Polymer, resin additive, resin composition, and molded article
By introducing core-shell structure polymer A prepared by the (meth)acrylate monomer and emulsion polymerization method as a resin additive in a polyester-based polymer, polybutylene terephthalate resin and polystyrene resin are solved. The problem of insufficient compatibility improves the compatibility of the resin composite and the tensile elongation of the molded body, and improves performance and toughness.
Patent Information
- Application Number
- CN202380034212.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-19
- Filing Date
- 2023-04-18
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, the degree of improvement in compatibility between the polybutylene terephthalate resin and the polystyrene resin is insufficient, resulting in a decrease in the composite performance.
A polymer is used, which consists of a polyester-based polymer and a second polymer having different structural units. The second polymer part contains (meth)acrylate monomers and is prepared by emulsion polymerization to form a core-shell structure. The polymer A is used as a resin additive to improve the compatibility of the resin and the tensile elongation of the molded body.
It effectively improves the compatibility of various resins, reduces phase separation, improves the tensile elongation and toughness of the molded body, and enhances the industrial utilization value.
Smart Images

Figure BDA0005084764150000131 
Figure BDA0005084764150000141 
Figure HDA0005084764160000011
Abstract
Description
Technical Field
[0001] The present invention relates to a polymer, a resin additive, a resin composition and a molded body. Background Art
[0002] In the past, attempts have been made to mix multiple resins to achieve functional performance or performance improvement that cannot be achieved by a single resin. However, the combination of multiple resin types will show incompatibility, so the performance or function obtained by compounding is often lower than that of a single resin. Therefore, in order to improve the compatibility of multiple resin types, the operation of adding a compatibilizer is carried out.
[0003] Patent Document 1 discloses that polybutylene terephthalate resin, polystyrene resin, and carbon fiber have good low warpage and mechanical properties by using polycarbonate as a compatibilizing agent.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2020-176159 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, according to the research of the present inventors, it was found that the compatibilizer described in Patent Document 1 sometimes does not sufficiently improve the compatibility of polybutylene terephthalate resin and polystyrene resin. Therefore, an object of one embodiment of the present invention is to provide a polymer or the like which can improve the compatibility of a polyester resin represented by polybutylene terephthalate resin and other resins when compounded, and furthermore, can also provide a molded product having excellent tensile elongation.
[0009] Means for solving problems
[0010] One embodiment of the present invention is a polymer comprising a first polymer portion and a second polymer portion, wherein the first polymer portion is a polyester-based polymer, the second polymer portion has a structural unit different from a structural unit constituting the first polymer portion, the proportion of the first polymer in a total of 100 parts by mass of the first polymer portion and the second polymer portion is more than 20 parts by mass and less than 90 parts by mass, and the second polymer portion has a structural unit derived from a (meth)acrylate monomer.
[0011] Effects of the Invention
[0012] According to one embodiment of the present invention, it is possible to provide a polymer or the like which can improve the compatibility of resins and reduce phase separation when two or more resins are mixed, and also has excellent tensile elongation of a molded article. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] [ Figure 1 ] is a cross-sectional photograph of the molded body of Example 1 observed using a transmission electron microscope.
[0014] [ Figure 2 ] is a cross-sectional photograph of the molded body of Comparative Example 1 observed using a transmission electron microscope. DETAILED DESCRIPTION
[0015] Hereinafter, this embodiment will be described in detail. It should be noted that what is described below is one embodiment of the present invention, and the present invention is not limited to the following configuration. The polymer of this embodiment is a polymer (hereinafter sometimes referred to as polymer A) having a first polymer portion which is a polyester-based polymer and a second polymer portion which has a structural unit different from the structural unit constituting the above-mentioned first polymer portion. By using the polymer A as a resin additive for two or more base resins including a polyester resin, the compatibility of the first base resin and the second base resin can be improved. Therefore, the phase separation of the first base resin and the second base resin can be reduced.
[0016] <1. Polymer A>
[0017] The polymer A involved in this embodiment is a polymer having a first polymer part and a second polymer part, the first polymer part is a polyester polymer, the second polymer part has a structural unit different from the structural unit constituting the above-mentioned first polymer part, the proportion of the first polymer in the total of 100 parts by mass of the first polymer part and the second polymer part exceeds 20 parts by mass and is less than 90 parts by mass, and the second polymer part has a structural unit derived from a (meth)acrylate monomer. It should be noted that in one embodiment of the present invention, the polymer having the first polymer part and the second polymer part can be a polymer in which the first polymer part and the second polymer part are covalently bonded. In addition, in one embodiment of the present invention, even if the first polymer part and the second polymer part are not covalently bonded, a polymer in which the first polymer is enclosed or enclosed by the second polymer is included.
[0018] As a polymer covalently bonded to the first polymer part and the second polymer part, for example, a block copolymer having the first polymer part and the second polymer part can be cited. In addition, as a polymer in which the first polymer is enclosed or enclosed by the second polymer, a polymer having a core-shell structure can be cited, and the core-shell structure is a core-shell structure in which the core part includes a polymer part of one of the first polymer part and the second polymer part, and the shell part includes a polymer part of the other of the first polymer part and the second polymer part. It should be noted that the core-shell structure refers to a structure in which the part called the core is enclosed in the part called the shell.
[0019] Among them, the polymer A is preferably a polymer having a core-shell structure, and the first polymer part constitutes the shell part of the core-shell structure. That is, the polymer A is preferably a polymer in which the first polymer part, which is a polyester-based polymer, constitutes the shell part of the core-shell structure, and the second polymer part having a structural unit different from the structural unit constituting the first polymer part constitutes the core part. Hereinafter, as a representative example, a preferred embodiment of the polymer A having the core-shell structure is described in detail.
[0020] <1-1. First polymer portion>
[0021] As described above, the first polymer portion is composed of a polyester polymer. It should be noted that, in one embodiment of the present invention, a polyester polymer refers to a polymer composed of a structural unit containing an ester bond as a repeating unit, and polyester is synthesized by a polycondensation reaction of a dicarboxylic acid component and a diol component. Since the first polymer portion is composed of a polyester polymer, the affinity with the first matrix resin, which is a polyester resin, is improved, and as a result, the compatibility of the first matrix resin and the second matrix resin is improved.
[0022] The dicarboxylic acid is not particularly limited, and examples thereof include aromatic dicarboxylic acids, aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, and the like. Examples of the aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, 2,5-norbornane dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, 4,4-oxybenzoic acid, fumaric acid, maleic anhydride, succinic acid, glutaric acid, adipic acid, sebacic acid, dodecanedicarboxylic acid, tetrahydrophthalic anhydride, tetrahydroterephthalic acid, 5-sodium sulfoisophthalate, 5-lithium sulfoisophthalate, trimellitic acid (anhydride), and pyromellitic acid (anhydride).
[0023] The diol component is not particularly limited, and examples thereof include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, triethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, cyclohexanedimethanol, ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, ethylene oxide and propylene oxide adducts of bisphenol A, ethylene oxide and propylene oxide adducts of hydrogenated bisphenol A, polytetramethylene glycol, polyethylene glycol, polypropylene glycol and modified products thereof, sodium sulfobutylene glycol, and the like.
[0024] In addition, two or more dicarboxylic acid components may be used, and similarly, two or more diol components may be used.
[0025] It should be noted that the first polymer portion may be composed of a plurality of polymers each having a plurality of different structural units. In this case, the structural unit may be any of the structural units exemplified as the structural unit of the first polymer.
[0026] The mass average molecular weight of the first polymer part is not particularly limited, but for the handleability of the powder, it is preferably 3000 or more, more preferably 5000 or more, and particularly preferably 7000 or more. On the other hand, in order to suppress the increase in viscosity when the matrix resin is added, the mass average molecular weight is preferably 200000 or less, more preferably 100000 or less, and particularly preferably 50000 or less. It should be noted that the mass average molecular weight can be measured by gel permeation chromatography (GPC).
[0027] The glass transition temperature of the first polymer portion is not particularly limited, but is preferably 40° C. or higher, more preferably 45° C. or higher, and particularly preferably 50° C. or higher to ensure powder recyclability. On the other hand, in order to avoid micronization of the powder, the glass transition temperature is preferably 150° C. or lower, more preferably 130° C. or lower, and particularly preferably 100° C. or lower.
[0028] <1-2. Second polymer portion>
[0029] The second polymer portion has a structural unit different from the structural unit constituting the first polymer portion. The second polymer portion has a structural unit derived from a (meth)acrylate monomer. By having a structural unit derived from a (meth)acrylate monomer, the tensile elongation of the molded body is improved. In addition, the second polymer portion preferably has a structural unit other than the structural unit derived from the (meth)acrylate monomer, and such a structural unit is preferably a component with excellent affinity with the second matrix resin. Specifically, it is preferred that at least a portion of the structural units of the second polymer portion is the same as at least a portion of the structural units constituting the above-mentioned second matrix resin.
[0030] Regarding the structural unit derived from the (meth)acrylate monomer constituting the second polymer part, examples of the (meth)acrylate monomer include methyl methacrylate, ethyl methacrylate, methyl acrylate, ethyl acrylate, butyl acrylate, butyl methacrylate, propyl acrylate, 2-ethylhexyl acrylate, glycidyl acrylate, propyl methacrylate, 2-ethylhexyl methacrylate, glycidyl methacrylate, phenyl acrylate, phenyl methacrylate, hydroxyethyl acrylate, 4-hydroxybutyl acrylate, benzyl acrylate, benzyl methacrylate, polyalkylene glycol monoacrylate, or polyalkylene glycol monomethacrylate. Among them, methyl methacrylate, butyl acrylate, glycidyl methacrylate, or polyalkylene glycol monomethacrylate is preferred from the viewpoint of tensile elongation of the molded article.
[0031] The proportion of the structural unit derived from the (meth)acrylate monomer in all structural units constituting the second polymer portion is not particularly limited, but is preferably 5 parts by mass or more, and 80 parts by mass or less, in order to further improve the compatibility of the first matrix resin and the second matrix resin and to further improve the tensile elongation of the molded article. More preferably, it is 8 parts by mass or more and 60 parts by mass or less.
[0032] As a structural unit constituting the second polymer part other than the structural unit derived from the (meth)acrylate monomer, it is preferably set according to the structure of the second base resin used, and for example, a structural unit derived from an aromatic vinyl monomer can be cited. In the case where the structural unit constituting the second polymer part contains a structural unit derived from an aromatic vinyl monomer, for example, when a polystyrene-containing resin is used as the second base resin, the affinity of the second polymer part and the polystyrene-containing resin becomes good, and as a result, it can be expected that the compatibility of the first base resin and the second base resin becomes better. Among them, as a structural unit constituting the second polymer part, a structural unit derived from an aromatic vinyl monomer having a monocyclic structure of a 6-membered ring is more preferred, and a structural unit derived from styrene that may have a substituent is further preferred. As a structural unit derived from styrene that may have a substituent, a structural unit derived from styrene or a structural unit derived from α-methylstyrene can be cited, among which a structural unit derived from styrene is particularly preferred.
[0033] Among all the structural units of the second polymer part, the proportion of the structural units derived from the aromatic vinyl monomer is not particularly limited. In order to further improve the compatibility between the first matrix resin and the second matrix resin, it is preferably 30 parts by mass or more, more preferably 50 parts by mass or more, further preferably 60 parts by mass or more, and particularly preferably 70 parts by mass or more. On the other hand, it is preferably 95 parts by mass or less and less than 100 parts by mass.
[0034] The second polymer portion may further have other structural units. The proportion of other structural units in all structural units of the second polymer portion is not particularly limited, but in order to further improve the compatibility of the first matrix resin and the second matrix resin, it is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and particularly preferably 20 parts by mass or less, and on the other hand, it is 0 parts by mass or more.
[0035] It should be noted that the second polymer portion may be composed of a plurality of polymers having a plurality of different structural units. In this case, the structural unit may be any of the structural units exemplified as the structural unit of the second polymer.
[0036] In order to further improve the compatibility of the first matrix resin and the second matrix resin when the polymer A is added as a resin additive to the first matrix resin and the second matrix resin, the proportion of the first polymer in the total 100 parts by mass of the first polymer part and the second polymer part is preferably more than 20 parts by mass and less than 90 parts by mass. More preferably, it is more than 20 parts by mass and less than 80 parts by mass, further preferably, it is more than 20 parts by mass and less than 70 parts by mass, further preferably, it is more than 20 parts by mass and less than 60 parts by mass, further preferably, it is more than 20 parts by mass and less than 50 parts by mass, further preferably, it is more than 20 parts by mass and less than 45 parts by mass, and particularly preferably, it is more than 20 parts by mass and less than 40 parts by mass.
[0037] <1-3. Method for producing polymer A>
[0038] The manufacturing method of polymer A when having a core-shell structure is not particularly limited, and it can be manufactured by known methods such as suspension polymerization, solution polymerization or emulsion polymerization. Among them, from the viewpoint of ease of manufacture, it is preferably manufactured by emulsion polymerization. That is, polymer A is preferably a polymer obtained by emulsion polymerization of the monomer components constituting the second polymer part in the presence of the polymer constituting the first polymer part finally obtained. It should be noted that when performing emulsion polymerization, it can be carried out by adding the monomer components together and polymerizing them, or it can be carried out by dropwise polymerization added in stages.
[0039] More specifically, the monomer components constituting the second polymer are added to a solution prepared by dispersing the polymer constituting the first polymer part in an arbitrary solvent, emulsified using various mixers, and a polymerization initiator is added to carry out polymerization.
[0040] The solution formed by dispersing the first polymer in any solvent can be obtained by, for example, adding the polymer constituting the first polymer part to one or more solvents such as water, isopropanol, ethanol, methanol, etc., acetone, methyl ethyl ketone, diethyl ether, etc., and stirring while applying shear. From the aspect of excellent dispersibility, the proportion of the first polymer in the dispersed solution is preferably 10% by mass or more, and from the viewpoint of operability considering the viscosity of the dispersed solution, it is preferably 50% by mass or less.
[0041] When the monomer components constituting the second polymer part are added to the solution formed by dispersing the polymer constituting the first polymer part in an arbitrary solvent, a surfactant may be further added. Examples of the surfactant include anionic surfactants, cationic surfactants, and neutral surfactants. More than one of these may be used.
[0042] The polymerization initiator may be a polymerization initiator generally used for free radical polymerization. Specific examples thereof include persulfates such as potassium persulfate, sodium persulfate, and ammonium persulfate, oil-soluble azo compounds such as azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile, 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,2'-azobis{2-methyl-N-[2-(1-hydroxyethyl)]propionamide}, and 2,2'-azobis{2- Water-soluble azo compounds such as methyl-N-[2-(1-hydroxybutyl)propionamide}2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] and its salts, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] and its salts, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane} and its salts, 2,2'-azobis(2-methylpropionamidine) and its salts, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine], benzoyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, etc. The above polymerization initiators may be used alone or in combination of two or more.
[0043] Preferred radical polymerization methods in one embodiment of the present invention include, for example, a method of performing polymerization using a water-soluble polymerization initiator and a method of performing polymerization using a redox reaction of an organic peroxide and a reducing agent such as ferrous sulfate or isoascorbic acid.
[0044] The amount of the polymerization initiator used is preferably 0.05 to 1.0 parts by mass relative to a total of 100 parts by mass of the monomers constituting the second polymer, and more preferably the lower limit is 0.1 parts by mass or more and the upper limit is 0.3 parts by mass or less. It should be noted that when a peroxide-based polymerization initiator is used, it can be combined with a reducing agent and used as a redox-based polymerization initiator. The amount of the reducing agent used is preferably 0.0001 to 1 parts by mass relative to a total of 100 parts by mass of the monomers constituting the second polymer.
[0045] In addition, as a molecular weight modifier, a known chain transfer agent such as n-dodecyl mercaptan, tert-dodecyl mercaptan, or α-methylstyrene dimer may be used to polymerize the monomer.
[0046] The reaction temperature is not particularly limited, but is usually 45° C. to 80° C. The reaction time is not particularly limited, but is usually 30 minutes to 300 minutes.
[0047] The latex of the polymer A obtained by emulsion polymerization can be dried or coagulated by spray drying or freeze drying to recover the polymer as powder. Among them, drying or coagulation by spray drying is preferred.
[0048] When drying by spray drying, it is preferred to spray the latex of polymer A onto fine droplets and blow hot air thereto for drying. As a device for generating droplets, any of a rotating disk type, a pressure nozzle type, a two-fluid nozzle type, etc. can be used.
[0049] When hot air is blown to dry the latex of polymer A, the hot air temperature is preferably 100° C. to 200° C. When the hot air temperature is 100° C. or higher, the latex can be dried sufficiently, and when the hot air temperature is 200° C. or lower, thermal decomposition of the obtained powder can be suppressed.
[0050] In the case of coagulation, the latex of polymer A is put into hot water in which a coagulant is dissolved, and polymer A is salted out, separated, refined, coagulated to form a wet state, and then dehydrated and dried. As the coagulant, for example, inorganic salts such as aluminum chloride, aluminum sulfate, sodium sulfate, magnesium sulfate, sodium nitrate, calcium acetate, or acids such as sulfuric acid can be cited, and calcium acetate is particularly preferred. These coagulants can be used alone or in combination of two or more. In the case of using in combination, it is preferred to select a combination that does not form an insoluble salt in water. For example, if calcium acetate and sulfuric acid or its sodium salt are used in combination, an insoluble calcium salt will be formed in water, so it is not preferred.
[0051] It should be noted that, depending on the manufacturing method of polymer A, the polymerization mode of the first polymer part and the second polymer part will change, which is common technical knowledge, but it is difficult to determine what polymerization mode will be used. For example, it is believed that the polymerization mode of polymer A obtained by emulsion polymerization of the monomer components constituting the second polymer part in the presence of the polymer constituting the first polymer part will change compared with polymer A obtained by other methods, and there will be differences in structure or characteristics. However, it is technically impossible or basically impractical to determine the structure or characteristics in order to make such a difference clear.
[0052] [Resin additives]
[0053] Polymer A can be used as a resin additive such as a compatibilizer. It should be noted that the resin additive can be directly polymer A, or it can be mixed with any auxiliary agent. As auxiliary agents, known auxiliary agents can be mentioned, for example, flame retardants, anti-drip agents, antioxidants, ultraviolet absorbers, light stabilizers, mold release agents, lubricants, sliding agents, colorants, fluorescent brighteners, light-storing pigments, fluorescent dyes, antistatic agents, etc.
[0054] <2. Resin composition>
[0055] The resin composition of the present embodiment includes polymer A and a first matrix resin. In addition, the resin composition may further include a second matrix resin that is a resin different from the first matrix resin. The proportion of polymer A relative to a total of 100 parts by mass of the first matrix resin and the second matrix resin is not particularly limited, and is preferably 0.1 to 30 parts by mass, and more preferably 5 to 20 parts by mass. If the proportion of the resin additive is 0.1 parts by mass or more, the compatibility of the first matrix resin and the second matrix resin is further improved, and if it is 30 parts by mass or less, the processability of the resin composition during manufacture is excellent.
[0056] The resin composition of the present embodiment may further include other components. For example, in order to impart functions or improve characteristics, known auxiliary agents may be added as needed. Examples of the auxiliary agents include flame retardants, anti-drip agents, antioxidants, ultraviolet absorbers, light stabilizers, mold release agents, lubricants, sliding agents, colorants, fluorescent brighteners, light-storing pigments, fluorescent dyes, antistatic agents, and the like.
[0057] <2-1. First Matrix Resin>
[0058] The first matrix resin is not particularly limited, and is preferably a polyester resin, for example, a resin comprising at least one of the group consisting of polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), polybutylene succinate (PBS), polyhydroxyalkanoic acid (PHA) and polylactic acid (PLA). In addition, they may also use recycled materials.
[0059] <2-2. Second Matrix Resin>
[0060] The second matrix resin is not particularly limited as long as it is a resin different from the first matrix resin. For example, it is a resin containing polystyrene. Polystyrene, high impact polystyrene (HIPS) and acrylonitrile-butadiene-styrene copolymer (ABS) and other polystyrene-containing resins can be used. In addition, they can also use recycled materials. From the viewpoint of improving compatibility, it is preferred that at least a part of the structural units constituting the second matrix resin is the same as at least a part of the structural units of the second polymer part in polymer A.
[0061] The proportion of the first matrix resin in 100 parts by mass of the total of the first matrix resin and the second matrix resin is not particularly limited, but is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, further preferably 20 parts by mass or more, and particularly preferably 25 parts by mass or more. On the other hand, the proportion of the first matrix resin is preferably 95 parts by mass or less, more preferably 90 parts by mass or less, further preferably 80 parts by mass or less, and particularly preferably 75 parts by mass or less.
[0062] <2-3. Method for producing resin composition>
[0063] The method for producing the resin composition is not particularly limited, and the resin composition can be produced by mixing or melt-kneading the polymer A, the first matrix resin, and the second matrix resin in the form of powders. For the mixing or melt-kneading, for example, a Henschel mixer, a Banbury mixer, a single-screw extruder, a twin-screw extruder, a twin-roller, a kneader, a Brabender, etc. are used.
[0064] <3. Molded body>
[0065] The resin combination of the present embodiment can be processed into a molded body. In addition, the resin combination of the present embodiment can also be processed into a molded body after being mixed with other materials. That is, the molded body can contain the resin combination. It should be noted that, as a molding method, known methods can be used, for example, compression molding, transfer molding, injection molding, blow molding, vacuum molding, extrusion molding, stacking molding, calendering molding can be cited.
[0066] <4. Conclusion>
[0067] As described above, the present invention has the following aspects.
[0068] [1] A polymer comprising a first polymer portion and a second polymer portion, wherein the first polymer portion is a polyester-based polymer, the second polymer portion has a structural unit different from a structural unit constituting the first polymer portion, the proportion of the first polymer in a total of 100 parts by mass of the first polymer portion and the second polymer portion is more than 20 parts by mass and less than 90 parts by mass, and the second polymer portion has a structural unit derived from a (meth)acrylate monomer.
[0069] [2] The polymer according to [1], wherein the ratio of the structural unit derived from the (meth)acrylic acid ester monomer in all structural units constituting the second polymer part is 5 parts by mass or more.
[0070] [3] The polymer according to claim [1] or [2], wherein the second polymer portion further has a structural unit derived from an aromatic vinyl monomer.
[0071] [4] The polymer according to [3], wherein a ratio of the structural unit derived from the aromatic vinyl monomer in all structural units constituting the second polymer portion is 30 parts by mass or more and 95 parts by mass or less.
[0072] [5] The polymer according to any one of [1] to [4], which has a core-shell structure, wherein the first polymer portion constitutes a shell portion of the core-shell structure, and the second polymer portion constitutes a core portion of the core-shell structure.
[0073] [6] The polymer according to any one of [1] to [5], obtained by emulsion polymerization of the monomer components constituting the second polymer part in the presence of the polymer constituting the first polymer part.
[0074] [7] A resin additive comprising the polymer described in any one of [1] to [6].
[0075] [8] A resin composition comprising the polymer described in any one of [1] to [6] and a polyester resin as a first matrix resin.
[0076] [9] The resin composition according to [8], further comprising a second matrix resin, wherein the second matrix resin is a resin different from the first matrix resin.
[0077]
[10] The resin composition according to [9], wherein the second matrix resin is a resin containing polystyrene.
[0078]
[11] A resin composition comprising the polymer described in [1], [5] or [6], a polyester resin as a first matrix resin, and a second matrix resin as a resin different from the first matrix resin, wherein at least a part of the structural units of the second polymer part are the same as at least a part of the structural units constituting the second matrix resin.
[0079]
[12] A molded article comprising the resin composition according to any one of [8] to
[11] .
[0080] Example
[0081] One embodiment of the present invention is described below by way of examples. In the examples, "parts" means "parts by mass".
[0082] <Tensile elastic modulus, tensile elongation>
[0083] A tensile test was conducted in accordance with JIS K7139 using a Tensilon universal testing machine (model name: "RTC-1250A-PL", manufactured by ORIENTEC Corporation) to measure the tensile modulus and tensile elongation of the molded article.
[0084] <Phase size>
[0085] A transmission electron microscope (TEM) (model name "H-7600", manufactured by Hitachi) was used to observe the phase size of a portion of the molded body. The test piece was stained with osmium tetroxide for 12 hours and then stained with ruthenium tetroxide for 5 hours to make an observation section. The average diameter of the long-axis portion of any 30 dispersed phases in the TEM photo was obtained as the phase size.
[0086] (Production Example 1)
[0087] 240 parts of Nichigo Polyester WR-905 (manufactured by Mitsubishi Chemical Corporation: solid content 20%) as an aqueous dispersion solution of the polymer constituting the first polymer part, 90 parts of styrene (St) as a free radical polymerizable monomer, and 10 parts of glycidyl methacrylate (GMA) were added, and emulsified using a homomixer to obtain a pre-emulsion of the free radical polymerizable monomer.
[0088] Add the pre-emulsion and 222 parts of deionized water to a flask equipped with a stirrer, a reflux cooling tube, and a temperature control device, and heat to 50°C while bubbling nitrogen at a flow rate of 200 ml per minute, and keep it for 1 hour. Add 0.7 parts of PERCUMYL P (manufactured by NOF Corporation) as a polymerization initiator, 0.002 parts of ferrous sulfate as a reducing agent, 0.006 parts of sodium ethylenediaminetetraacetate (EDTA), 0.3 parts of sodium formaldehyde sulfoxylate, and 10 parts of deionized water, switch to nitrogen flow, and initiate polymerization. After 1 hour, heat to 60°C, keep for 2 hours, and cool to obtain a latex of polymer A1 of one embodiment of the present invention. The obtained polymer A1 latex is added to 460 parts of deionized water added with 5 parts by mass of calcium acetate for coagulation, washed with water, dehydrated, and dried to obtain polymer A1 in the form of powder.
[0089] (Production Examples 2 to 9)
[0090] The amount of the first polymer portion used, the type of radical polymerizable monomer, and the copolymerization amount are changed according to the following Table 1. Except for this, polymers A2 to A6 of one embodiment of the present invention and polymers B1 to B3 of the comparative example are obtained by the same preparation method as in Preparation Example 1. As the radical polymerizable monomer, one or two (meth)acrylates are used. In Table 1, the two (meth)acrylates are marked as "a1" and "a2", respectively. In Preparation Examples 2 to 7, as the radical polymerizable monomer, at least any one of glycidyl methacrylate (GMA), butyl acrylate (BA), methyl methacrylate (MMA) and polypropylene glycol monomethacrylate (Blemmer PP-800 manufactured by NOF Corporation) is used.
[0091] <Polymerization Stability>
[0092] As the polymerization stability of each polymer, if the radical polymerizable monomer remained in an emulsified state due to the first polymer throughout the polymerization process, it was evaluated as "suitable", and if it separated, it was evaluated as "unsuitable".
[0093] (Example 1)
[0094] 70 parts of polybutylene terephthalate (PBT, manufactured by Mitsubishi Engineering-Plastics Corporation: NOVADURAN 5010R) as the first matrix resin, 30 parts of polystyrene (PS, manufactured by Toyo Styrol Co., Ltd.: ToyoStyrol GP200) as the second matrix resin, and 10 parts of polymer A1 manufactured in Manufacturing Example 1 were placed in a polyethylene bag. The polyethylene bag was shaken thoroughly by hand and mixed manually, and then melt-kneaded at 250° C. using a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., trade name: TEM35B), and the extruded strands were cut to obtain pellets. The obtained pellets were molded using an injection molding machine (manufactured by Toshiba Machine Co., Ltd., trade name: IS100EN) at a molding temperature of 250° C. and a mold temperature of 60° C. to manufacture a dumbbell-shaped molded body in accordance with JIS K7139, thereby obtaining a molded body of Example 1. The molded body was subjected to cross-sectional observation using a transmission electron microscope (TEM) and a tensile test. The TEM photograph of the cross section of the molded body is shown in Figure 1 The average diameter of the major axis portion of any 30 dispersed phases in the TEM photograph was 0.58 μm. The tensile modulus of the molded body in a tensile test was 2.2 GPa, and the tensile elongation was 3.1%.
[0095] (Examples 2 to 8)
[0096] A molded article was obtained and evaluated in the same manner as in Example 1 except that the second matrix resin was changed to high-impact polystyrene (HIPS, manufactured by Toyo Styrene: Toyo Styrol H350), or the ratio of the first matrix resin to the second matrix resin, the type of polymer used, and the amount added were changed as shown in Table 2 below.
[0097] (Comparative Example 1)
[0098] A resin composition and a molded body were prepared by the same method as in Example 1 except that the polymer A1 obtained in Preparation Example 1 was not added, thereby obtaining a molded body of Comparative Example 1. The molded body was subjected to cross-sectional observation and tensile testing using TEM. A TEM photograph of the cross-sectional area of the molded body is shown in Figure 2 The average diameter of the major axis portion of any 30 dispersed phases in the TEM photograph was 1.01 μm. The tensile modulus of the molded body in a tensile test was 2.1 GPa, and the tensile elongation was 2.9%.
[0099] (Comparative Examples 2 to 7)
[0100] Molded articles were obtained and evaluated in the same manner as in Example 1 except that the second matrix resin was changed to high-impact polystyrene (HIPS, manufactured by Toyo Styrene: Toyo Styrol H350), or the presence or absence of polymer addition, the type of polymer used, and the amount of polymer added were changed as shown in Table 2 below.
[0101] [Table 1]
[0102]
[0103] [Table 2]
[0104]
[0105] From the above results, it can be seen that when the ratio of the first matrix resin to the second matrix resin is 70 / 30 (first matrix resin / second matrix resin), the average diameter of the dispersed phase in Example 1 using the polymer of one embodiment of the present invention is greatly reduced relative to Comparative Example 1 in which the polymer of one embodiment of the present invention is not used. In addition, when Comparative Example 1 is set to 100%, the tensile elongation of the molded body is increased by 7%. In addition, it can be seen that, relative to Comparative Example 1, when the polymer of one embodiment of the present invention is used, the average diameter of the dispersed phase and the tensile elongation of the molded body are also improved in Examples 4 and 6. From the above results, it can be seen that by using the polymer of one embodiment of the present invention as a resin additive, the compatibility of the first matrix resin and the second matrix resin and the tensile elongation of the molded body are improved. By improving the tensile elongation, the toughness of the molded body becomes good, so the industrial utilization value is high.
[0106] It was also confirmed that the average diameter of the dispersed phase in Example 2 in which the proportion of the first polymer part was sufficient was smaller than that in Comparative Example 5 in which the polymer in which the proportion of the first polymer part was small was used, and when Comparative Example 5 was set to 100%, the tensile elongation of the molded body was also improved by 3%. It can be seen that in Comparative Example 4 in which the polymer in which the proportion of the first polymer part was small was used and in Example 7 in which the proportion of the first polymer part was sufficient, the average diameter of the dispersed phase and the tensile elongation of the molded body were also improved. From the above results, it can be seen that by using a polymer of one embodiment of the present invention as a resin additive, the compatibility between the first matrix resin and the second matrix resin and the tensile elongation of the molded body are improved. By improving the tensile elongation, the toughness of the molded body becomes good, so the industrial utilization value is high.
[0107] Furthermore, it was confirmed that the average diameter of the dispersed phase in Examples 2, 5 and 7 containing a (meth)acrylate monomer in the second polymer portion was smaller than that in Comparative Example 6 using a polymer without a (meth)acrylate monomer in the second polymer portion, and the tensile elongation of the molded body was improved. It was confirmed that in Examples 2, 5 and 7, when the tensile elongation of Comparative Example 6 was set to 100%, the tensile elongation was improved by 20%, 44% and 96%, respectively. From the above results, it can be seen that by using a polymer of one embodiment of the present invention as a resin additive, the compatibility between the first matrix resin and the second matrix resin and the tensile elongation of the molded body are improved. By improving the tensile elongation, the toughness of the molded body is improved, so the industrial utilization value is high.
[0108] It can be seen that in Example 3 where the ratio of the first matrix resin to the second matrix resin is 90 / 10 (first matrix resin / second matrix resin), the average diameter of the dispersed phase is greatly reduced compared to Comparative Example 2 where the polymer of one embodiment of the present invention is not used, and when Comparative Example 2 is set to 100%, the tensile elongation of the molded body is increased by 29%. From the above results, it can be seen that by using the polymer of one embodiment of the present invention as a resin additive, the compatibility of the first matrix resin and the second matrix resin and the tensile elongation of the molded body are improved. By improving the tensile elongation, the toughness of the molded body is improved, so the industrial utilization value is high.
[0109] It can be seen that in Example 8 in which HIPS is used in the second matrix resin, the average diameter of the dispersed phase is significantly smaller than that of Comparative Example 3 in which the polymer of one embodiment of the present invention is not used, and the tensile elongation of the molded body is increased by 14% when Comparative Example 3 is set as 100%. From the above results, it can be seen that by using the polymer of one embodiment of the present invention as a resin additive, the compatibility of the first matrix resin and the second matrix resin and the tensile elongation of the molded body are improved. By improving the tensile elongation, the toughness of the molded body is improved, so the industrial utilization value is high.
[0110] In Comparative Example 7 using a polymer having no second polymer part, the polymer had poor polymerizability stability and the tensile elongation of the molded article was inferior to that of Comparative Example 1 having no polymer, and thus the industrial applicability was poor.
[0111] Possibility of Industrial Application
[0112] The polymer according to one embodiment of the present invention can reduce phase separation of resins when two or more resins are mixed, and can be suitably used as a compatibilizer having excellent tensile elongation when a resin composition containing the polymer is formed into a molded article.
Claims
1. A polymer having a first polymer portion and a second polymer portion, The first polymer portion is a polyester-based polymer, and the second polymer portion has a structural unit different from a structural unit constituting the first polymer portion. In 100 parts by mass of the total of the first polymer part and the second polymer part, the proportion of the first polymer part is more than 20 parts by mass and less than 90 parts by mass, The second polymer portion has a structural unit derived from a (meth)acrylate monomer. 2 . The polymer according to claim 1 , wherein a ratio of the structural unit derived from the (meth)acrylic acid ester monomer in all structural units constituting the second polymer portion is 5 parts by mass or more. 3 . The polymer according to claim 1 , wherein the second polymer portion further comprises a structural unit derived from an aromatic vinyl monomer. 4 . The polymer according to claim 3 , wherein a ratio of the structural unit derived from the aromatic vinyl monomer in all structural units constituting the second polymer portion is 30 parts by mass or more and 95 parts by mass or less.
5. The polymer according to claim 1, which has a core-shell structure, The first polymer portion constitutes the shell portion of the core-shell structure, The second polymer portion constitutes the core portion of the core-shell structure. 6 . The polymer according to claim 1 , which is obtained by emulsion polymerization of monomer components constituting the second polymer portion in the presence of the polymer constituting the first polymer portion. 7 . A resin additive comprising the polymer according to claim 1 .
8. A resin composition comprising the polymer according to claim 1 and a polyester resin as a first base resin. 9 . The resin composition according to claim 8 , further comprising a second base resin, the second base resin being a resin different from the first base resin. 10 . The resin composition according to claim 9 , wherein the second base resin is a resin containing polystyrene.
11. A resin composition comprising: the polymer according to claim 1, a polyester resin as a first matrix resin, and a second matrix resin as a resin different from the first matrix resin, At least a part of structural units of the second polymer portion is identical to at least a part of structural units constituting the second base resin. 12 . A molded product comprising the resin composition according to claim 8 .