Adsorption material, adsorption sheet, separation membrane, artificial dialysis machine, and manufacturing method
By using the 2-dimensional particle material MXene with a specific structure, the problems of limited types and low efficiency of existing adsorption materials are solved, and efficient adsorption of a variety of pathogenic substances is achieved, which significantly improves the removal efficiency of hemodialysis, and has a wide range of Clinical application potential.
Patent Information
- Application Number
- CN202380034701.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-11
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing adsorption materials are limited in types and it is difficult to effectively adsorb a variety of pathogenic substances, especially in hemodialysis, the removal efficiency of a variety of uremia substances and electrolytes is low.
Using a 2-dimensional particle material with a specific structure, called MXene, through its layered structure and surface modification, it realizes efficient adsorption of a variety of adsorbents, including adsorption of proteins, uremia substances and electrolytes.
It provides a wide range of adsorption capacity, significantly improving the removal efficiency of a variety of pathogenic substances during hemodialysis, including proteins and electrolytes, and enhancing the prevention and treatment effects of uremia and inflammatory diseases.
Smart Images

Figure CN119031979A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an adsorption material, an adsorption sheet, a separation membrane, an artificial dialysis machine and a manufacturing method. Background Art
[0002] The number of patients with kidney disease tends to increase year by year. According to statistics from the Japanese Dialysis Medical Association, the number of chronic dialysis patients increased by about 17% between 2010 and 2020. If kidney function decreases due to kidney disease, pathogenic substances accumulate in the blood, which may result in uremia, electrolyte metabolism disorders, autoimmune diseases, etc. In order to treat various symptoms associated with such kidney diseases, hemodialysis-type renal function substitutes that remove pathogenic substances from the body are used.
[0003] Non-Patent Document 1 describes an adsorption-type blood purifier using cellulose beads to which hexadecylamine is fixed as an adsorbent as a filter used in a hemodialysis-type renal function substitute.
[0004] Prior art literature
[0005] Non-patent literature
[0006] Non-patent document 1: Medical device accessories "Lixelle", Kaneka Co., Ltd., revised in January 2017 (10th edition) Summary of the invention
[0007] Problems to be solved by the invention
[0008] In the adsorbent described in Non-Patent Document 1, the type of adsorbate is limited.
[0009] One object of the present disclosure is to provide a novel adsorbent material for adsorbing a wider range of adsorbates than that of Non-Patent Document 1. Another object of the present disclosure is to provide an adsorption sheet, a separation membrane, an artificial dialysis machine using the adsorbent material, and a method for producing the adsorbent.
[0010] Means for solving problems
[0011] The adsorbent material disclosed herein is used for adsorbing pathogenic substances, and the adsorbent material comprises 2-dimensional particles having one or more layers.
[0012] The layer comprises the following formula:
[0013] M m X n
[0014] (wherein, M is at least one metal of Group 3, 4, 5, 6, or 7,
[0015] X is a carbon atom, a nitrogen atom or a combination thereof,
[0016] n is greater than or equal to 1 and less than or equal to 4,
[0017] m is greater than n and less than 5)
[0018] The layer body represented by the invention and the modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom and a hydrogen atom) present on the surface of the layer body.
[0019] Effects of the Invention
[0020] According to the present disclosure, it is possible to provide a novel adsorbent material for adsorbing a wider range of adsorbates than that of Non-Patent Document 1. In addition, the present disclosure can also provide an adsorption sheet, a separation membrane, an artificial dialysis machine using an adsorbent material for adsorbing a wider range of adsorbates than that of Non-Patent Document 1, and a method for producing the adsorbent material.
[0021] Brief description of the attached figure
[0022] Figure 1 The figures are simplified schematic cross-sectional views showing two-dimensional particles as layered materials that can be used as the adsorbent of the present invention, wherein (a) shows a single-layer MXene and (b) shows a multi-layer (exemplarily a double-layer) MXene.
[0023] Figure 2 This is a diagram schematically illustrating an example of an artificial dialysis machine using the adsorbent according to the present invention.
[0024] Figure 3 This is a diagram schematically illustrating another example of an artificial dialysis machine using the adsorbent according to the present invention.
[0025] Specific embodiments of the invention
[0026] (Implementation 1: Adsorbent Material)
[0027] The adsorption material disclosed in the present invention is used to adsorb pathogenic substances.
[0028] It comprises 2-dimensional particles having one or more layers,
[0029] The layer comprises the following composition formula:
[0030] M m X n
[0031] (wherein, M is at least one metal of Group 3, 4, 5, 6, or 7,
[0032] X is a carbon atom, a nitrogen atom or a combination thereof,
[0033] n is greater than or equal to 1 and less than or equal to 4,
[0034] m is greater than n and less than 5)
[0035] The layer body represented by the invention and the modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom and a hydrogen atom) present on the surface of the layer body.
[0036] According to the present disclosure, an adsorbent material capable of adsorbing multiple adsorbents can be provided, and in particular, an adsorbent material capable of adsorbing pathogenic substances can be provided. Although the present disclosure should not be interpreted in a limited manner, the reasons why the adsorbent material of the present disclosure can adsorb multiple adsorbents are as follows.
[0037] That is, the two-dimensional particles contained in the adsorbent material of the present disclosure are particles of a layered material also called MXene. m X n The surface of the layer body represented has one or more modifications or terminations T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom and a hydrogen atom). According to the structure, there are charged positions in the layer contained in the two-dimensional particle, and the surface of the layer of the two-dimensional particle is usually negatively charged. In addition, the end face of the two-dimensional particle (the periphery of the layer of the two-dimensional particle) is usually positively charged. Therefore, from the perspective of the two-dimensional particle as a whole, there is a tendency for positively charged adsorbates (such as cations, etc.) to be adsorbed between the layers, and negatively charged adsorbates (such as anions, etc.) to be adsorbed on the end faces of the layers.
[0038] The inventors of the present disclosure have studied the adsorbates that can be adsorbed by the above-mentioned two-dimensional particles and found that in addition to the above-mentioned positively or negatively charged adsorbates, the two-dimensional particles can also adsorb relatively high molecular weight compounds such as proteins.
[0039] The above two-dimensional particles can be understood as layered materials or layered compounds, also expressed as "M m X n T s ", where s is an arbitrary number, and x or z may be used instead of s. Typically, n may be 1, 2, 3 or 4, but is not limited thereto.
[0040] In addition, in the present disclosure, the above-mentioned layer may be referred to as a MXene layer, and the above-mentioned two-dimensional particles may be referred to as MXene two-dimensional particles or MXene particles.
[0041] In the above formula of MXene, M is preferably at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo and Mn, including at least Ti, and more preferably at least one selected from the group consisting of Ti, V, Cr and Mo, including at least Ti.
[0042] The ratio of Ti atoms in M may be preferably 50 atomic % or more and 100 atomic % or less, more preferably 70 atomic % or more and 100 atomic % or less, and further preferably 90 atomic % or more and 100 atomic % or less.
[0043] For MXene, the above formula is known: m X n As shown below. Sc2C, Ti2C, Ti2N, Zr2C, Zr2N, Hf2C, Hf2N, V2C, V2N, Nb2C, Ta2C, Cr2C, Cr2N, Mo2C, Mo 1.3 C.Cr 1.3 C, (Ti, V) 2C, (Ti, Nb) 2C, W2C, W 1.3 C, Mo2N, Nb 1.3 C.Mo 1.3 Y 0.6 C (in the above formula, "1.3" and "0.6" mean approximately 1.3 (= 4 / 3) and approximately 0.6 (= 2 / 3) respectively),
[0044] Ti3C2, Ti3N2, Ti3(CN), Zr3C2, (Ti, V)3C2, (Ti2Nb)C2, (Ti2Ta)C2, (Ti2Mn)C2, Hf3C2, (Hf2V)C2, (Hf2Mn)C2, (V2Ti)C2, (Cr2Ti)C2, (Cr2V)C 2. (Cr2Nb)C2, (Cr2Ta)C2, (Mo2Sc)C2, (Mo2Ti)C2, (Mo2Zr)C2, (Mo2Hf)C2, (Mo2V)C2, (Mo2Nb)C2, (Mo2Ta)C2, (W2Ti)C2, (W2Zr)C2, (W2Hf)C2,
[0045] Ti4N3, V4C3, Nb4C3, Ta4C3, (Ti, Nb)4C3, (Nb, Zr)4C3, (Ti2Nb2)C3, (Ti2Ta2)C3, (V2Ti2)C3, (V2Nb2)C3, (V2Ta2)C3, (Nb2Ta2)C3, (Cr2Ti2)C3, (Cr2V 2)C3, (Cr2Nb2)C3, (Cr2Ta2)C3, (Mo2Ti2)C3, (Mo2Zr2)C3, (Mo2Hf2)C3, (Mo2V2)C3, (Mo2Nb2)C3, (Mo2Ta2)C3, (W2Ti2)C3, (W2Zr2)C3, (W2Hf2)C3, (Mo 2.7 V 1.3 )C3 (In the above formula, "2.7" and "1.3" mean approximately 2.7 (=8 / 3) and approximately 1.3 (=4 / 3) respectively).
[0046] Typically, in the above formula, M may include Ti and X may be a carbon atom or a nitrogen atom, preferably M may be Ti and X may be a carbon atom. For example, MAX phase is Ti3AlC2, MXene is Ti3C2T s (In other words, M is Ti, X is C, n is 2, and m is 3).
[0047] In addition, in the present disclosure, MXene may contain a relatively small amount of A atoms derived from the MAX phase of the precursor, for example, 10% by mass or less relative to the original A atoms. The residual amount of A atoms may preferably be 8% by mass or less, and more preferably 6% by mass or less. However, even if the residual amount of A atoms exceeds 10% by mass, there may be no problem depending on the purpose and use conditions of the two-dimensional particles.
[0048] The above two-dimensional particles are composed of Figure 1 The MXene particle 10a (single-layer MXene particle) schematically illustrated in (a) is a collection of particles of a layer of MXene (hereinafter referred to as "MXene particles") 10a. More specifically, the MXene particle 10a has a m X n The layer body represented by m X n The MXene layer 7a is a modified or terminated MXene layer 1a and a MXene layer 7a existing on the surface of the layer body 1a (more specifically, at least one of the two surfaces facing each other in each layer). Therefore, the MXene layer 7a is also represented as “MXene layer 1a”. m X n T s ", s is an arbitrary number.
[0049] The above-mentioned 2D particles may comprise one or more layers. Figure 1 As schematically shown in (b), examples of the plurality of layer MXene particles (multilayer MXene particles) include double-layer MXene particles 10b, but the invention is not limited thereto. Figure 1 1b, 3b, 5b, 7b in (b) and the above Figure 1 1a, 3a, 5a, and 7a in (a) are the same. Two adjacent MXene layers (e.g., 7a and 7b) of a multilayer MXene particle do not need to be completely separated and may be partially in contact. The MXene particle 10a is a particle in which the multilayer MXene particles 10b are separated and exist as one layer, and sometimes is a mixture of the single-layer MXene particles 10a and the multilayer MXene particles 10b in which unseparated multilayer MXene particles 10b remain.
[0050] Although not limited to the present embodiment, the thickness of each layer contained in the MXene particle (corresponding to the above-mentioned MXene layers 7a and 7b) can be, for example, 0.8 nm to 5 nm, and in particular 0.8 nm to 3 nm (may vary mainly depending on the number of M atomic layers contained in each layer). For each stack of multilayer MXene particles that can be included, the interlayer distance (or gap size, Figure 1 The thickness (represented by Δd in (b)) may be, for example, 0.8 nm to 10 nm, particularly 0.8 nm to 5 nm, more particularly about 1 nm, and the total number of layers may be 2 to 20,000.
[0051] In one aspect, the ratio of (the average value of the major diameter of the two-dimensional surface of the two-dimensional particle) / (the average value of the thickness of the two-dimensional particle) is 1.2 or more, preferably 1.5 or more, and more preferably 2 or more. The average value of the major diameter of the two-dimensional surface of the two-dimensional particle and the average value of the thickness of the two-dimensional particle can be obtained by the method described below.
[0052] In one aspect, the two-dimensional particles in the present embodiment preferably contain the above-mentioned multilayer MXene particles that can be included, which contain two-dimensional particles with a small number of layers obtained by delamination. The above-mentioned "small number of layers" means, for example, that the number of stacking layers of the MXene layer is 6 or less. In addition, the thickness of the multilayer MXene particles with a small number of layers in the stacking direction is preferably 15nm or less, and more preferably 10nm or less. Hereinafter, the "multilayer MXene particles with a small number of layers" are sometimes referred to as "few-layer MXene particles". In addition, single-layer MXene particles and few-layer MXene particles are sometimes referred to as "single-layer·few-layer MXene particles" together. By including single-layer·few-layer MXene particles, the conductivity of the obtained film can be improved.
[0053] In multilayer MXene particles with a small number of layers, the ratio of (the average value of the major diameter of the two-dimensional surface of the two-dimensional particle) / (the average value of the thickness of the two-dimensional particle) is greater than 1.2, preferably greater than 1.5 and less than 10, and more preferably greater than 2 and less than 5. Hereinafter, the "MXene particles with a small number of layers" are sometimes referred to as "few-layer MXene particles". In addition, single-layer MXene particles and few-layer MXene particles are sometimes referred to as "single-layer·few-layer MXene particles" together. As a result, the film-forming properties of the film containing the two-dimensional particles can be improved.
[0054] Examples of the single-layer or few-layer MXene particles include two-dimensional particles obtained by a delamination process.
[0055] In one aspect, the 2D particles of the present embodiment preferably include monolayer MXene particles and few-layer MXene particles, i.e., monolayer·few-layer MXene particles. In the 2D particles of the present embodiment, the proportion of monolayer·few-layer MXene particles having a thickness of 15 nm or less is preferably 90% by volume or more, more preferably 95% by volume or more. Thus, the film-forming property of the film containing the 2D particles can be improved.
[0056] (Average value of the major diameter of the two-dimensional surface of the two-dimensional particle)
[0057] The average value of the major diameter of the two-dimensional surface of the two-dimensional particle of the present embodiment is 0.01 μm or more and 20 μm or less. Hereinafter, the average value of the major diameter of the two-dimensional surface may be referred to as "average flake size".
[0058] The larger the average flake size is, the better the orientation of the two-dimensional particles becomes in the material containing the two-dimensional particles. The orientation of the two-dimensional particles can be evaluated, for example, by the electrical conductivity of the material containing the two-dimensional particles.
[0059] The average value of the major diameter of the two-dimensional surface is preferably 0.02 μm or more, and more preferably 0.05 μm or more. In the case of MXene delamination by ultrasonic treatment of MXene, since most of the MXene is reduced in major diameter to about several hundred nm by ultrasonic treatment, it is believed that the orientation of the two-dimensional particles of the film formed by the monolayer MXene delaminated by ultrasonic treatment is low.
[0060] From the viewpoint of dispersibility in a dispersion medium, the average value of the major axis of the two-dimensional surface is 20 μm or less, preferably 15 μm or less, and more preferably 10 μm or less.
[0061] The major diameter of the two-dimensional surface refers to the major diameter when each MXene particle is approximated as an elliptical shape in the electron microscope photograph, and the average value of the major diameter of the two-dimensional surface refers to the number average of the major diameters of more than 80 particles. As an electron microscope, a scanning electron microscope (SEM) or a transmission electron microscope (TEM) photograph can be used.
[0062] The average value of the major diameter of the two-dimensional particles of this embodiment can be measured by dissolving a material including the two-dimensional particles in a solvent and dispersing the two-dimensional particles in the solvent. Alternatively, the average value can be measured based on an SEM image of the material.
[0063] (Average value of the thickness of 2D particles)
[0064] The average value of the thickness of the two-dimensional particles of this embodiment is preferably 1 nm or more and 15 nm or less. The above thickness is preferably 10 nm or less, more preferably 7 nm or less, and further preferably 5 nm or less. On the other hand, if the thickness of a single-layer MXene particle is considered, the lower limit of the thickness of the two-dimensional particle can be 1 nm.
[0065] The average value of the thickness of the two-dimensional particles can be obtained as a number average size (for example, a number average of at least 40 particles) based on an atomic force microscope (AFM) photograph or a transmission electron microscope (TEM) photograph.
[0066] Hereinafter, the method for producing the two-dimensional particles will be described in detail, but the present invention is not limited to this embodiment.
[0067] The method for producing the above-mentioned two-dimensional particles comprises:
[0068] (a) preparing a specified precursor,
[0069] (b) removing at least a portion of the A atoms from the precursor using an etching solution, thereby obtaining an etched product, and
[0070] (c) cleaning the etched product to obtain an etched and cleaned product;
[0071] The above method may further include:
[0072] (d) mixing the etching and cleaning product with a metal compound containing metal cations to obtain an intercalation product in which the metal cations are intercalated in the etching and cleaning product,
[0073] (e) stirring the intercalation product to obtain a layered product in which the intercalation product is layered.
[0074] In one aspect, the etching processed product or the delamination processed product can be used as the two-dimensional particles, and the etching and cleaning processed product is preferably used as the two-dimensional particles.
[0075] Hereinafter, each step will be described in detail.
[0076] Process (a)
[0077] First, a specific precursor is prepared. The specific precursor that can be used in this embodiment is a MAX phase that is a precursor of MXene.
[0078] It is expressed by the following formula:
[0079] M m AX n
[0080] (wherein, M is at least one metal of Groups 3, 4, 5, 6, and 7, including at least Ti, and X is a carbon atom, a nitrogen atom, or a combination thereof,
[0081] A is at least one metal of Group 12, 13, 14, 15, or 16,
[0082] n is greater than or equal to 1 and less than or equal to 4,
[0083] m is greater than n and less than 5).
[0084] The above-mentioned M, X, n and m are as described above.
[0085] A is at least one element of Groups 12, 13, 14, 15, and 16, usually an element of Group A, typically Group IIIA and Group IVA, and more specifically may include at least one selected from the group consisting of Al, Ga, In, Tl, Si, Ge, Sn, Pb, P, As, S and Cd, preferably Al.
[0086] MAX phase is composed of M m X n The MAX phase has the following repeating units, but is not limited thereto. Typically, when m=n+1, a layer of X atoms is arranged between each layer of n+1 layers of M atoms (also collectively referred to as "M m X n layer”), and the layer of A atoms (“A atomic layer”) is configured as a layer next to the layer of the n+1th M atoms.
[0087] The MAX phase can be produced by a known method. For example, TiC powder, Ti powder and Al powder are mixed in a ball mill, and the obtained mixed powder is sintered in an Ar atmosphere to obtain a sintered body (massive MAX phase). Then, the obtained sintered body is crushed with an end mill to obtain a powdered MAX phase for the next step.
[0088] Process (b)
[0089] In step (b), etching is performed using an etching solution to remove the precursor M m AX n The etching treatment removes at least a portion of the A atoms. m X n The layer indicated remains unchanged, but at least a part of the layer composed of A atoms is removed.
[0090] The etching solution may contain an acid such as HF, HCl, HBr, HI, sulfuric acid, phosphoric acid, nitric acid, etc., and typically an etching solution containing F atoms may be used. Examples of the etching solution include a mixture of LiF and hydrochloric acid; a mixture of hydrofluoric acid and hydrochloric acid; a mixture containing hydrofluoric acid, etc., and these mixtures may further contain phosphoric acid, etc. The etching solution may typically be an aqueous solution.
[0091] As the etching operation and other conditions using the above-mentioned etching solution, the conditions conventionally performed can be adopted.
[0092] Process (c)
[0093] In step (c), the product obtained by etching is cleaned to obtain an etching-cleaned product. The acid and the like used in the etching process can be sufficiently removed by cleaning.
[0094] Cleaning can be carried out using a cleaning solution, typically by mixing the etched product and the cleaning solution. The cleaning solution typically contains water, preferably pure water. On the other hand, in addition to pure water, it may further contain a small amount of hydrochloric acid or the like. The amount of the cleaning solution mixed with the etched product and the method of mixing the etched product and the cleaning solution are not particularly limited. For example, as the mixing method, the etched product and the cleaning solution may be coexisted, stirred, centrifuged, etc. As the stirring method, stirring methods using manual vibration (handshake), automatic vibrator, shared mixer, pot mill, etc. may be mentioned. The degree of stirring such as the stirring speed and stirring time can be adjusted according to the amount or concentration of the etched product to be processed. The cleaning in the above-mentioned cleaning solution may be carried out more than once, and preferably the cleaning in the above-mentioned cleaning solution is carried out multiple times. For example, specifically, the cleaning in the above-mentioned cleaning solution can be carried out by sequentially carrying out step (i) (adding the cleaning solution to the treated material or the remaining precipitate obtained in the following (iii)) for stirring, step (ii) for centrifugal separation of the stirred material, and step (iii) for discarding the supernatant after centrifugal separation, and repeating steps (i) to (iii) within a range of more than 2 times, for example, less than 15 times.
[0095] Step (d)
[0096] In step (d), a metal compound containing metal cations is used to intercalate the etching and cleaning product with metal cations to obtain an intercalation product. m X n The intercalation treatment between the layers can also be carried out in a dispersion medium.
[0097] The metal cations may be the same as the metal cations contained in the two-dimensional particles, including Li cations, or may include other metal cations.
[0098] However, the metal of the metal cation is different from the M atom. In addition, the metal of the metal cation is different from the A atom contained in the precursor.
[0099] As the above-mentioned metal compound, there can be mentioned an ionic compound in which the above-mentioned metal cation and an anion are combined. For example, there can be mentioned iodides, phosphates, sulfide salts including sulfates, nitrates, acetates, and carboxylates of the above-mentioned metal cations. As the above-mentioned metal cation, lithium ions are preferred, and as the metal compound, metal compounds containing lithium ions are preferred, and ionic compounds of lithium ions are more preferred, and more preferably, iodides, phosphates, and sulfide salts of lithium ions are more preferred. If lithium ions are used as metal ions, water hydrated with lithium ions has the most negative dielectric constant, so it is considered that it becomes easy to form a single layer.
[0100] The specific method of intercalation treatment is not particularly limited. For example, the etched and cleaned product and the metal compound can be mixed and stirred or left to stand. For example, stirring at room temperature can be cited. For example, the above stirring method can include a method using a stirrer such as a stirring rod, a method using a stirring blade, a method using a mixer, and a method using a centrifugal device. The stirring time can be set according to the manufacturing scale of the single-layer and few-layer MXene particles, for example, it can be set between 12 and 24 hours.
[0101] The intercalation treatment can be carried out in the presence of a dispersion medium, such as water, N-methylpyrrolidone, N-methylformamide, N,N-dimethylformamide, methanol, ethanol, dimethyl sulfoxide, ethylene glycol, acetic acid and other organic media.
[0102] The order of mixing the dispersion medium, the etching and cleaning product, and the metal compound is not particularly limited. In one aspect, the dispersion medium and the etching and cleaning product may be mixed before the metal compound is mixed. Typically, an etching solution after etching may be used as the dispersion medium.
[0103] The intercalation treatment can typically be performed on the etched and cleaned product, but in another aspect, it can also be performed on the above-mentioned precursor simultaneously with the etching treatment. Specifically, the etching and intercalation treatment includes mixing the precursor, the etching solution and the metal compound containing the metal cation, removing at least a portion of the A atoms from the above-mentioned precursor, and intercalating the metal cation into the precursor from which the A atoms have been removed, thereby obtaining the intercalated product. Thus, it is possible to obtain a precursor (MAX) in which at least a portion of the A atoms have been removed while the M in the precursor (MAX) has been removed. m X n Layers remain, and in the adjacent multiple Mm X n Intercalation treatment material with metal cations intercalated between layers.
[0104] As the etching solution and the metal compound used in the etching and intercalation treatment, the same etching solution and the metal compound as used in step (b) can be used, respectively.
[0105] Process (e)
[0106] In step (e), the intercalation product is stirred to separate the intercalation product into layers, thereby obtaining a layered product. By stirring, shear stress is applied to the intercalation product, and two adjacent M m X n At least a portion between the layers can make the MXene particles single-layer or few-layer.
[0107] The conditions for the layering treatment are not particularly limited and can be carried out by known methods. For example, as a method for applying shear stress to the intercalation treatment material, a method of dispersing and stirring the intercalation treatment material in a dispersion medium can be cited. As a stirring method, stirring using a mechanical vibrator, a vortex mixer, a homogenizer, ultrasonic treatment, manual vibration, an automatic vibrator, etc. can be cited. The degree of stirring such as the stirring speed and stirring time can be adjusted according to the amount or concentration of the treatment object to be treated. For example, it can be cited that after the above-mentioned intercalation slurry is centrifuged and the supernatant is discarded, pure water is added to the remaining precipitate, and the layer separation is performed by stirring such as manual vibration or automatic vibrator. Regarding the removal of unpeeled objects, it can be cited that after centrifugation and the supernatant is discarded, the process of washing the remaining precipitate with water can be cited. For example, (i) pure water is added to the remaining precipitate after the supernatant is discarded, stirring, (ii) centrifugation, and (iii) recovering the supernatant. The operations (i) to (iii) are repeated once or more, preferably twice or more and 10 times or less, to obtain a supernatant containing single-layer and few-layer MXene particles as a demixed product. Alternatively, the supernatant may be centrifuged, and the supernatant after centrifugation may be discarded to obtain a clay containing single-layer and few-layer MXene particles as a demixed product.
[0108] The above-mentioned demixed product may be further washed. By this washing, at least a part of impurities etc. may be removed. Hereinafter, the product obtained by washing the demixed product is also referred to as demixed washed product, and the demixed washed product is included in the technical scope of demixed product.
[0109] In one aspect, the above-mentioned cleaning can be carried out using a cleaning solution, and typically, can be carried out by mixing the stratified treated product and the cleaning solution. In another aspect, the above-mentioned cleaning can be carried out by mixing the acid-treated product and the cleaning solution after the stratified treated product is subjected to an acid treatment. As the acid, inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, perchloric acid, hydroiodic acid, hydrobromic acid, and hydrofluoric acid; organic acids such as acetic acid, citric acid, oxalic acid, benzoic acid, and sorbic acid can be appropriately used, and the concentration of the acid in the acid solution can be appropriately adjusted according to the stratified treated product. In addition, the cleaning in the above-mentioned cleaning solution can be carried out by sequentially performing step (i) (in the treated product or the remaining precipitate obtained in the following (iii)) adding the cleaning solution to stir, step (ii) centrifuging the stirred product, and step (iii) discarding the supernatant after centrifugation, and repeating steps (i) to (iii) within a range of 2 or more, for example, 15 or less. The above-mentioned stirring can be carried out using manual vibration, automatic vibrator, shared mixer, pot mill, etc. Acid treatment can be carried out more than once, and as required, it can be mixed and stirred with fresh acid solution (acid solution not used for acid treatment) more than 2 times, for example, within the range of less than 10 times. As the above-mentioned cleaning solution, the same cleaning solution as the cleaning solution in the process (c) can be used, for example, specifically, as the cleaning solution, water, preferably pure water can be used. The above-mentioned mixing can be implemented by the same method as the mixing method in the process (c), for example, specifically, stirring, centrifugation, etc. can be mentioned. As the stirring method, the stirring method using manual vibration, automatic vibrator, shared mixer, pot mill, etc. can be mentioned.
[0110] The intermediates and target products in the above-described production methods, such as the intercalation products and layered products, can be dried by suction filtration, heat drying, freeze drying, vacuum drying, or the like.
[0111] The proportion of two-dimensional particles in the film disclosed in the present invention is preferably greater than 20 volume % and less than 100 volume %, more preferably greater than 50 volume % and less than 100 volume %, further preferably greater than 70 volume % and less than 100 volume %, further preferably greater than 90 volume % and less than 100 volume %, and even more preferably greater than 95 volume % and less than 100 volume %.
[0112] The adsorbent material of the present disclosure may further include one or more materials selected from ceramics, metals, and resins in addition to the two-dimensional particles. For example, when the adsorbent material of this embodiment includes materials such as ceramics, metals, and resins, the adsorption performance can be easily and stably exerted.
[0113] Examples of the ceramics include metal oxides such as silicon dioxide, aluminum oxide, zirconium oxide, titanium dioxide, magnesium oxide, cerium oxide, zinc oxide, barium titanate, hexaferrite, and mullite, and non-oxide ceramics such as silicon nitride, titanium nitride, aluminum nitride, silicon carbide, titanium carbide, tungsten carbide, boron carbide, and titanium boride.
[0114] Examples of the metal include Group 2 to Group 13 metals such as iron, titanium, magnesium, and aluminum; and alloys based on the Group 2 to Group 13 metals.
[0115] The resin may be any of natural resins and synthetic resins, and may be hydrophilic resins or hydrophobic resins. The hydrophilic resin may include a hydrophobic resin made hydrophilic by adding a hydrophilic auxiliary agent such as a surfactant, and a hydrophobic resin partially modified with a hydrophilic group.
[0116] Examples of the hydrophilic resin include resins having polar groups (e.g., hydroxyl groups, substituted or unsubstituted amino groups, carboxyl groups, sulfonic acid groups, carbonyl groups, ester bonds, amide bonds, etc.), and specifically, include cellulose resins such as cellulose, cellulose acetate, and regenerated cellulose; polysulfone resins such as polysulfone and polyethersulfone; hydrophilic polyurethanes; polyvinyl alcohol and its copolymers; sodium alginate; acrylic resins; substituted or unsubstituted polyacrylamides; acrylonitrile; polyaniline sulfonic acid; and polyamide resins such as nylon.
[0117] In one aspect, the hydrophilic resin preferably has a group as a polar group that can form a hydrogen bond with the modification or terminal T of the layer. Examples of the group include hydroxyl, carboxyl, sulfonic acid, carbonyl, and amide bonds. Examples of the resin having these groups include water-soluble polyurethane, polyvinyl alcohol, sodium alginate, acrylic acid-based water-soluble polymers, polyacrylamide, polyaniline sulfonic acid, and nylon, among which water-soluble polyurethane, polyvinyl alcohol, and sodium alginate are preferred, and water-soluble polyurethane is more preferred.
[0118] In another aspect, as the hydrophilic resin, acrylic resin, polyacrylonitrile, cellulose resin, polysulfone resin, polyvinyl alcohol and copolymers thereof are preferred, polymethyl methacrylate, polyacrylonitrile, cellulose, cellulose acetate, polysulfone, polyvinyl alcohol, copolymers of polyvinyl alcohol and polyethylene are more preferred, polysulfone, polymethyl methacrylate, cellulose acetate are further preferred, and polysulfone and polymethyl methacrylate are further preferred. These resins are resins that can be used for dialysis or blood filtration, and can be preferred when the adsorbent material disclosed in the present invention is applied to a dialysis device.
[0119] Examples of the hydrophobic resin include resins that do not contain the polar group.
[0120] The adsorbent of the present disclosure can be manufactured using the above-mentioned two-dimensional particles. The above-mentioned two-dimensional particles can be used directly as the adsorbent of the present disclosure, or the above-mentioned two-dimensional particles can be mixed with one or more materials selected from ceramics, metals and resins used as needed, and formed into a specified shape as the adsorbent.
[0121] In one aspect, when the adsorbent includes a resin, the adsorbent can be produced by mixing the two-dimensional particles and the resin to form a mixture and then molding the mixture.
[0122] The mixing of the two-dimensional particles and the resin can be carried out in the absence of a solvent or in the presence of a dispersion medium. The dispersion medium is typically water, and depending on the circumstances, in addition to water, a relatively small amount (e.g., 30% by mass or less, preferably 20% by mass or less, of other liquid substances may be included.
[0123] The two-dimensional particles and the resin may be stirred using a dispersing device such as a homogenizer, a propeller stirrer, a thin film rotary stirrer, a planetary stirrer, a mechanical vibrator, or a vortex mixer.
[0124] The forming method is not particularly limited. For example, the mixture of the two-dimensional particles and the resin can be directly formed into a specified shape, or the two-dimensional particles, the resin and the dispersion medium can be mixed to obtain a mixture, and the mixture is applied to a substrate (e.g., a substrate) to obtain a precursor film containing the dispersion medium, and the precursor film is dried to remove at least a portion of the dispersion medium contained in the precursor film to form a film. As the coating method, for example, there can be cited a method of spraying using a nozzle such as a 1-fluid nozzle, a 2-fluid nozzle, an air brush, etc., a slit coating using a bench coater, a comma coater, a rod coater, screen printing, metal mask printing, etc., and a coating method by spin coating, dipping, and dripping.
[0125] The coating and drying can be repeated as many times as necessary until a film of desired thickness is obtained. The drying can be performed, for example, in a normal pressure oven or a vacuum oven at a temperature of 400 degrees or less.
[0126] In another aspect, when the adsorbent includes ceramics or metals, the two-dimensional particles are mixed with, for example, granular ceramics or metals, and heated at a low temperature at which the composition of the two-dimensional particles can be maintained, thereby producing the adsorbent.
[0127] The adsorbent is used to adsorb pathogenic substances, and can be used, for example, to remove or reduce pathogenic substances in blood by adsorption. The ability of the adsorbent to adsorb pathogenic substances can be confirmed, for example, in an adsorption test using human plasma.
[0128] The pathogenic substance preferably contains protein. As the protein, for example, uremic proteins such as parathyroid hormone, β2-microglobulin, tumor necrosis factor (TNF)-α (specifically, middle-molecular uremic substances); cytokines such as interleukins, interferons, chemokines, hematopoietic factors, cell growth factors, tumor necrosis factors (in one aspect, inflammatory cytokines such as interleukin 18); albumin, M protein and other proteins. The above-mentioned uremic proteins (specifically, middle-molecular uremic substances) are equivalent to uremic substances, and by adsorbing them, the preventive effect of uremia can be expected. The above-mentioned inflammatory cytokines can cause various inflammatory symptoms in the body, and by adsorbing them, the preventive effect of inflammation can be expected.
[0129] In the present disclosure, "uremic" means that the concentration in the blood increases with the decrease in kidney function, which may be the cause of various symptoms of kidney diseases such as acute kidney injury (including acute renal failure) and chronic kidney disease (including chronic renal failure and late-stage renal failure), especially various symptoms associated with kidney injury.
[0130] In addition, by adsorbing inflammatory substances that are pathogenic substances, a preventive effect on various symptoms associated with inflammatory diseases can be expected. Examples of various symptoms associated with inflammatory diseases include vascular dementia, inflammatory bowel disease, hepatitis, and myocarditis.
[0131] The pathogenic substance preferably contains an electrolyte (ionic substance). That is, the adsorbent can also be used to adsorb electrolytes. Examples of the electrolyte include cations and anions. Examples of the cation include cations that can be excreted in the kidney, specifically, Na + , K + Mg 2+ , Ca 2+ In the present disclosure, anions that can be excreted in the kidneys are exemplified, and specifically, anions containing P (e.g., PO4 3- ).
[0132] When renal function is reduced, the concentration of the above electrolytes (especially electrolytes that can be excreted by the kidneys) in the blood may increase, which may cause electrolyte metabolic abnormalities such as hypernatremia, hyperkalemia, hypermagnesemia and hyperphosphatemia. By adsorbing these electrolytes with the above adsorbent, a preventive effect on electrolyte metabolic abnormalities can be expected.
[0133] The above-mentioned pathogenic substances preferably further include protein-bound uremic substances such as creatinine, homocysteine or indoxylsulfuric acid, p-tolylsulfuric acid, etc.; carcinogens, etc. That is, the above-mentioned adsorbent can also be used to adsorb protein-bound uremic substances and carcinogens. Therefore, by using the adsorbent material containing the above-mentioned two-dimensional particles as a separation membrane in a dialysis device, the treatment or prevention effect of the above-mentioned various diseases can be expected.
[0134] The adsorbent material disclosed in the present invention can adsorb the above-mentioned adsorbent, so that it can be expected to prevent or treat various symptoms associated with kidney diseases such as acute kidney injury (including acute renal failure), chronic kidney disease (including chronic renal failure, late renal failure), and various symptoms associated with inflammatory diseases, especially various symptoms associated with kidney injury and / or inflammatory diseases. Specifically, it can be expected to prevent or treat uremia; electrolyte metabolism abnormalities such as hypernatremia, hyperkalemia, hypermagnesemia and hyperphosphatemia; autoimmune diseases; infectious diseases; inflammatory diseases; endocrine and metabolic diseases; circulatory system diseases; blood diseases; digestive system diseases; neurological diseases; malignant tumors; drug poisoning; vascular dementia, inflammatory bowel disease, hepatitis, myocarditis and other inflammatory diseases.
[0135] The adsorption method is also included in the technical scope of the present invention, and the above-mentioned adsorption method includes using the above-mentioned adsorbent material to adsorb the above-mentioned pathogenic substance. The adsorption method preferably includes using the above-mentioned adsorbent material to adsorb proteins as pathogenic substances. The above-mentioned adsorption method may further include adsorbing electrolytes as pathogenic substances. That is, the above-mentioned adsorption method may include using the above-mentioned adsorbent material to adsorb the above-mentioned proteins and electrolytes as the above-mentioned pathogenic substances. The adsorption method may further include using the above-mentioned adsorbent material to adsorb other adsorbates. In one aspect, the adsorption of the pathogenic substance can be implemented by contacting a liquid containing adsorbents such as proteins and electrolytes as pathogenic substances with an adsorbent material. The liquid containing the adsorbent may contain substances other than proteins and electrolytes as pathogenic substances. Specific examples of liquids containing the above-mentioned adsorbents include blood, dialysate, etc.
[0136] (Implementation 2: Adsorption sheet)
[0137] The adsorption sheet in this embodiment includes the above-mentioned adsorption material. By including the above-mentioned adsorption material, the adsorption sheet can adsorb a variety of adsorbates, especially pathogenic substances, and the adsorption material can be physically fixed, so the adsorption performance can be stably exerted.
[0138] The adsorption sheet in this embodiment may be composed of the above-mentioned adsorption material, and in addition to the above-mentioned adsorption material, may also contain one or more materials selected from the above-mentioned ceramics, metals and resins. As the ceramics, metals and resins, the same materials as the ceramics, metals and resins that can be contained in the above-mentioned adsorption material can be used respectively.
[0139] When the adsorption sheet of the present embodiment further comprises one or more materials selected from the above-mentioned ceramics, metals and resins, the above-mentioned adsorption sheet may include the above-mentioned adsorption material and a component in which the material is uniformly mixed, or may separately include a component containing the above-mentioned adsorption material and a component containing the material.
[0140] In one aspect, the adsorption sheet in this embodiment may include: a substrate including one selected from the above ceramic, metal and resin; and a film including the above adsorption material and disposed on the substrate. The film including the adsorption material may cover at least a portion of the substrate surface, or may cover the entire substrate surface.
[0141] The adsorption sheet can be manufactured by forming a film containing an adsorbent material on the surface of the substrate. The method for manufacturing a film containing the adsorbent material is not particularly limited, and may include, for example, mixing the two-dimensional particles, a dispersion medium, and two-dimensional particles as required to obtain a mixture, applying the mixture on the substrate to obtain a precursor film containing a dispersion medium, and drying the precursor film to remove at least a portion of the dispersion medium contained in the precursor film to form a film. As a method for applying the mixture to the substrate, commonly used coating methods such as dipping, brushing, rollers, roller coaters, air spraying, vacuum spraying, curtain flow coaters, roller curtain coaters, die coaters, and electrostatic coating can be used. The thickness of the adsorption sheet and the thickness of the substrate can be appropriately set according to the application.
[0142] (Embodiment 3: Separation membrane)
[0143] The separation membrane in this embodiment includes the above-mentioned adsorbent. By including the above-mentioned adsorbent, the separation membrane can adsorb a variety of adsorbates, especially pathogenic substances, and the adsorbent can be physically fixed, so the adsorption performance can be stably exerted. The separation membrane in this embodiment is particularly suitable for use as a separation membrane for artificial dialysis such as the above-mentioned hemodialysis.
[0144] The separation membrane may be composed of the adsorbent material, and in addition to the adsorbent material, may also contain one or more materials selected from the ceramics, metals and resins. In one aspect, it may include: a substrate; a substrate containing one selected from the ceramics, metals and resins; and a membrane containing the adsorbent material and disposed on the substrate. The membrane containing the adsorbent material may cover at least a portion of the substrate surface, or may cover the entire substrate surface. The shape of the substrate is not particularly limited, and may be a film, sheet, plate, porous, hollow fiber, bead, etc.
[0145] As the ceramic, metal and resin, the same materials as the ceramic, metal and resin that can be contained in the above-mentioned adsorbent can be used respectively. Among them, cellulose-based and synthetic polymer-based materials for hemodialysis are preferred, and specifically, polymethyl methacrylate, polyacrylonitrile, cellulose, cellulose acetate, polysulfone, polyvinyl alcohol, vinyl alcohol copolymers such as copolymers of polyvinyl alcohol and ethylene can be preferably used, and polysulfone, polymethyl methacrylate, cellulose acetate are more preferably used, and polysulfone and polymethyl methacrylate are further preferably used. The form of the above-mentioned separation membrane for artificial dialysis is not particularly limited, and for example, porous type, hollow fiber type, and flat membrane stacking type can be cited.
[0146] (Implementation 4: Artificial Dialysis Machine)
[0147] The artificial dialysis machine in this embodiment includes the above-mentioned adsorbent. By including the above-mentioned adsorbent, the artificial dialysis machine can adsorb a variety of adsorbents, especially pathogenic substances, and can be used for adsorption and removal of various wastes in hemodialysis, hemofiltration, hemodiafiltration, peritoneal dialysis, etc. In other words, the adsorbent of this embodiment can be used in artificial dialysis machines that perform the above-mentioned hemodialysis, hemofiltration, hemodiafiltration, peritoneal dialysis, etc.
[0148] The artificial dialysis machines described above are classified into, for example, hemodialysis machines and peritoneal dialysis machines, and the hemodialysis machines are divided into a one-way type (single-pass type) and a circulation type. Furthermore, the circulation type includes the REDY system (recirculating dialysate system) and other systems. The artificial dialysis machines described above can also be divided by a method of removing urea from the cross flow of the patient's blood and the dialysate without contacting the blood, and a method of directly filtering the blood. In addition, the mainstream of the peritoneal dialysis machine is a one-way type. The adsorbent of the present embodiment can be used for any of these hemodialysis and peritoneal dialysis, and can be used as an adsorption membrane, a separation membrane, an adsorption material box, etc. in artificial dialysis machines such as hemodialysis machines and peritoneal dialysis machines. For example, when used in the REDY system (recirculating dialysate system), the adsorbent of the present embodiment is used in an adsorption material box.
[0149] exist Figure 2 In FIG. 1 , as an example of an artificial dialysis machine using the adsorbent material disclosed in the present invention, a general hemodialysis machine is schematically shown. Figure 2In the hemodialysis machine 40, the untreated blood introduced from the blood inlet 41 is transported to the blood purification machine 44 by the blood pump 43. On the other hand, the dialysate from the unused dialysate tank 48 is transported to the blood purification machine 44 by the dialysate pump 50. In the blood purification machine 44, the blood in the blood passage area 46 of the blood purification machine is subjected to hemodialysis, hemofiltration dialysis or hemofiltration through the separation membrane 45, and the substance to be removed is moved to the dialysate passage area 47 of the blood purification machine through the separation membrane 45. The purified blood is transported to the blood outlet 42. On the other hand, the dialysate in the dialysate passage area 47 containing the substance to be removed is transported to the dialysate tank 49 after use. Although Figure 2 Although not shown in the figure, the following device may be provided, which includes a path for supplementing drugs, proteins, etc. to the blood as needed during the blood transportation before and / or after treatment. In addition, a sensor for measuring the blood flow rate, the dialysate flow rate, and the protein concentration in the blood as needed may be provided. In addition, an on-off valve that can open and close the flow path as needed may be provided in the flow path of blood and / or dialysate.
[0150] exist Figure 3 , as another example of an artificial dialysis machine using the adsorbent of the present disclosure, a general hemodialysis machine is schematically shown. Figure 2 Hemodialysis machine 40A with Figure 2 The difference between the hemodialysis machine 40 in FIG. 4 is that a separation membrane 45A is arranged between the blood pump 43A and the blood purification machine 44A, and a semipermeable membrane 51A is arranged in the blood purification machine as a membrane for separating blood and dialysate. Figure 2 The same symbols are given to the hemodialysis machine 40 in FIG. 1 and the like, and the description thereof is omitted.
[0151] exist Figure 3 In the hemodialysis machine 40A, before the blood passes through the blood purification machine 44A, it comes into contact with the separation membrane 45A, and adsorbates such as pathogenic substances can be adsorbed, thereby improving the dialysis efficiency.
[0152] The separation membrane 45A may be covered with a resin or the like and arranged in the form of a column. In addition, in the column, filters may be arranged on the blood inflow side and the blood outflow side of the column, respectively, so that the blood is distributed in the separation membrane 45A.
[0153] exist Figure 3 In the hemodialysis machine 40A, the membrane that separates blood and dialysate is the semipermeable membrane 51A, but the separation membrane of the present disclosure may be used instead of the semipermeable membrane 51A.
[0154] The present invention is described in more detail by the following examples, but the present invention is not limited thereto.
[0155] Example 1
[0156] [Production of MXene]
[0157] In Examples 1 and 2, (1) preparation of a precursor (MAX), (2) etching of the precursor, and (3) cleaning and drying, which are described in detail below, were sequentially performed to produce two-dimensional particles.
[0158] (1) Preparation of precursor (MAX)
[0159] TiC powder, Ti powder and Al powder (all made by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill with zirconia balls at a molar ratio of 2:1:1 and mixed for 24 hours. The obtained mixed powder was sintered at 1350°C for 2 hours under Ar atmosphere. The sintered body (block) thus obtained was crushed with an end mill to a maximum size of less than 40 μm. Thus, Ti3AlC2 particles were obtained as a precursor (MAX).
[0160] (2) Etching of the precursor
[0161] The Ti3AlC2 particles (powder) prepared by the above method are etched under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the Ti3AlC2 powder.
[0162] (Etching conditions)
[0163] Precursor: Ti3AlC2 (sieved with a mesh size of 45 μm)
[0164] Etching solution composition: 50 mass% HF 6mL
[0165] H2O 18mL
[0166] HCl (12M) 36 mL
[0167] Precursor input amount: 3.0g
[0168] Etching container: 100mL Iboy
[0169] Etching temperature: 35°C
[0170] Etching time: 24h
[0171] Stirring rod speed: 400rpm
[0172] 3) Cleaning and drying
[0173] The slurry was divided into two parts, each of which was placed in two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain Ti3C2T s - Aqueous medium clay. The obtained clay is freeze-dried to obtain a dry powder of two-dimensional particles.
[0174] Example 2
[0175] In Example 2, after (1) preparing the precursor (MAX) in the same manner as in Example 1, the following step (2) was performed, and (3) washing and drying were performed in the same manner as in Example 1 to produce two-dimensional particles.
[0176] (1) Preparation of precursor: Same as Example 1
[0177] (2) Etching of the precursor
[0178] Precursor: Ti3AlC2 (sieved with a mesh size of 45 μm)
[0179] Etching solution composition: 50 mass% HF 5mL
[0180] H2O 45mL
[0181] Precursor input amount: 3.0g
[0182] Etching container: 100mL Iboy
[0183] Etching temperature: 35°C
[0184] Etching time: 24h
[0185] Stirring rod speed: 400rpm
[0186] (3) Cleaning: Same as Example 1
[0187] Example 3
[0188] In Example 3, after (1) preparing the precursor (MAX) in the same manner as in Example 1, the following step (2) was performed, and (3) washing and drying were performed in the same manner as in Example 1 to produce two-dimensional particles.
[0189] (1) Preparation of precursor: Same as Example 1
[0190] (2) Etching of the precursor
[0191] Precursor: Ti3AlC2 (sieved with a mesh size of 45 μm)
[0192] Etching solution composition: 6 mL of 49 mass% HF aqueous solution
[0193] H2O 9mL
[0194] 85 mass% H3PO4 aqueous solution 45mL
[0195] Precursor input amount: 3.0g
[0196] Etching container: 100mL Iboy
[0197] Etching temperature: 35°C
[0198] Etching time: 24h
[0199] Stirring rod speed: 400rpm
[0200] (3) Cleaning: Same as Example 1
[0201] Example 4
[0202] In Example 4, after (1) preparing the precursor (MAX) in the same manner as in Example 1, the following step (2) was performed, and (3) washing and drying were performed in the same manner as in Example 1 to produce two-dimensional particles.
[0203] (1) Preparation of precursor: Same as Example 1
[0204] (2) Etching of the precursor
[0205] Precursor: Ti3AlC2 (sieved with a mesh size of 45 μm)
[0206] Etching solution composition: LiF 4.8g
[0207] HCl (9M) 60 mL
[0208] Precursor input amount: 3.0g
[0209] Etching container: 100mL Iboy
[0210] Etching temperature: 35°C
[0211] Etching time: 24h
[0212] Stirring rod speed: 400rpm
[0213] (3) Cleaning: Same as Example 1
[0214] Example 5
[0215] In Example 5, (1) preparation of a precursor (MAX), (2) etching of the precursor, and (3) cleaning and drying, which are described in detail below, are sequentially performed to produce two-dimensional particles.
[0216] (1) Preparation of precursor (MAX)
[0217] 73 g of Ti powder, 47.2 g of TiN powder, 20.6 g of Al powder and 9.2 g of C powder (all manufactured by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill containing zirconia balls and mixed for 24 hours. The obtained mixed powder was sintered at 1400°C for 2 hours under an Ar atmosphere. The sintered body (block) thus obtained was crushed with an end mill to a maximum size of less than 40 μm. Thus, Ti3AlCN particles were obtained as a precursor (MAX).
[0218] (2) Etching of the precursor
[0219] The Ti3AlCN particles (powder) prepared by the above method were etched under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the Ti3AlCN powder.
[0220] (Etching conditions)
[0221] Precursor: Ti3AlCN (sieved with a mesh size of 45 μm)
[0222] Etching solution composition: 48 mass% HF 6mL
[0223] 38.8 mass% HCl 36 mL
[0224] H2O 18mL
[0225] Precursor input amount: 3.0g
[0226] Etching container: 100mL Iboy
[0227] Etching temperature: 25°C
[0228] Etching time: 24h
[0229] Stirring rod speed: 400rpm
[0230] (3) Cleaning and drying
[0231] The slurry was divided into two parts, each of which was placed in two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain Ti3CNT s - Aqueous medium clay. The obtained clay is freeze-dried to obtain a dry powder of two-dimensional particles.
[0232] Example 6
[0233] In Example 6, (1) preparation of a precursor (MAX), (2) etching of the precursor, and (3) cleaning and drying, which are described in detail below, are sequentially performed to produce two-dimensional particles.
[0234] (1) Preparation of precursor (MAX)
[0235] 21.5 g of V powder, 6.3 g of Al powder and 2.3 g of C powder (all manufactured by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill containing zirconia balls and mixed for 24 hours. The obtained mixed powder was sintered at 1550° C. for 2 hours under an Ar atmosphere. The sintered body (block) thus obtained was crushed with a jaw crusher to a maximum size of 45 μm or less. Thus, V2AlC particles were obtained as a precursor (MAX).
[0236] (2) Etching of the precursor
[0237] The V2AlC particles (powder) prepared by the above method were etched under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the V2AlC powder.
[0238] (Etching conditions)
[0239] Precursor: V2AlC (sieved with a mesh size of 45 μm)
[0240] Etching solution composition: 48 mass% HF 6mL
[0241] 38.8 mass% HCl 24 mL
[0242] Precursor input amount: 3.0g
[0243] Etching container: 100mL Iboy
[0244] Etching temperature: 50℃
[0245] Etching time: 48h
[0246] Stirring rod speed: 400rpm
[0247] (3) Cleaning and drying
[0248] The slurry was divided into two parts, each of which was placed in two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain V2CT s - Aqueous medium clay. The obtained clay is freeze-dried to obtain a dry powder of two-dimensional particles.
[0249] Example 7
[0250] In Example 7, (1) preparation of a precursor (MAX), (2) etching of the precursor, and (3) cleaning and drying, which are described in detail below, are sequentially performed to produce two-dimensional particles.
[0251] (1) Preparation of precursor (MAX)
[0252] 105.4 g of Ti powder, 32.7 g of Al powder and 11.9 g of C powder (all made by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill with zirconia balls and mixed for 24 hours. The obtained mixed powder was sintered at 1550°C for 2 hours under Ar atmosphere. The sintered body (block) thus obtained was crushed with an end mill to a maximum size of less than 40 μm. Thus, Ti2AlC particles were obtained as a precursor (MAX).
[0253] (2) Etching of the precursor
[0254] The Ti2AlC particles (powder) prepared by the above method were etched under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the Ti2AlC powder.
[0255] (Etching conditions)
[0256] Precursor: Ti2AlC (sieved with a mesh size of 45 μm)
[0257] Etching solution composition: 48 mass% HF 2mL
[0258] 38.8 mass% HCl 12 mL
[0259] H2O 6mL
[0260] Precursor input amount: 1.0g
[0261] Etching container: 100mL Iboy
[0262] Etching temperature: 35°C
[0263] Etching time: 24h
[0264] Stirring rod speed: 400rpm
[0265] (3) Cleaning and drying
[0266] The slurry was divided into two parts, each of which was placed in two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain Ti2CT s- Aqueous medium clay. The obtained clay is freeze-dried to obtain a dry powder of two-dimensional particles.
[0267] Example 8
[0268] In Example 8, (1) preparation of a precursor (MAX), (2) etching of the precursor, and (3) cleaning and drying, which are described in detail below, are sequentially performed to produce two-dimensional particles.
[0269] (1) Preparation of precursor (MAX)
[0270] TiC powder, Ti powder and Al powder (all made by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill with zirconia balls at a molar ratio of 2:1:1 and mixed for 24 hours. The obtained mixed powder was sintered at 1350°C for 2 hours under Ar atmosphere. The sintered body (block) thus obtained was crushed with an end mill to a maximum size of less than 40 μm. Thus, Ti3AlC2 particles were obtained as MAX particles.
[0271] (2) Etching of the precursor
[0272] The Ti3AlC2 particles (powder) prepared by the above method are etched under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the Ti3AlC2 powder.
[0273] (Etching conditions)
[0274] Precursor: Ti3AlC2 (sieved with a mesh size of 45 μm)
[0275] Etching solution composition: 48% HF 6mL
[0276] H2O 54mL
[0277] Precursor input amount: 3.0g
[0278] Etching container: 100mL Iboy
[0279] Etching temperature: 50℃
[0280] Etching time: 24h
[0281] Stirring rod speed: 400rpm
[0282] (3) Cleaning and drying
[0283] The slurry was divided into two parts, each of which was placed in two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to the remaining precipitate in each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain Ti3C2T x -Water medium clay.
[0284] The obtained clay was freeze-dried to obtain dry powder, thereby obtaining dry powder of two-dimensional particles.
[0285] Example 9
[0286] In Example 9, (1) preparation of a precursor (MAX), (2) etching of the precursor, and (3) cleaning and drying, which are described in detail below, are sequentially performed to produce two-dimensional particles.
[0287] (1) Preparation of precursor (MAX)
[0288] TiC powder, Ti powder and Al powder (all made by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill with zirconia balls at a molar ratio of 2:1:1 and mixed for 24 hours. The obtained mixed powder was sintered at 1350°C for 2 hours under Ar atmosphere. The sintered body (block) thus obtained was crushed with an end mill to a maximum size of less than 40 μm. Thus, Ti3AlC2 particles were obtained as MAX particles.
[0289] (2) Etching of the precursor
[0290] The Ti3AlC2 particles (powder) prepared by the above method are etched under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the Ti3AlC2 powder.
[0291] (Etching conditions)
[0292] Precursor: Ti3AlC2 (sieved with a mesh size of 45 μm)
[0293] Etching solution composition: 48 mass% HF 6mL
[0294] 38.8 mass% HCl 38 mL
[0295] H2O 16mL
[0296] Precursor input amount: 3.0g
[0297] Etching container: 100mL Iboy
[0298] Etching temperature: 50℃
[0299] Etching time: 24h
[0300] Stirring rod speed: 400rpm
[0301] (3) Cleaning and drying
[0302] The slurry was divided into two parts, each of which was placed in two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to the remaining precipitate in each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain Ti3C2T x -Water medium clay.
[0303] The obtained clay was freeze-dried to obtain dry powder, thereby obtaining dry powder of two-dimensional particles.
[0304] Example 10
[0305] In Example 10, the following detailed steps (1) preparation of a precursor (MAX), (2) etching of the precursor, (3) cleaning, (4) Li intercalation, (5) delamination, (6) modification using amino groups and drying are sequentially performed to produce two-dimensional particles.
[0306] (1) Preparation of precursor (MAX)
[0307] TiC powder, Ti powder and Al powder (all made by Kojun Chemical Research Institute Co., Ltd.) were put into a ball mill with zirconia balls at a molar ratio of 2:1:1 and mixed for 24 hours. The obtained mixed powder was sintered at 1350°C for 2 hours under Ar atmosphere. The sintered body (block) thus obtained was crushed with an end mill to a maximum size of less than 40 μm. Thus, Ti3AlC2 particles were obtained as MAX particles.
[0308] (2) Etching of the precursor
[0309] The Ti3AlC2 particles (powder) prepared by the above method are etched under the following etching conditions to obtain a solid-liquid mixture (slurry) containing a solid component derived from the Ti3AlC2 powder.
[0310] (Etching conditions)
[0311] Precursor: Ti3AlC2 (sieved with a mesh size of 45 μm)
[0312] Etching solution composition: 48 mass% HF 2mL
[0313] 38.8 mass% HCl 38 mL
[0314] H2O 16mL
[0315] Precursor input amount: 3.0g
[0316] Etching container: 100mL Iboy
[0317] Etching temperature: 50℃
[0318] Etching time: 24h
[0319] Stirring rod speed: 400rpm
[0320] (3) Cleaning and drying
[0321] The slurry was divided into two parts, each of which was placed in two 50 mL centrifuge tubes. After centrifugation at 3500G using a centrifuge, the supernatant was discarded. 40 mL of pure water was added to the remaining precipitate in each centrifuge tube, and centrifugation was performed again at 3500G to separate and remove the supernatant. This operation was repeated 11 times. After the final centrifugation, the supernatant was discarded to obtain Ti3C2T x -Water medium clay.
[0322] (4) Li intercalation
[0323] For Ti3C2T prepared by the above method x - Aqueous clay was subjected to Li intercalation using LiCl as a Li-containing compound under the following conditions and stirred at 20° C. to 25° C. for 12 hours.
[0324] (Li intercalation conditions)
[0325] Ti3C2T x - Water medium clay (MXene after washing): solid content 0.75g
[0326] LiCl: 0.75g
[0327] Intercalation container: 100mL Iboy
[0328] Temperature: 20°C or above and 25°C or below (room temperature)
[0329] Time: 10h
[0330] Stirring rod speed: 800rpm
[0331] (5) Delamination
[0332] In the above Ti3C2T x-After adding 40 mL of pure water to the aqueous medium clay and stirring for 15 minutes with a vibrator, (ii) centrifugation was performed at 3500G, and (iii) the supernatant was recovered as a liquid containing a monolayer MXene. The operations (i) to (iii) were repeated 4 times in total to obtain a supernatant containing a monolayer MXene. Furthermore, the supernatant was centrifuged at 4300G for 2 hours using a centrifuge, and the supernatant was discarded as a sample containing a monolayer·few-layer MXene to obtain a clay containing a monolayer·few-layer MXene.
[0333] (6) Modification and drying using amino groups
[0334] To 0.34 g of clay containing monolayer and few-layer MXene, 20 mg of 6-aminohexyl phosphate hydrochloride and 5 mL of pure water were added, and stirred at room temperature for 2 hours at a stirring rod speed of 800 rpm. The obtained slurry was centrifuged at a speed of 8000 rpm for 8 minutes, and the supernatant was discarded. Pure water of the same volume as the discarded supernatant was added and centrifuged at a speed of 8000 rpm for 8 minutes. The discarding of the supernatant, the addition of the same volume of pure water as the discarded supernatant, and the centrifugation at a speed of 8000 rpm for 8 minutes were repeated once. Then, the supernatant was discarded, and the same volume of ethanol as the discarded supernatant was added to disperse it, and then dried naturally to obtain Ti3C2 particles (powder) modified with amino groups.
[0335] Comparative Example 1
[0336] Spherical adsorbent carbon ("KREMEZIN Tablets 500 mg", manufactured by Kureha Corporation) was powdered using a mortar and subjected to adsorption evaluation.
[0337] Comparative Example 2
[0338] The adsorbent taken out from the decomposition and adsorption type blood purifier ("Lixelle", manufactured by Kaneka Corporation) was subjected to adsorption evaluation.
[0339] Comparative Example 3
[0340] Medicinal charcoal (manufactured by NIKIKO CO., LTD.) was used for adsorption evaluation.
[0341] Adsorption evaluation method
[0342] Human plasma collected from healthy subjects and the two-dimensional particles of the embodiment and the spherical adsorbent carbon, adsorption-type blood purifier or medicinal carbon of the comparative example (hereinafter collectively referred to as "adsorbent material") were measured into a 50 mL centrifuge tube and vibrated for 60 minutes using a constant temperature vibrator (TAITEC BR-33FL) set at 37°C. Then, a few mL of the mixed solution was sampled, and the adsorbent material was separated using a syringe filter with a pore size of 0.45 μm (Merck Millipore sterilization Millex: diameter 33 mm, pore size 0.45 μm), and then the components were analyzed. In Examples 1 to 4 and Comparative Examples 1 to 3, the amount of human plasma was set to 10 mL and the amount of adsorbent material was set to 0.6 g. In Examples 5 to 8 and Example 10, the amount of human plasma was set to 4 mL and the amount of adsorbent material was set to 0.2 g. In Example 9, the amount of human plasma was set to 4 mL and the amount of adsorbent material was set to 0.2 g.
[0343] In Examples 1-4 and Comparative Examples 1-3, component analysis was performed on Na, P, K, urea, creatinine, homocysteine, folic acid, parathyroid hormone, β2-microgloblin, interleukin-18, trypsin, TNF-α (Tumor necrosis factor-α), α-amylase, and albumin.
[0344] In Examples 5 to 10, component analysis was performed on albumin, chloride (Cl), serum urea nitrogen (BUN), α-amylase (AMY), lipase, Na, K, inorganic phosphorus (IP), and β2-microglobulin.
[0345] The determination of Na, K, and Cl is carried out by the electrode method; the determination of P, inorganic phosphorus, α-amylase, lipase, and creatinine is carried out by the enzymatic method; the determination of urea and serum urea nitrogen is carried out by the urease·GLDH·UV method; the determination of homocysteine is carried out by the HPLC method; the determination of folic acid is carried out by the CLIA method; the determination of parathyroid hormone is carried out by the ECLIA method; the determination of β2-microglobulin is carried out by the latex agglutination method; the determination of interleukin-18, trypsin, and TNF-α is carried out by the EIA method; the determination of albumin is carried out by the colorimetric method (BGC method).
[0346] In addition, the same treatment was performed on human plasma placed in a centrifuge tube without the adsorbent, and this was used as the baseline for the component concentration. The concentration of component A in human plasma after the adsorption test was defined as C. A1 , let the concentration of component A in the baseline be C A0 The adsorption removal rate was calculated according to the following formula: When the adsorption removal rate was less than 0 mass %, it was set to 0 mass %.
[0347] Adsorption removal rate (mass %) = (C A0 -C A1 ) / C A0 × 100
[0348] Tables 1 and 2 show the results.
[0349] Table 1
[0350] Element Molecular weight Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Na 23 21 22 21 20 0 0 0 P 31 44 46 40 42 0 0 0 K 39 29 29 29 28 0 0 0 Urea 60 0 0 2 1 13 0 9 Creatinine 113 92 91 90 90 91 0 90 Homocysteine 135 70 72 68 70 0 0 86 Folic acid 441 87 80 81 75 68 0 42 Parathyroid hormone 9,500 73 75 70 70 0 0 35 β2-microglobulin 11,818 50 55 46 52 0 99 5 Interleukin-18 18,000 29 33 28 27 0 0 0 Trypsin 24,000 26 25 22 24 0 0 0 TNF-α 25,000 50 39 28 32 0 0 0 α-Amylase 54,000 26 22 22 18 0 0 0 albumin 66,000 11 10 8 11 0 0 0
[0351] Table 2
[0352] Element Molecular weight Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 albumin 66,000 3 3 0 0 3 0 Cl 35 95 13 95 55 30 0 BUN 60 0 0 0 0 0 0 AMY 54,000 0 0 16 0 0 0 Lipase 45,000 0 0 0 0 0 0 Na 23 19 6 26 6 8 1 K 39 32 21 46 10 11 3 IP 31 56 0 58 7 42 33 β2-microglobulin 11,818 8 0 75 0 0 25
[0353] It was confirmed that the adsorbents of Examples 1 to 4 showed adsorption of parathyroid hormone, β2-microglobulin, tumor necrosis factor (TNF)-α and other middle-molecular uremic substances as pathogenic substances; inflammatory cytokines such as interleukin-18; proteins such as albumin, and further adsorbed Na + , K + , P and other electrolytes; creatinine, homocysteine and other protein-bound uremic substances. Therefore, the adsorbent material containing the above two-dimensional particles can adsorb a variety of adsorbents, and can be expected to be used in adsorption sheets, separation membranes and artificial dialysis machines using the adsorbent material.
[0354] In addition, it was confirmed that the two-dimensional particles of Examples 5 to 10 showed the effect of adsorbing pathogenic substances, especially electrolytes (ionic substances), uremic substances, and other proteins. Therefore, the adsorbent material containing the above two-dimensional particles can adsorb a variety of adsorbates, and it is expected to be used in adsorption sheets, separation membranes, and artificial dialysis machines using the adsorbent material.
[0355] Comparative Examples 1 to 3 do not contain the specified two-dimensional particles, and the results of the adsorption test confirmed that the adsorbate was limited. In particular, no adsorption of Na + , K + , P and other electrolytes.
[0356] This disclosure includes the following:
[0357] <1>
[0358] An adsorbent material for adsorbing pathogenic substances, comprising two-dimensional particles having one or more layers,
[0359] The layer comprises the following formula:
[0360] M m X n
[0361] (wherein, M is at least one metal of Group 3, 4, 5, 6, or 7,
[0362] X is a carbon atom, a nitrogen atom or a combination thereof,
[0363] n is greater than or equal to 1 and less than or equal to 4,
[0364] m is greater than n and less than 5)
[0365] The layer body represented by the invention and the modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom and a hydrogen atom) present on the surface of the layer body.
[0366] <2>
[0367] according to <1> The adsorption material, wherein the pathogenic substance contains protein.
[0368] <3>
[0369] according to <1> or <2> The adsorption material, wherein the pathogenic substance comprises uremic protein.
[0370] <4>
[0371] according to <3> The adsorption material, wherein the uremic substance comprises β2-microglobulin.
[0372] <5>
[0373] according to <1> ~ <4> The adsorption material according to any one of the preceding claims, wherein the pathogenic substance comprises a cytokine.
[0374] <6>
[0375] according to <5> The adsorption material, wherein the cytokine comprises at least one selected from the group consisting of interleukins, interferons, chemokines, hematopoietic factors, cell growth factors and tumor necrosis factors.
[0376] <7>
[0377] according to <1> ~ <6> The adsorbent material described in any one of the preceding claims, wherein the pathogenic substance contains an electrolyte.
[0378] <8>
[0379] according to <7> The adsorption material, wherein the electrolyte comprises a + , K + Mg 2+ , Ca 2+ and PO4 3- At least one of the group consisting of.
[0380] <9>
[0381] An adsorption sheet comprising <1> ~ <8> The adsorbent material described above.
[0382] <10>
[0383] A separation membrane comprising <1> ~ <8> The adsorbent material described above.
[0384] <11>
[0385] Artificial dialysis machine, comprising <1> ~ <8> The adsorbent material described above.
[0386] <12>
[0387] A method for manufacturing an adsorbent material for adsorbing pathogenic substances, comprising:
[0388] (a) preparing a specified precursor; and
[0389] (b) removing at least a portion of the A atoms from the precursor using an etching solution, thereby obtaining an etched product;
[0390] (c) cleaning the etched product to obtain an etched and cleaned product;
[0391] The etching and cleaning product is used as two-dimensional particles to obtain an adsorbent material.
[0392] Explanation of symbols
[0393] 1a, 1b: Layer main body (M m X n layer)
[0394] 3a, 5a, 3b, 5b: Modified or terminal T
[0395] 7a, 7b: MXene layer
[0396] 10a, 10b: MXene particles (particles of layered materials)
[0397] 40: Hemodialysis machine
[0398] 41, 41A: Blood inlet
[0399] 42, 42A: Blood outlet
[0400] 43, 43A: Blood pump
[0401] 44, 44A: Blood purification machine
[0402] 45, 45A: Separation membrane
[0403] 46, 46A: Blood passing area of blood purification machine
[0404] 47, 47A: Dialysate passing area of blood purification machine
[0405] 48, 48A: Unused dialysate tank
[0406] 49, 49A: Used dialysis fluid box
[0407] 50, 50A: Dialysis fluid pump
[0408] 51: Semipermeable membrane
Claims
1. An adsorbent material for adsorbing pathogenic substances, comprising 2-dimensional particles having one or more layers, The layer comprises the following formula: M m X n (wherein, M is at least one metal of Group 3, 4, 5, 6, or 7, X is a carbon atom, a nitrogen atom or a combination thereof, n is greater than or equal to 1 and less than or equal to 4, m is greater than n and less than 5) The layer body represented by the invention and the modification or termination T (T is at least one selected from the group consisting of a hydroxyl group, a fluorine atom, a chlorine atom, an oxygen atom and a hydrogen atom) present on the surface of the layer body.
2. The adsorbent material according to claim 1, wherein The pathogenic substance comprises protein.
3. The adsorbent material according to claim 1 or 2, wherein The pathogenic substance includes a uremic substance having a molecular weight of 100 or more.
4. The adsorbent material according to claim 3, wherein The uremic substances include β2-microglobulin.
5. The adsorbent material according to any one of claims 1 to 4, wherein The pathogenic substances include cytokines.
6. The adsorbent material according to claim 5, wherein The cytokine comprises at least one selected from the group consisting of interleukins, interferons, chemokines, hematopoietic factors, cell growth factors and tumor necrosis factors.
7. The adsorbent material according to any one of claims 1 to 6, wherein The pathogenic substances include electrolytes.
8. The adsorbent material according to claim 7, wherein The electrolyte comprises a member selected from the group consisting of Na + , K + Mg 2+ , Ca 2+ and PO4 3- At least one of the group consisting of.
9. An adsorption sheet comprising the adsorption material according to any one of claims 1 to 8.
10. A separation membrane comprising the adsorption material according to any one of claims 1 to 8.
11. An artificial dialysis machine comprising the adsorption material according to any one of claims 1 to 8.
12. A method for producing an adsorbent material for adsorbing pathogenic substances, comprising: (a) preparing a specified precursor; and (b) removing at least a portion of the A atoms from the precursor using an etching solution, thereby obtaining an etched product; (c) cleaning the etched product to obtain an etched and cleaned product; The etching and cleaning product is used as two-dimensional particles to obtain an adsorbent material.