Shell preparation method, shell and electronic equipment
By etching first and then hot pressing molding, the problem of uneven etching of the shell of the electronic device is solved, uniform etching of the shell and high-quality appearance effect are achieved, and the preparation needs of complex structural shells are met.
Patent Information
- Application Number
- CN202310594275.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the matte effect etching process of the shell of an electronic device is usually carried out after cutting and forming, resulting in uneven etching of the shell, affecting the appearance effect, and possibly damaging the strength of the shell.
The shell is formed by first etching the initial substrate and then hot-pressing it in the molding mold. The protective layer is formed on the surface of the etched substrate to protect the texture, and the protective layer is removed after hot-pressing. To maintain matte finish.
The uniformity and appearance effect of shell etching are improved, and the problem of uneven etching is avoided. At the same time, the strength and matte effect of the shell are maintained, meeting the preparation needs of complex structural shells.
Smart Images

Figure CN119031623A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of shell manufacturing, and in particular to a shell preparation method, a shell and an electronic device. Background Art
[0002] As users pursue the appearance and texture of electronic devices, more and more electronic devices use matte effect shell materials for their shells. In recent years, the demand for matte effect shells has increased. Matte effect shells do not have strong reflections of highlights, and fingerprint residues are not obvious. In related technologies, the etching process to form a matte effect is usually performed after cutting, forming and polishing. The formed shell is usually a non-planar structure. Performing a matte effect etching process on the formed shell will cause uneven etching of the shell. For example, the etching effect at the edge of the shell will be different from the etching effect in the middle, resulting in an unsatisfactory appearance of the final shell. Summary of the invention
[0003] In order to solve the problems existing in the related art, the present disclosure provides a method for preparing a shell, a shell and an electronic device.
[0004] According to a first aspect of an exemplary embodiment of the present disclosure, a method for preparing a housing is provided, the method comprising:
[0005] Etching the first surface of the initial substrate to obtain an etched substrate;
[0006] The etched substrate is hot-pressed in a molding die to form the shell, wherein the first surface is the outer surface of the shell.
[0007] In some exemplary embodiments, when the etching depth of the first surface is greater than a preset threshold, the preparation method further includes:
[0008] A first protective layer is formed on the first surface of the etched substrate.
[0009] In some exemplary embodiments, the thickness of the first protection layer is greater than or equal to an etching depth of the first surface etching process.
[0010] In some exemplary embodiments, the preset threshold is in the range of 20 microns to 50 microns.
[0011] In some exemplary embodiments, after the step of hot pressing the etched substrate in a forming mold, the preparation method further comprises:
[0012] The first protective layer is removed.
[0013] In some exemplary embodiments, before the step of etching the first surface of the initial substrate to obtain an etched substrate, the preparation method further comprises:
[0014] A second protective layer is formed on the second surface of the initial substrate to protect the second surface during the etching process.
[0015] In some exemplary embodiments, after the step of hot pressing the etched substrate in a forming mold, the preparation method further comprises:
[0016] removing the second protective layer;
[0017] The second surface is polished with a first preset polishing solution.
[0018] In some exemplary embodiments, etching the first surface of the initial substrate to obtain an etched substrate includes:
[0019] The first surface of the initial substrate is sprayed or immersed with a preset etching solution for a first preset time to obtain the etched substrate.
[0020] In some exemplary embodiments, the predetermined etching solution is an acid solution with a pH value of 1-2 or an alkaline solution with a pH value of 10-14.
[0021] In some exemplary embodiments, the preparation method further comprises:
[0022] Processing the initial substrate or the etched substrate into a substrate of a preset shape;
[0023] The processed part of the substrate with the preset shape is polished with a second polishing solution.
[0024] In some exemplary embodiments, the step of hot pressing the etched substrate in a forming mold comprises:
[0025] Heating the etched substrate in the molding die to a preset temperature according to a first preset rule, so that the etched substrate is in a first state;
[0026] According to the second preset rule, the substrate in the first state is hot pressed to form a shape.
[0027] In some exemplary embodiments, heating the etched substrate to a preset temperature in the molding die according to a first preset rule comprises:
[0028] heating the etched substrate to the preset temperature in the molding die in a linear temperature increasing manner; or
[0029] The etched substrate is heated to the preset temperature in the molding die in a step-by-step heating manner.
[0030] In some exemplary embodiments, the step of hot pressing the substrate in the first state to form the substrate according to the second preset rule includes:
[0031] According to a preset time interval, hot-pressing the substrate in the first state for a preset number of times to shape the substrate in the first state; or
[0032] According to the preset time interval difference, the substrate in the first state is hot-pressed for a preset number of times to shape the substrate in the first state.
[0033] In some exemplary embodiments, the substrate includes a glass substrate or a ceramic substrate.
[0034] In some exemplary embodiments, after the step of hot-pressing the etched substrate in a molding die to form the housing, the preparation method further comprises:
[0035] The shell is immersed in the molten strengthening liquid for a second preset time so that the lithium ions in the shell are exchanged with the potassium ions or sodium ions in the molten strengthening liquid, and the sodium ions in the shell are exchanged with the potassium ions in the molten strengthening liquid to strengthen the shell.
[0036] In some exemplary embodiments, the molten strengthening solution includes a molten solution of potassium nitrate and sodium nitrate configured in a preset ratio.
[0037] According to a second aspect of an exemplary embodiment of the present disclosure, a shell is provided. The shell is manufactured according to the above-mentioned method for manufacturing the shell.
[0038] According to a third aspect of an exemplary embodiment of the present disclosure, an electronic device is provided. The electronic device includes the above-mentioned housing.
[0039] The beneficial effects of the present disclosure include but are not limited to: the shell preparation method provided by the present disclosure, which is a preparation process of first etching the substrate and then hot pressing to form the shell, so that the preparation method can meet the needs of preparing complex structure shells and avoid the problems of uneven etching and poor appearance caused by hot pressing and then etching the substrate.
[0040] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings incorporated into the specification and constituting a part of the specification illustrate embodiments of the present disclosure and are used together with the description to explain the principles of the embodiments of the present disclosure. In these drawings, similar reference numerals are used to represent similar elements. The drawings described below are some embodiments of the present disclosure, rather than all embodiments. For those skilled in the art, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 It is a schematic diagram of the preparation process of a shell in the related technology of an exemplary embodiment of the present disclosure;
[0043] Figure 2 It is a schematic diagram of a method for preparing a shell according to an exemplary embodiment of the present disclosure;
[0044] Figure 3 It is a schematic diagram of the preparation process of a shell according to an exemplary embodiment of the present disclosure;
[0045] Figure 4 is a schematic longitudinal cross-sectional view of a substrate according to an exemplary embodiment of the present disclosure;
[0046] Figure 5 It is a schematic diagram of a process after the step of hot pressing the etched substrate in a forming mold according to an exemplary embodiment of the present disclosure;
[0047] Figure 6 A method for preparing a housing according to an exemplary embodiment of the present disclosure further includes a flow chart;
[0048] Figure 7 It is a schematic diagram of a process of hot pressing an etched substrate in a forming mold according to an exemplary embodiment of the present disclosure;
[0049] Figure 8 The figure is a schematic diagram of a process of preparing a battery cover of a mobile terminal according to an exemplary embodiment of the present disclosure. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solutions and advantages of the embodiments of the present disclosure clearer, the technical solutions of the present disclosure will be clearly and completely described below in combination with the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure. It should be noted that the embodiments in the present disclosure and the features in the embodiments can be arbitrarily combined with each other without conflict.
[0051] As users pursue the appearance and texture of electronic devices, more and more electronic devices use matte effect shell materials for their shells. In recent years, the demand for matte effect shells has increased. Matte effect shells do not have strong reflections of highlights, and fingerprint residues are not obvious. In related technologies, the etching process to form a matte effect is usually performed after cutting, forming and polishing. The formed shell is usually a non-planar structure. Performing a matte effect etching process on the formed shell will cause uneven etching of the shell. For example, the etching effect at the edge of the shell will be different from the etching effect in the middle, resulting in an unsatisfactory appearance of the final shell.
[0052] like Figure 1 The preparation process of the shell shown in the figure is to first cut the initial substrate to obtain the substrate 10', then perform hot pressing on the substrate 10' to obtain the hot pressed substrate 20', and then perform etching on the hot pressed substrate 20' to obtain the etched shell 30'. This preparation process of first hot pressing and then etching will result in uneven etching at the edges of the substrate and the hot pressed bends, ultimately resulting in poor appearance and damaging the strength of the shell.
[0053] Based on this, the exemplary embodiment of the present disclosure provides a method for preparing a shell. The method for preparing a shell provided by the present disclosure can be applied to any field requiring shell manufacturing, such as the manufacturing of a battery cover of an electronic device. Figure 2 As shown, the preparation method of the shell provided by the present disclosure includes:
[0054] S100: etching the first surface of the initial substrate to obtain an etched substrate.
[0055] In this step, an etching process is performed on the first surface of the initial substrate so that the first surface of the substrate presents a desired matte effect or texture effect, thereby obtaining an etched substrate.
[0056] In an exemplary embodiment of the present disclosure, the first surface of the initial substrate can be etched with a preset etching solution so that the initial substrate presents a desired matte effect or texture effect after etching. For example, a strong acid solution or a strong alkali solution can be used as the preset etching solution to chemically etch the first surface of the initial substrate in preparation for subsequent shell preparation.
[0057] S200: hot-pressing the etched substrate in a molding die to form a shell, wherein the first surface is an outer surface of the shell.
[0058] In this step, the etched substrate is placed in a mold made of graphite or metal material with a desired shape, and the etched substrate is heated and pressure is applied to form the etched substrate into a shape that matches the mold to obtain the desired shell, wherein the first surface presenting a matte effect or a textured effect is the outer surface of the shell.
[0059] In the preparation method of the shell provided in the exemplary embodiment of the present disclosure, the preparation process of the shell is formed by first etching the initial substrate and then hot pressing it, so that the preparation method can meet the needs of preparing shells with complex structures and avoid the problems of uneven etching and poor appearance caused by first hot pressing the substrate and then etching it.
[0060] The preparation process of the shell provided in the exemplary embodiment of the present disclosure is as follows: Figure 3 As shown, the initial substrate 10 is first etched to obtain an etched substrate 20, and the etched substrate 20 is hot-pressed to obtain a molded shell 30. Figure 1 Compared with the preparation process of the shell in the related art shown in FIG. Figure 3 The preparation process of etching first and then hot pressing is provided in the exemplary embodiment of the present disclosure. The initial substrate is first etched to have a texture effect or a matte effect, and then hot pressing is performed, thereby avoiding the problem of uneven shell etching caused by forming first and then etching, and at the same time will not affect the strength of the shell.
[0061] In the exemplary embodiments provided in the present disclosure, Figure 4 The schematic diagram of the longitudinal section of the substrate shown, when the etching depth h of the first surface is greater than the preset threshold value, the preparation method also includes: forming a first protective layer on the first surface of the etched substrate. Wherein, the thickness of the first protective layer is d. When the etching depth h of the first surface of the etched substrate is greater than the preset threshold value, when the etched substrate is placed in the molding mold for hot pressing, the texture etched on the first surface of the etched substrate will be damaged, and the service life of the molding mold will also be affected. For example, when the etching depth h of the first surface of the etched substrate is too large, after the etched substrate is softened by heat in the molding mold, when pressure is applied to the heat-softened substrate for hot pressing, the etching texture of the heat-softened first surface of the substrate will be affected by the pressure during the hot pressing process, thereby affecting the final appearance of the first surface of the prepared shell; at the same time, because the texture of the first surface of the substrate has an excessively large etching depth, it will also generate a large reverse pressure on the surface of the inner cavity of the molding mold that is bonded to it, causing damage to the surface of the inner cavity of the molding mold, affecting the life of the molding mold.
[0062] Therefore, when the etching depth h of the first surface is greater than a preset threshold, a first protective layer needs to be formed on the first surface of the substrate, so that the texture on the first surface produced by the etching treatment can be protected during the hot pressing process of the substrate to ensure the final appearance of the first surface of the prepared shell while reducing damage to the molding mold.
[0063] It should be noted that the step of forming a protective layer on the first surface can be performed at any time point between the end of the etching process and before the hot pressing forming.
[0064] In the exemplary embodiment provided by the present disclosure, the thickness d of the first protective layer is greater than or equal to the etching depth h of the first surface etching treatment. The thickness d of the first protective layer is greater than or equal to the etching depth h of the first surface etching treatment to ensure that the first protective layer covers all positions of the texture on the first surface, so as to protect the texture on the first surface of the substrate generated by the etching treatment during the hot pressing process of the substrate, while reducing damage to the molding mold. Figure 4 In the exemplary embodiment shown, the thickness d of the first protective layer is greater than the etching depth h. The thickness d of the first protective layer may also be equal to the etching depth h, that is, the surface of the first protective layer is flush with the first surface of the substrate.
[0065] In the exemplary embodiments provided in the present disclosure, the first protective layer may include a layer of a high temperature resistant material. The high temperature resistant material may be any material that does not soften and deform during the hot pressing process to protect the texture produced by the etching process on the first surface of the substrate, such as ink. The ink is a viscous colloidal fluid that can be coated on the first surface of the substrate and then dried, fixed and formed into a film to form a first protective layer on the first surface to protect the texture produced by the etching process on the first surface of the substrate during the hot pressing process of the substrate.
[0066] In the exemplary embodiment provided by the present disclosure, the preset threshold value is taken in the range of 20 microns to 50 microns. When the preset threshold value is taken in the range of 20 microns to 50 microns, and the etching depth of the first surface is greater than the preset threshold value, when the etched substrate is placed in the molding die for hot pressing, the etching texture on the first surface of the substrate will be damaged, thereby affecting the final appearance of the first surface of the prepared shell; at the same time, because the texture of the first surface of the substrate has an excessively large etching depth, it will also produce a large reverse pressure on the surface of the inner cavity of the molding die that is bonded thereto, causing damage to the inner cavity surface of the molding die, affecting the life of the molding die. Therefore, the preset threshold value is set to 20 microns to 50 microns. When the etching depth h of the first surface is greater than the preset threshold value, a first protective layer is formed on the first surface of the etched substrate, so that the texture generated by the etching process on the first surface can be protected during the hot pressing process of the substrate to ensure the final appearance of the first surface of the prepared shell, while reducing damage to the molding die.
[0067] In an exemplary embodiment provided by the present disclosure, after the etched substrate is hot-pressed in a molding die, the preparation method further includes removing the first protective layer.
[0068] The first protective layer is formed on the first surface of the substrate to protect the texture on the first surface produced by etching during the hot pressing process of the substrate, so as to ensure the final appearance of the first surface of the prepared shell and reduce damage to the forming mold. After the etched substrate is hot pressed in the forming mold, the first protective layer can be removed, for example, by washing or soaking the first protective layer in an alkaline solution, so that the first surface of the shell after hot pressing, that is, the outer surface, presents the texture formed by etching, that is, the first surface of the prepared shell presents a matte effect. When the shell is applied to the manufacture of electronic equipment, the matte appearance requirements of electronic equipment products can be met.
[0069] In an exemplary embodiment provided in the present disclosure, before the step of etching the first surface of the initial substrate to obtain an etched substrate, the preparation method further includes: forming a second protective layer on the second surface of the initial substrate to protect the second surface during the etching process.
[0070] If the shell does not need to present a matte effect on the second surface, before etching the first surface of the initial substrate with a preset etching solution to obtain the etched substrate, a second protective layer needs to be formed on the second surface of the initial substrate to protect the second surface and prevent the second surface from being etched during the etching process of the first surface of the initial substrate with the preset etching solution. The second surface may be a surface opposite to the first surface.
[0071] In the exemplary embodiments provided in the present disclosure, the second protective layer may include a corrosion-resistant material layer. The corrosion-resistant material may be any material that is not etched by the preset etching solution during the etching process to protect the second surface of the substrate, such as ink. The ink is coated on the second surface of the initial substrate, and the ink dries, fixes and forms a film on the second surface of the substrate to form a second protective layer on the second surface, which can protect the second surface during the etching process to prevent the preset etching solution from etching the first surface of the initial substrate.
[0072] The types and components of the inks used for the first protective layer and the second protective layer may be the same or different, and may be selected according to the actual production needs of the shell, and the present disclosure does not limit this.
[0073] In the exemplary embodiment provided by the present disclosure, after the step of hot pressing the etched substrate in the forming mold, as Figure 5The method also includes:
[0074] S301: removing the second protective layer.
[0075] The second protective layer is formed on the second surface of the initial substrate before the first surface of the initial substrate is etched to protect the second surface during the etching process. When the material contained in the second protective layer is ink, due to the viscosity of the ink, when it is coated on the second surface, the brittleness of the substrate can be reduced. During the hot pressing process, the substrate can be protected to a certain extent, reducing the scrap rate in the shell preparation process. After the etched substrate is hot-pressed in the molding mold, the second protective layer can be removed, for example, by washing or soaking the second protective layer in an alkaline solution.
[0076] S302: polishing the second surface with a first preset polishing solution.
[0077] After removing the second protective layer on the second surface, the first preset polishing liquid is used with a brush-like tool to polish the second surface for 60 minutes to 120 minutes, for example, 60 minutes, 80 minutes, 100 minutes, or 120 minutes. The first preset polishing liquid is prepared by dissolving cerium oxide or zirconium oxide powder, that is, polishing powder in water, and the concentration of the polishing liquid is 20 to 50%, for example, 20%, 30%, 40%, or 50%; the brush-like tool is made of materials such as bristles or polyurethane. After the first preset polishing liquid is used with a brush-like tool to polish the second surface, the indentations on the second surface can be removed, and the second surface can be further smoothed. At the same time, the second protective layer remaining on the second surface can be removed cleanly, so that the second surface meets the appearance or functional requirements.
[0078] In the exemplary embodiment of the present disclosure, the first surface of the initial substrate is first etched to produce a matte effect. The second surface is a surface opposite to the first surface. The matte effect of the first surface of the initial substrate has a certain covering effect on the second surface. Therefore, the first surface of the initial substrate is first etched and then hot-pressed. It is not necessary to polish the first surface, and only other surfaces, such as the second surface, need to be polished. This can reduce the polishing time of the substrate, save the time of the polishing process, and reduce the production cost.
[0079] In an exemplary embodiment provided by the present disclosure, etching is performed on a first surface of an initial substrate to obtain an etched substrate, comprising:
[0080] The first surface of the initial substrate is sprayed or immersed with a preset etching solution for a first preset time to obtain an etched substrate.
[0081] The preset etching solution should be a solution that can chemically corrode the first surface of the initial substrate. The first surface of the initial substrate is etched for a first preset time by spraying or immersing the preset etching solution, so that a substrate with a matte effect after etching can be obtained. The first preset time can be specifically selected according to the etching difficulty of the substrate and the desired texture effect, such as etching depth. For example, the first preset time can be 20 seconds to 5 minutes.
[0082] In an exemplary embodiment provided by the present disclosure, the preset etching solution is an acid solution with a pH value of 1 to 2 or an alkaline solution with a pH value of 10 to 14.
[0083] In the exemplary embodiment of the present disclosure, an acid solution with a pH value of 1 to 2 or an alkaline solution with a pH value of 10 to 14 is selected to chemically corrode the first surface of the initial substrate, for example, a hydrofluoric acid solution with a pH value of 1 to 2 or a sodium hydroxide solution with a pH value of 10 to 14 is selected. The first surface of the initial substrate is etched for a first preset time by spraying or immersing the acid solution with a pH value of 1 to 2 or the alkaline solution with a pH value of 10 to 14, and a substrate with a matte effect after etching can be obtained. Among them, the concentration of the preset etching solution can be specifically selected according to the etching difficulty of the substrate and the desired texture effect, such as the etching depth. This etching method is simple to operate, and the preset etching solution used is easy to obtain, and can be applied in large-scale mass production.
[0084] In the exemplary embodiments provided in the present disclosure, the preparation method, such as Figure 6 As shown, it also includes:
[0085] S101: Processing an initial substrate or an etched substrate into a substrate of a preset shape.
[0086] In step S101, the large piece of initial substrate can be etched first to obtain a large piece of etched substrate, and the large piece of etched substrate can be divided into small pieces of substrates of preset size according to the preset size. For example, when the prepared shell is applied to the battery cover of an electronic device, it can be divided into rectangles or squares. During the division, a diamond knife is used to cut the large piece of etched substrate according to the preset size. The cutting operation is stopped when the cutting depth is 1 / 3 to 1 / 2 of the thickness of the large piece of etched substrate. The large piece of etched substrate is broken into small pieces of substrates of preset size by hand or machine. This division method can prevent the diamond knife from crushing the large piece of etched substrate or damaging the cutting edge when the large piece of etched substrate is thoroughly cut, thereby reducing the scrap rate in the shell preparation process.
[0087] Through the CNC (Computerized Numerical Control) process, a substrate of a preset size is processed with a cutting wheel rod coated with diamond sand on the surface, so that the substrate of the preset size has a preset shape that meets the subsequent application requirements of the shell. For example, when the prepared shell is applied to the battery cover of an electronic device, the preset shape of the substrate should correspond to the outer contour of the battery cover and have characteristic structures such as a camera module hole.
[0088] In order to improve the yield rate, the processing process is divided into two steps: rough milling and fine milling. The rough milling cutter number is 600~800#, and the rough milling cuts to the substrate shape with a remaining reserve of 0.10mm~0.15mm; the fine milling cutter number is 1000~1200#, and the fine milling is divided into 1~2 cuts, the first cut processes 0.06mm~0.10mm, and the second cut processes 0.04mm~0.05mm. This rough milling and then fine milling processing method first uses rough milling to process the substrate of the preset size into a rough outline and shape, and then fine milling is used to finely process the substrate after rough milling, so that the substrate's shape and contour can better meet the subsequent application requirements of the shell.
[0089] In step S101, the large initial substrate may be directly cut into preset sizes as described above, processed into preset shapes, and then the substrate in the preset shape may be etched.
[0090] S102: polishing the processed part of the substrate with a preset shape with a second polishing solution.
[0091] After the processing is completed, the substrate with a preset shape is polished with a second preset polishing liquid and a brush-like tool to polish the processed part of the substrate for 20 minutes to 35 minutes, for example, it can be 20 minutes, 25 minutes, 30 minutes, 35 minutes. Among them, the second preset polishing liquid is prepared by dissolving cerium oxide or zirconium oxide powder, that is, polishing powder in water, and the concentration of the polishing liquid is 20% to 50%, for example, 20%, 30%, 40%, 50%; the brush-like tool is made of materials such as bristles, plastic wires or polyurethane. After the second preset polishing liquid is used with a brush-like tool to polish the processed part of the substrate with a preset shape, such as the outer shape or circumference of the substrate, the microcracks generated by the CNC processing process can be removed, and the processed part of the substrate can be smoothed, so that the outer contour of the substrate can better meet the subsequent application requirements of the shell.
[0092] If a large initial substrate is directly cut into preset sizes and processed into a preset shape, and then the substrate of the preset shape is etched, the processed portion of the substrate of the preset shape can be polished with a second polishing solution after the etching of the substrate of the preset shape.
[0093] In the exemplary embodiment provided by the present disclosure, the etched substrate is hot-pressed in a molding die, such as Figure 7 Shown include:
[0094] S201: heating the etched substrate to a preset temperature in a molding die according to a first preset rule, so that the etched substrate is in a first state.
[0095] In this step, after the etched substrate is placed in the forming mold, the etched substrate is heated to a preset temperature according to a first preset rule, so that the etched substrate is softened to a first state, so as to wait for the subsequent hot pressing of the softened substrate to form the required shell. The first state includes a state in which the etched substrate can be hot pressed after being softened at a preset temperature. If the substrate is directly pressed and molded, it will cause the substrate to break and increase the scrap rate in the shell preparation process. Therefore, after the substrate is heated to soften, hot pressing is performed to obtain a shell that matches the shape of the forming mold.
[0096] In the exemplary embodiment provided by the present disclosure, the etched substrate is heated to a preset temperature in the molding die according to a first preset rule, including: heating the etched substrate to a preset temperature in a linear heating manner in the molding die; or heating the etched substrate to a preset temperature in a stepwise heating manner in the molding die. The preset temperature is 50°C to 100°C above the softening point of the substrate.
[0097] In an exemplary embodiment of the present disclosure, the forming mold is heated to a preset temperature in accordance with a first preset rule, thereby avoiding directly heating the forming mold to a preset temperature to ensure the basic performance of the substrate after etching. The first preset rule may be any heating rule that ensures the basic performance of the substrate after etching. For example, the heating method of the first preset rule may be a gentle heating method, so that the substrate can better adapt to temperature changes, prevent the substrate from breaking due to severe heating, and reduce the scrap rate in the shell preparation process.
[0098] For example, after the etched substrate is placed in the molding mold, the etched substrate is uniformly heated to a preset temperature in the molding mold in a linear heating manner; or, after the etched substrate is placed in the molding mold, the etched substrate is heated to a preset temperature in a step-by-step heating manner, that is, after the substrate is heated to a certain temperature node, the temperature is kept constant at the temperature node for a certain time, and then the temperature is continued to be raised, and after the temperature is raised to the next temperature node, the temperature is kept constant at this temperature node for a certain time, and the heating is performed 6 to 10 times until the temperature reaches the preset temperature.
[0099] S202: According to a second preset rule, hot pressing the substrate in the first state to form a shape.
[0100] The base material softened to the first state after heating is pressurized according to the second preset rule, and the base material softened to the first state is shaped to obtain a shell that matches the shape of the molding mold.
[0101] In an exemplary embodiment provided by the present disclosure, according to a second preset rule, hot pressing a substrate in a first state to form a shape includes: hot pressing the substrate in the first state a preset number of times according to a preset time interval to form the substrate in the first state; or hot pressing the substrate in the first state a preset number of times according to a preset time interval difference to form the substrate in the first state.
[0102] The etched substrate is heated to a preset temperature in a molding die, and after softening to the first state, the substrate in the first state is hot pressed 2 to 4 times according to a preset time interval, the preset time interval ranges from 5 to 50 seconds, and the time for each pressurization is 3 to 10 seconds, so as to mold the substrate in the first state. For example, the time interval between the first pressurization and the second pressurization is 10 seconds, the time interval between the second pressurization and the third pressurization is 10 seconds, and the time interval between the third pressurization and the fourth pressurization is 10 seconds; or, the time interval between the first pressurization and the second pressurization is 10 seconds, the time interval between the second pressurization and the third pressurization is 20 seconds, and the time interval between the third pressurization and the fourth pressurization is 30 seconds; or, the time interval between the first pressurization and the second pressurization is 10 seconds, the time interval between the second pressurization and the third pressurization is 20 seconds, and the time interval between the third pressurization and the fourth pressurization is 40 seconds.
[0103] The etched substrate is heated to a preset temperature in a molding die, and after softening to the first state, the substrate in the first state is hot pressed 2 to 4 times according to a preset time interval difference, the preset time interval difference ranges from 0 to 30 seconds, and the time for each pressurization is 3 seconds to 10 seconds, so as to mold the substrate in the first state. For example, the time interval between the first pressurization and the second pressurization is 10 seconds, the time interval difference between the second pressurization and the third pressurization is 5 seconds, and the time interval difference between the third pressurization and the fourth pressurization is 10 seconds; or, the time interval between the first pressurization and the second pressurization is 10 seconds, the time interval difference between the second pressurization and the third pressurization is 5 seconds, and the time interval difference between the third pressurization and the fourth pressurization is 5 seconds.
[0104] The substrate in the first state is hot pressed at a molding frequency of 60s / sheet to 120s / sheet. The pressure during the hot pressing process can be selected according to the difficulty of hot pressing of the substrate and the matching temperature, which is not limited in the present disclosure.
[0105] In addition to hot pressing the substrate in the first state, hot pressing can also be started after the substrate reaches a softening point and before a preset temperature, and continued until the substrate reaches the preset temperature.
[0106] This method of hot pressing the substrate in the first state according to a preset time interval or a preset time interval difference can relatively gently hot press the substrate in the first state in steps to form it, avoiding the problem of the substrate breaking due to hot pressing the substrate under high pressure at one time, thereby reducing the scrap rate in the shell preparation process.
[0107] In the exemplary embodiments provided in the present disclosure, the substrate includes a glass substrate or a ceramic substrate. Both the glass substrate and the ceramic substrate have the characteristics of high hardness and scratch resistance. When used in the manufacture of the housing of an electronic device, the glass substrate or the ceramic substrate can provide a good appearance and feel after being etched.
[0108] In an exemplary embodiment provided by the present disclosure, after the step of hot-pressing the etched substrate in a molding die to form a shell, the preparation method further includes: immersing the shell in a molten strengthening liquid for a second preset time so that the lithium ions in the shell are exchanged with the potassium ions or sodium ions in the molten strengthening liquid, and the sodium ions in the shell are exchanged with the potassium ions in the molten strengthening liquid to strengthen the shell.
[0109] When the substrate is a glass substrate, the hot-pressed glass shell is immersed in the molten strengthening liquid for a second preset time, and the lithium ions with a smaller radius in the surface layer of the glass shell are exchanged with the potassium ions or sodium ions with a larger radius in the molten strengthening liquid, and the sodium ions with a smaller radius in the surface layer of the glass shell are exchanged with the potassium ions with a larger radius in the molten strengthening liquid, and an ion exchange layer is formed on the surface of the glass shell. After cooling to room temperature, the glass shell is in a state where the inner layer is tensile and the outer layer is compressed, thereby achieving the purpose of increasing the strength of the glass shell. The second preset time can be determined according to actual needs, for example, it can be 50 minutes to 200 minutes.
[0110] In the exemplary embodiment provided by the present disclosure, the melt strengthening liquid includes a melt of potassium nitrate and sodium nitrate configured in a preset ratio. When the substrate is a glass substrate, the hot-pressed glass shell is immersed in a melt of potassium nitrate and sodium nitrate, so that the ions with smaller radius in the surface layer of the glass shell are exchanged with the ions with larger radius in the melt, that is, the lithium ions on the surface layer of the glass shell are exchanged with the potassium ions or sodium ions in the melt, and the sodium ions on the surface layer of the glass shell are exchanged with the potassium ions in the melt, and the difference in the volume of the metal ions is used to form an extrusion stress on the surface layer of the glass shell, so as to achieve the purpose of strengthening the glass shell and improving the shell performance. The preset ratio can be set according to actual needs, for example, the mass ratio of potassium nitrate and sodium nitrate can be 0.5:1 to 3:1.
[0111] In the exemplary embodiments provided in the present disclosure, after the etched substrate is hot-pressed in a molding mold, the hot-pressed shell is also subjected to appearance processing. For example, when the shell is applied to a battery cover of an electronic device, the second surface (inner surface) of the shell is plated and sprayed, and the first surface (outer surface) of the shell is subjected to anti-fingerprint treatment to reduce fingerprints left on the outer surface during the use of the electronic device and improve the friction feel of the surface of the battery cover of the electronic device.
[0112] In the exemplary embodiment of the present disclosure, Figure 8 As shown, a specific example of applying the method for preparing a shell provided by an exemplary embodiment of the present disclosure to preparing a battery cover of a mobile terminal is provided.
[0113] S401: forming a protective layer on the second surface: selecting a glass substrate as an initial substrate, coating a second surface, i.e., an inner surface, of a large piece of the initial glass substrate with an ink protective layer, so as to protect the second surface, i.e., the inner surface, of the initial glass substrate during the subsequent chemical etching process of the first surface, i.e., the outer surface, of the initial glass substrate.
[0114] S402: Etching treatment: Using a hydrofluoric acid solution with a pH of 1 to 2 as a preset etching solution, chemically etch the first surface of a large glass initial substrate by spraying or immersing. The etching time is 20 seconds to 5 minutes, and a large piece of etched substrate is obtained for subsequent battery cover preparation.
[0115] S403: Cutting: According to the size of the mobile terminal, a diamond knife is used to cut the large piece of etched substrate. The cutting operation is stopped when the cutting depth of the etched substrate is 1 / 3 to 1 / 2 of the thickness. The etched substrate is broken into several rectangular substrates of approximately the size of the mobile terminal according to the cutting marks.
[0116] S404: Processing: Through CNC technology, with a cutter wheel bar coated with diamond sand on the surface, the rectangular substrate is processed. The processing process is divided into two steps: rough milling and fine milling. The rough milling cutter wheel number is 600-800#, and the rough milling cuts to the substrate shape with a remaining reserve of 0.10mm-0.15mm; the fine milling cutter wheel number is 1000-1200#, and the fine milling is divided into 1-2 cuts, the first cut processes 0.06mm-0.10mm, and the second cut processes 0.04mm-0.05mm. After the two steps of rough milling and fine milling, a substrate with a shape corresponding to the outline of the mobile terminal battery cover and having characteristic structures such as the camera module hole is obtained, that is, a substrate with a preset shape is obtained.
[0117] It should be noted that, in this embodiment, the step of processing the substrate into a substrate of a preset shape can be performed before or after the etching treatment. For example, in other embodiments, the initial substrate can be first processed into a substrate of a preset shape, and then the substrate of the preset shape can be etched.
[0118] S405: First polishing: Cerium oxide or zirconium oxide powder is dissolved in water to prepare a polishing liquid with a concentration of 20-50%, and a brush-like tool made of materials such as bristles or polyurethane is used to polish the outer circumference of the above-mentioned preset shape of the substrate for 10 minutes to 20 minutes to remove micro cracks generated by the CNC process.
[0119] S406: Second polishing: Cerium oxide or zirconium oxide powder is dissolved in water to prepare a polishing liquid with a concentration of 20-50%, and a brush-like tool made of pig bristles or plastic wire is used to polish the camera hole module of the above-mentioned preset shape substrate for 10 minutes to 15 minutes to remove micro cracks generated by the CNC process.
[0120] S407: forming a protective layer on the first surface: if the etching depth formed on the first surface of the etched substrate is greater than a preset threshold, an ink protective layer needs to be coated on the first surface of the etched substrate to protect the etching texture on the substrate of a preset shape during the subsequent hot pressing process, while avoiding damage to the mold cavity caused by excessive etching depth.
[0121] It should be noted that, in this embodiment, the step of forming a protective layer on the first surface is arranged between the second polishing and the hot pressing molding. It can be determined that the step of forming a protective layer on the first surface can be performed at any time point between the end of the etching process and the beginning of the hot pressing molding. For example, in other embodiments, the step of forming a protective layer on the first surface can be arranged between the etching process and the cutting process.
[0122] S408: Hot pressing: Place the polished substrate with a preset shape and a protective layer in a forming mold made of graphite or metal material, and heat it 6 to 8 times according to the first preset rule until the substrate with the preset shape is heated to 50°C to 100°C above the glass softening point, at which time the substrate softens, and then pressurize the softened substrate 2 to 3 times according to the second preset rule, and finally hot press the substrate into a shape that matches the mold shape to form a shell. The frequency of hot pressing is 60 to 120s / piece.
[0123] S409: Removing the protective layer: The hot-pressed substrate is immersed or sprayed with an alkaline solution to remove the ink protective layer on the first surface and the second surface of the substrate.
[0124] S410: Third polishing: Cerium oxide or zirconium oxide powder is dissolved in water to prepare a polishing liquid with a concentration of 20-50%, and a brush-like tool made of bristles or polyurethane is used to polish the second surface of the hot-pressed shell, that is, the inner surface and the circumference, to remove the indentation produced during the hot-pressing process, so that the shell has a more perfect appearance. Since the first surface of the initial glass substrate is etched in advance in step S402, in this step, when polishing the surface of the shell, only the second surface needs to be polished.
[0125] It should be noted that the polishing liquids used in the first polishing, the second polishing and the third polishing may be the same or different.
[0126] S411: Strengthening: The hot-pressed shell is immersed in a molten solution of sodium nitrate and potassium nitrate, so that the lithium ions on the surface of the shell are exchanged with the potassium ions or sodium ions in the molten solution, and the sodium ions on the surface of the shell are exchanged with the potassium ions in the molten solution, so as to achieve the purpose of strengthening the glass shell and improving the performance of the shell.
[0127] S412: Appearance processing: The above-mentioned reinforced shell is subjected to appearance processing, specifically, the second surface of the shell, that is, the inner surface, is subjected to coating and spraying, and the first surface of the shell, that is, the outer surface, is subjected to anti-fingerprint processing to reduce fingerprints left on the first surface during the use of the mobile terminal, and to improve the friction feel of the surface of the battery cover of the mobile terminal, and finally the battery cover of the mobile terminal is obtained.
[0128] An exemplary embodiment of the present disclosure provides a shell, which is manufactured according to the above-mentioned shell manufacturing method.
[0129] The shell provided by the exemplary embodiment of the present disclosure includes a first surface after etching. When the shell is applied to the battery cover of an electronic device, the first surface of the shell serves as the outer surface of the battery cover of the electronic device. The first surface has a matte effect, which enables the electronic device to meet the user's appearance requirements and use feel requirements. In the preparation process of the shell, the substrate is first etched and then hot-pressed to form the shell, so that the shell can have a complex structure without affecting the etching effect and appearance texture of the shell.
[0130] An exemplary embodiment of the present disclosure provides an electronic device, which includes the above-mentioned housing.
[0131] The electronic device provided by the exemplary embodiment of the present disclosure includes a shell provided by the exemplary embodiment of the present disclosure, and the shell includes a first surface after etching. The first surface after etching is used as the outer surface of the battery cover of the electronic device. The first surface has a matte effect, which can enable the electronic device to meet the user's appearance and usage feel requirements.
[0132] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them. Although the present disclosure has been described in detail with reference to the above embodiments, a person skilled in the art should understand that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents; and these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present disclosure.
Claims
1. A method for preparing a shell, characterized in that: The preparation method comprises: Etching the first surface of the initial substrate to obtain an etched substrate; The etched substrate is hot-pressed in a molding die to form the shell, wherein the first surface is the outer surface of the shell.
2. The method for preparing a shell according to claim 1, characterized in that: When the etching depth of the first surface is greater than a preset threshold, the preparation method further includes: A first protective layer is formed on the first surface of the etched substrate.
3. The method for preparing a shell according to claim 2, characterized in that: The thickness of the first protection layer is greater than or equal to the etching depth of the first surface etching process.
4. The method for preparing a shell according to claim 2, characterized in that: The preset threshold is in the range of 20 micrometers to 50 micrometers.
5. The method for preparing a shell according to claim 2, characterized in that: After the step of hot pressing the etched substrate in a forming mold, the preparation method further comprises: The first protective layer is removed.
6. The method for preparing a housing according to claim 1, characterized in that: Before etching the first surface of the initial substrate to obtain an etched substrate, the preparation method further comprises: A second protective layer is formed on the second surface of the initial substrate to protect the second surface during the etching process.
7. The method for preparing a housing according to claim 6, characterized in that: After the step of hot pressing the etched substrate in a forming mold, the preparation method further comprises: removing the second protective layer; The second surface is polished with a first preset polishing solution.
8. The method for preparing a housing according to claim 1, characterized in that: The etching process is performed on the first surface of the initial substrate to obtain an etched substrate, comprising: The first surface of the initial substrate is sprayed or immersed with a preset etching solution for a first preset time to obtain the etched substrate.
9. The method for preparing a shell according to claim 8, characterized in that: The preset etching solution is an acid solution with a pH value of 1 to 2 or an alkaline solution with a pH value of 10 to 14.
10. The method for preparing a housing according to claim 1, characterized in that: The preparation method further comprises: Processing the initial substrate or the etched substrate into a substrate of a preset shape; The processed part of the substrate with the preset shape is polished with a second polishing solution.
11. The method for preparing a housing according to claim 1, characterized in that: The step of hot pressing the etched substrate in a forming mold comprises: Heating the etched substrate in the molding die to a preset temperature according to a first preset rule, so that the etched substrate is in a first state; According to the second preset rule, the substrate in the first state is hot pressed to form a shape.
12. The method for preparing a housing according to claim 11, characterized in that: The step of heating the etched substrate to a preset temperature in the molding die according to a first preset rule comprises: heating the etched substrate to the preset temperature in the molding die in a linear temperature increasing manner; or The etched substrate is heated to the preset temperature in the molding die in a step-by-step heating manner.
13. The method for preparing a housing according to claim 11, characterized in that: The step of hot pressing the substrate in the first state to form the substrate according to the second preset rule includes: According to a preset time interval, hot-pressing the substrate in the first state for a preset number of times to shape the substrate in the first state; or According to the preset time interval difference, the substrate in the first state is hot-pressed for a preset number of times to shape the substrate in the first state.
14. The method for preparing a housing according to claim 1, characterized in that: The substrate includes a glass substrate or a ceramic substrate.
15. The method for preparing a housing according to claim 14, characterized in that: After the step of hot pressing the etched substrate in a molding die to form the housing, the preparation method further comprises: The shell is immersed in the molten strengthening liquid for a second preset time so that the lithium ions in the shell are exchanged with the potassium ions or sodium ions in the molten strengthening liquid, and the sodium ions in the shell are exchanged with the potassium ions in the molten strengthening liquid to strengthen the shell.
16. The method for preparing a housing according to claim 15, characterized in that: The molten strengthening solution includes a molten solution of potassium nitrate and sodium nitrate configured in a preset ratio.
17. A housing, characterized in that: The shell is made according to the shell preparation method according to any one of claims 1-16.
18. An electronic device, characterized in that: The electronic device comprises the housing according to claim 17.