a certain chamber pressure is maintained, and the pressure range is preferably a fixed value between 1.5mt and 5mt. By applying a certain upper electrode power, the gas in the chamber is ionized to generate plasma, and the upper RF power range is preferably 50-300W; then a certain lower electrode power is applied to accelerate the plasma downward to bombard the material surface for etching, and the lower RF power range is preferably 0-150W; a certain pressure of He gas is introduced under the wafer to cool the wafer and reduce the surface temperature of the wafer, so that the surface temperature of the wafer is controlled at 70-110°C; the etching time is preferably 10-60s, and the etching depth is required to exceed 1 / 2 of the thickness of the GaN cap layer (the thickness of the GaN cap layer is D, the main etching depth is required to exceed 1 / 2D, and the etching depth is designed to be in the range of 1 / 2D to 2 / 3D to ensure the subsequent etching of the AlGaN surface roughness); the chemical reaction formula involved in the main etching process of the GaN cap layer in this step is as follows:

[0081] Cl2→2Cl-+e

[0082] GaN (bulk material) + Ar + +e→GaN↑(molecule)+Ar(physical bombardment)

[0083] GaN+Cl-→GaCl3↑+N2↑.

[0084] In other embodiments, this step may also use an etching system of BCl3 and SF6 to perform main etching on the GaN cap layer, and the adopted process parameters include: chamber pressure range is 3 to 30mt; upper RF power range is: 100 to 500W; lower RF power range is: 5 to 30W; BCl3 flow range is: 10 to 100sccm, SF6 gas flow range is: 5 to 50sccm; N2 flow range is: 0 to 3sccm; back He pressure range is: 4 to 8T; chiller temperature range is -20 to 40°C; ventilation time: 10 to 150s.

[0085] S3: Continue to etch the remaining GaN cap layer using an atomic layer etching process until the AlGaN layer is etched.

[0086] like Figure 7 As shown, the atomic layer etching process of this embodiment includes the following cyclic etching process steps S301-S305:

[0087] S301-gas adsorption step: introducing a first process gas into the process chamber so that the first process gas is adsorbed on the surface of the GaN cap layer;

[0088] Optionally, the first process gas may include at least one of Cl2, BCl3, and HBr. In this embodiment, the first process gas is preferably Cl2. Preferably, the process parameters used in this step include: Cl2 flow range: 20sccm~200sccm; chamber pressure range: 3mt~10mt, ventilation time range: 0.5s~5s; back He cooling pressure range: 4~8T, process temperature (chiller temperature) range: -20~40℃. The above process conditions can achieve the adsorption of Cl2 molecules on the GaN surface.

[0089] Among them, Cl2 gas is selected at 20-200sccm, which is mainly used for gas adsorption on the GaN surface to prepare for the next step of processing; the chamber pressure range is selected at 3-10mt, and the gas surface adsorption pressure needs to be prepared for the subsequent RF ignition; the ventilation time is selected at 0.5-5s, which is the time for gas adsorption on the wafer surface, which is related to the surface state of the wafer to ensure that the gas on the wafer surface can be completely wetted and adsorbed; the back He pressure is selected at 4-8T, which is used to cool the wafer and is determined according to the gas demand on the adsorbed sample surface (high temperature, increased free energy of gas molecules, and possible detachment from the adsorbed sample surface); the process temperature is selected at -20-40℃, which is consistent with the back He pressure condition requirements and can meet the sample gas adsorption.

[0090] S302-atomic layer reaction step: continue to introduce the first process gas into the process chamber and load the radio frequency power, so that the first process gas reacts with the surface atomic layer of the GaN cap layer to form a transition layer;

[0091] The preferred process parameters used in this step include: upper RF power range: 50W~200W; Cl2 flow range: 20sccm~200sccm; gas introduction time range: 0.5s~20s; chamber pressure range: 3mt~10mt; back He pressure range: 4T~8T; process temperature range: -20℃~40℃.

[0092] Specifically, after the above step S501 is completed, the conditions of step S501 are maintained, and the RF power is loaded, the power setting range is 50W to 200W, the ventilation time is controlled at 0.5s to 20s, the back he cooling pressure is 4 to 8T, and the chiller temperature is -20 to 40°C, so as to achieve the chlorination of the GaN surface atomic layer and reduce the surface energy. The loading of the RF power is mainly to adsorb the Cl2 molecules on the GaN surface and chlorinate the GaN atomic layer to form GaCl x For the transition layer, the upper RF power is selected to be 50W-200W for the depth requirement of chlorination treatment, and high power will affect this depth; the Cl2 gas flow rate is selected to be 20-200sccm and the chamber pressure is selected to be 3-10mt, which is required for RF ignition and to prepare for the next step of treatment; the ventilation time is selected to be 0.5-20s, which is required for chlorination treatment and is related to the surface state of the sample to ensure that the sample surface can be completely chlorinated; the back He pressure is selected to be 4T-8T and the Chiller temperature is selected to be -20-40℃ in order to cool the wafer to prevent the occurrence of glue sticking.

[0093] S303 - first purge step: introducing a purge gas into the process chamber to remove the residual first process gas and by-products in the process chamber;

[0094] Specifically, after the above step S302 is completed, this step switches the process gas system and switches the gas to a purge gas to remove residual Cl 2 and by-products in the chamber. The purge gas is an inert gas, and Ar is preferably used in this embodiment.

[0095] The process parameters of this step include: Ar flow range is 100~1000sccm, preferably the chamber is pumped at the maximum pumping speed (swing valve opening PV1000); ventilation time range is 0.5s~5s, back He cooling pressure range is 4~8T, chiller temperature range is -20~40℃; the chamber is purged by large air volume to purge the excess etching gas molecules in the chamber.

[0096] Among them, the Ar gas flow rate is selected to be 100~1000sccm, which is mainly used to purge excess Cl2 molecules in the chamber and prepare for the next etching step; the ventilation time is selected to be 0.5~5s, which is used to purge the residual gas in the chamber to ensure that the Cl2 in the chamber can be completely purged to prevent the subsequent etching steps from being affected; the back He cooling pressure is selected to be 4~8T, and the chiller temperature is selected to be -20~40℃ to cool the wafer and prevent the occurrence of glue sticking.

[0097] S304-atomic layer etching step: introducing a second process gas into the process chamber, and sequentially loading upper RF power and lower RF power to remove the transition layer;

[0098] Optionally, the second process gas includes at least one of Ar, N2, O2, Kr, Xe, and Ne. In this embodiment, the second process gas is Ar (in order to improve process efficiency and reduce the switching of process gases, the purge gas used in step S503 and step S505 in this embodiment is the same as the second process gas used in step S504). In other embodiments, the second process gas may also be replaced by other inert gases such as Ar, N2, O2, Kr, Xe, and Ne.

[0099] The process parameters used in this step include: Ar flow range: 20sccm~200sccm; chamber pressure range: 3mt~10mt; upper RF power range: 50W~200W; lower RF power range: 3W~15W; time range for introducing the second process gas: 0.5s~20s; back He pressure range: 4T~8T; process temperature range: -20℃~40℃.

[0100] Specifically, after the completion of the above step S303, bombarding gas Ar is continuously introduced, the flow rate is set to 20 to 200 sccm, the chamber maintains a certain chamber pressure, the pressure range is selected to be a fixed value between 3mt and 10mt, the upper RF power is loaded first, the power range is set to 50 to 200W, and then the lower RF power is loaded, the power range is set to 3 to 15W, the ventilation time is controlled at 0.5s to 20s, the back he cooling pressure is 4 to 8T, and the chiller temperature is -20 to 40°C, so that the GaN surface chloride layer (transition layer) can be etched away.

[0101] The upper RF power is selected from 50W to 200W, and the lower RF power is selected from 3 to 15W, mainly to control the GaCl xThe lower RF power is loaded to accelerate the plasma downward and increase the downward etching rate. For example, the lower RF power can be selected to be 3-15W, mainly to prevent the GaN cap layer interface from being etched through and reaching the AlGaN interface, causing significant damage to the AlGaN surface; the Ar gas flow rate is selected to be 20-200sccm, which is the best for etching GaCl x The transition layer is required; the chamber pressure is selected to be 3-10mt, the ventilation time is selected to be 0.5-20s, which is the etching angle and GaCl x The transition layer is required to ensure that GaN surface GaCl x The layer can be completely etched to achieve atomic layer etching; the selection of back He pressure and Chiller temperature is to cool the wafer to prevent the occurrence of glue sticking.

[0102] S305 - second purge step: introducing purge gas into the process chamber to remove residual etching byproducts in the process chamber;

[0103] The purge gas used in this step is preferably Ar (inert gas may also be used), and the process parameters include: purge time range is 0.5s to 5s, purge gas Ar flow range is 100 to 1000sccm, the chamber is purged at the maximum pumping speed, the back He cooling pressure range is 4 to 8T, and the chiller temperature range is -20 to 40°C to purge chamber by-products.

[0104] Among them, the Ar gas flow rate is selected to be 100~1000sccm, which is mainly used to purge by-products in the chamber to prepare for the next step of processing; the ventilation time is selected to be 0.5~5s, which is used to ensure that the by-products in the chamber are cleanly purged to prevent the impact on the subsequent etching steps; the back He pressure is: 4~8T, which is used to enhance the shedding of by-products on the chip surface and reduce the accumulation of by-products; the chiller temperature is selected to be -20~40℃ to prepare for the next step of processing.

[0105] The gas adsorption step S301 to the second purge step S305 are cyclically executed to a set number of times until the AlGaN layer is etched.

[0106] Specifically, the above S301-S305 is one cycle, and the specific implementation process can select multiple cycles to cooperate with each other according to the requirements of the etching depth. Preferably, the number of times is set to 5 to 30 times, and the CD size of the p-GaN gate formed by etching is less than 1um.

[0107] The cross-sectional photos of the etching in each step of the method of this embodiment are as follows Figure 8 As shown, it can be seen that there is no side erosion on the side wall of TiN in the final etching morphology.

[0108] In summary, the etching method of this embodiment switches the process recipe to the atomic layer etching (ALE) mode of 5-step cyclic etching in step S3, including: (1) introducing etching gas to be adsorbed on the wafer surface; (2) etching gas forms a transition layer on the surface; (3) purging excess gas and free radicals in the chamber; (4) introducing bombarding gas and loading RF power to bombard the transition layer on the sample surface; (5) the chamber is purged to clean the byproducts on the wafer surface in preparation for the next step of etching gas adsorption; and this cycle step is performed to supplement the thickness of the subsequent film layer. Because in the process of supplementary etching of the GaN cap layer, in order to meet the requirements of electrical results, the etching depth needs to reach the AlGaN interface and the AlGaN etching depth cannot be penetrated (that is, p-GaN is required to have a higher selectivity to AlGaN); secondly, in order to improve the overall product yield level, a certain amount of over-etching needs to be increased in the supplementary etching process (step S3).

[0109] Compared with the traditional etching scheme of prior art 1, the etching method of the present invention switches the traditional etching step to an ALE etching mode with a 5-step cycle in the supplementary etching step; using the atomic layer stripping etching scheme of the ALE mode, firstly, an etching gas is introduced to be adsorbed on the wafer surface; then, by starting the upper RF power, the etching gas forms a transition layer on the surface of each film layer of the wafer; then, by purging the excess gas and free radicals in the chamber, the etching of each film layer in the subsequent steps is reduced; then, a bombarding gas is introduced and the lower RF power is loaded to bombard the transition layer on the surface of the sample to remove the atoms in the surface transition layer; then, the chamber is purged and the by-products bombarded on the wafer surface are cleaned to reach a new interface, and preparation is made for the next step of etching gas adsorption; finally, the above 5 steps are recycled to achieve etching at the interface between the p-GaN cap layer and the AlGaN without affecting the TiN morphology. When the plasma reaches the AlGaN etching interface, although the ALE mode of the 5-step cyclic etching in this process also applies bias bombardment power and bombardment gas during the etching process, the side walls of the TiN layer and the GaN cap layer are partially protected by the top mask layer and the photoresist layer, which can reduce the lateral etching of the TiN layer and the GaN cap layer by the plasma to a certain extent. At the same time, in the ALE cyclic etching process, due to the addition of a cyclic purge process of the plasma (i.e., the first purge step and the second purge step), the plasma concentration in the process chamber can be reduced to a great extent and the scattering of the plasma on the wafer surface can be reduced, which effectively avoids the problem of significantly enhanced lateral chemical etching due to the concentration increase of the plasma in the chamber and scattering on the wafer surface in the traditional etching process, thereby reducing the lateral etching of TiN and p-GaN, and thus avoiding or greatly reducing the occurrence of lateral side etching of the TiN side wall.

[0110] Example 2

[0111] Fig. 9 Shown is a schematic structural diagram of a semiconductor process equipment according to an embodiment of the present application.

[0112] like Fig. 9 As shown, the semiconductor process equipment 200 includes a process chamber 20, an inlet assembly 20A, an upper electrode assembly 20B and a lower electrode assembly 20C and a controller ( Fig. 9 The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method for etching the semiconductor film layer of any one of the above embodiments is implemented.

[0113] Exemplarily, the controller can be a host computer or a slave computer. The controller can control the valve of the gas inlet component 20A to open so as to introduce the corresponding process gas into the process chamber 20; the controller can also control the opening and closing degree of the valve of the gas inlet component 20A to control the flow rate of the process gas. The controller can also control the exhaust component to exhaust the inside of the process chamber 20 to control the pressure inside the process chamber 20, discharge reaction byproducts, etc.

[0114] The upper electrode assembly 20B includes an RF coil 21, an upper RF power supply 23 and an upper matcher 25. The controller is also used to control the upper RF power supply 23 to provide upper electrode power to the RF coil 21 through the upper matcher 25, so that the RF coil 21 excites the process gas inside the process chamber 20 to generate plasma.

[0115] The lower electrode assembly 20C includes a wafer carrier 22, a lower RF power supply 24, and a lower matcher 26. The controller is also used to control the lower RF power supply 24 to provide lower electrode power to the lower electrode of the wafer carrier 22 through the lower matcher 26, so that the lower electrode of the wafer carrier 22 provides RF bias to absorb the plasma above the object to be etched 100 to bombard the object to be etched 100.

[0116] The semiconductor process equipment 200 of the embodiment of the present application may be an inductively coupled plasma (ICP) etching equipment or a capacitively coupled plasma (CCP) etching equipment. The embodiment of the present application does not limit the type of the semiconductor process equipment 200.

[0117] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for etching a semiconductor film layer, wherein the semiconductor film layer structure comprises an AlGaN layer, a GaN cap layer and an electrode contact layer stacked in sequence from bottom to top; characterized in that: The etching method comprises: Etching the electrode contact layer in a preset area until the GaN cap layer is exposed to form an electrode contact layer pattern; Etching the exposed GaN cap layer to a set depth; The remaining GaN cap layer is continuously etched using an atomic layer etching process until the AlGaN layer is etched.

2. The method for etching a semiconductor film layer according to claim 1, characterized in that: The atomic layer etching process comprises: Gas adsorption step: introducing a first process gas into the process chamber so that the first process gas is adsorbed on the surface of the GaN cap layer; Atomic layer reaction step: continue to introduce the first process gas into the process chamber and load RF power, so that the first process gas reacts with the surface atomic layer of the GaN cap layer to form a transition layer; Atomic layer etching step: introducing a second process gas into the process chamber, and sequentially loading upper RF power and lower RF power to remove the transition layer; The gas adsorption step-the atomic layer etching step is cyclically executed for a set number of times until the AlGaN layer is etched.

3. The method for etching a semiconductor film layer according to claim 2, characterized in that: The atomic layer etching process also includes: After the atomic layer reaction step, a first purge step is performed: introducing a purge gas into the process chamber to remove the residual first process gas and byproducts in the process chamber; and / or A second purge step is performed after the atomic layer etching step: a purge gas is introduced into the process chamber to remove residual etching byproducts in the process chamber.

4. The method for etching a semiconductor film layer according to claim 2, characterized in that: The first process gas includes at least one of Cl2, BCl3, and HBr.

5. The method for etching a semiconductor film layer according to claim 2, characterized in that: The second process gas includes at least one of Ar, N2, O2, Kr, Xe, and Ne.

6. The method for etching a semiconductor film layer according to claim 3, characterized in that: The purge gas is the same as the second process gas.

7. The method for etching a semiconductor film layer according to claim 2, characterized in that: The first process gas includes Cl2, and the process parameters used in the gas adsorption step include: Cl2 flow rate range: 20sccm~200sccm; The chamber pressure range is: 3mt~10m.

8. The method for etching a semiconductor film layer according to claim 7, characterized in that: The process parameters used in the atomic layer reaction step include: The upper RF power range is: 50W~200W; Cl2 flow rate range: 20sccm~200sccm; The chamber pressure range is: 3mt~10mt.

9. The method for etching a semiconductor film layer according to claim 2, characterized in that: The second process gas includes Ar, and the process parameters used in the atomic layer etching step include: Ar flow range: 20sccm~200sccm; The chamber pressure range is 3mt to 10mt; The upper RF power range is 50W to 200W; The lower RF power range is 3W to 15W.

10. The method for etching a semiconductor film layer according to claim 3, characterized in that: The purge gas includes Ar, and the process parameters used in the first purge step and the second purge step include: The Ar flow rate range is: 100 sccm~1000 sccm.

11. The method for etching a semiconductor film layer according to any one of claims 7 to 10, characterized in that: The process parameters used in the atomic layer etching process also include: The process temperature range is: -20℃~40℃.

12. The method for etching a semiconductor film layer according to claim 1, characterized in that: The set depth is 1 / 2 to 2 / 3 of the thickness of the GaN cap layer.

13. A semiconductor process equipment, comprising a process chamber, an air inlet assembly, an upper electrode assembly, a lower electrode assembly and a controller, characterized in that: The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method for etching a semiconductor film layer according to any one of claims 1 to 12 is implemented.

Citation Information

Cited By

  • VCSEL epitaxial growth method

    CN121556134A

  • Dry etch process for the production of high electron mobility transistors

    GB2703379A

  • Method for fabricating a HEMT device in an atomic layer etching reactor and use of the method in fabrication of a gallium-nitride-based HEMT

    WO2026119915A1