Plastic material and shaped article obtained therefrom

By rationally preparing inorganic particles and polymer compositions in plastic materials, the problem of electromagnetic wave transmission attenuation in radar detection systems is solved, low attenuation transmission of radar frequency is achieved, suitable for components such as vehicle bumpers, and improved the performance of the radar system .

CN119032129APending Publication Date: 2024-11-26BASELL POLIOLEFINE ITALIA SRL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034022.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-09
Filing Date
2023-04-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing plastic materials are severely attenuated by electromagnetic waves due to transmission losses in radar detection systems, making it difficult to meet the radar transparency requirements, especially in structural components such as vehicle bumpers.

Method used

Using plastic materials containing up to 7.0% by weight of inorganic particles and at least 93.0% by weight of polymer composition ensures that molded articles with thicknesses ranging from 0.5 mm to 20 mm meet specific equations when electromagnetic wave transmission in the frequency range of 1 GHz to 300 GHz , realize the transparency of electromagnetic waves.

Benefits of technology

It realizes low attenuation transmission of radar frequency and other electromagnetic waves, and is suitable for coverage and shielding of radar detection systems, improving the performance and reliability of radar systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005082789200000021
    Figure BDA0005082789200000021
  • Figure BDA0005082789200000081
    Figure BDA0005082789200000081
  • Figure BDA0005082789200000091
    Figure BDA0005082789200000091
Patent Text Reader

Abstract

The present disclosure relates to a molded article comprising a plastic material comprising inorganic particles (M) containing a metal element and a polymer composition (A) wherein the molded article makes attenuation of electromagnetic waves passing therethrough very low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a plastic material and shaped articles obtainable therefrom. Background Art

[0002] The future of mobility will increasingly be based on autonomous or driverless vehicles. Autonomous vehicles use sensors to perceive their environment and can drive safely with little or no human input. The most common sensors are camera- or radar-based systems. Radar technology has been used by automakers for years to assist with automatic cruise control and parking, and the same technology, combined with artificial intelligence, will soon be used in driverless vehicles.

[0003] In a radar system, a transmitter generates electromagnetic waves at radio or microwave frequencies that are emitted by a transmitting antenna. The emitted electromagnetic waves are reflected by radar-opaque objects and return to the receiver, providing information about the object's position and velocity, allowing the vehicle to navigate safely in the environment.

[0004] Currently, radar detection systems for unmanned vehicles use electromagnetic frequencies in the range from 76 GHz to 81 GHz. It is not ruled out that lower or higher frequencies will be used in the future.

[0005] In vehicles, radar detection systems are often embedded in or shielded by exterior trim, most often in the bumper. Radar transmission through plastic materials may be hampered by undesirable transmission losses, so the plastic material used to cover the radar detection system should be radar transparent, i.e., it should allow incident electromagnetic waves to pass through the covering with minimal or even no attenuation of the incident wave.

[0006] International patent application WO2022 / 011131 discloses a pigment having an aspect ratio of at least 5, the pigment comprising a non-conductive composite material comprising a semiconductor and / or a dielectric, and a metal dispersed in the semiconductor and / or the dielectric, wherein the pigment can be applied as a coating to a plastic object.

[0007] International patent application WO2021 / 030197 discloses a radar transparent TPO resin coated with a coating system, the coating system comprising a film-forming resin and a flake pigment composition, the flake pigment composition comprising 50 weight percent or more of a radar transmissive pigment and no more than 50 weight percent of a conductive pigment, wherein the coating system transmits at least 70% of electromagnetic radiation having a frequency of 1 GHz to 100 GHz.

[0008] In this context, there is a need for a plastic material that allows the transmission of electromagnetic waves (including but not limited to radar frequencies) with minimal or even no attenuation of the incident waves. The plastic material is suitable for producing molded articles, especially structural parts of molded articles, including but not limited to vehicle bumpers. Summary of the invention

[0009] The present disclosure provides a molded article comprising a plastic material, the material comprising up to and including 7.0 wt% of inorganic particles (M) containing a metal element and at least 93.0 wt% of a polymer composition (A), wherein a thickness d of the molded article ranges from 0.5 mm to 20 mm, and when the molded article is irradiated with an electromagnetic wave having a frequency of 1 GHz to 300 GHz, the thickness d satisfies equation (I),

[0010]

[0011] in

[0012] -d is the thickness of the molded product;

[0013] -λ0 is the vacuum wavelength corresponding to the frequency of the electromagnetic wave irradiating the molded article;

[0014] -ε r is the relative dielectric constant of the plastic material, and

[0015] -m is a positive integer equal to or greater than 1, and

[0016] The amounts of (A) and (M) are based on the total weight of the plastic material, and the total weight is 100%.

[0017] The present disclosure also provides for the use of a shaped article for at least partially covering a device for emitting and / or receiving electromagnetic waves, preferably a radar detection system.

[0018] The present disclosure also provides the use of a plastic material for optimizing the transmission and / or detection of electromagnetic waves having a frequency in the range from 1 GHz to 300 GHz through a shaped article having a thickness d in the range from 0.5 mm to 20 mm.

[0019] The plastic materials of the present disclosure and the shaped articles obtained therefrom allow for the transmission of electromagnetic waves, including but not limited to radar frequencies, with minimal or even no attenuation of the incident waves.

[0020] Thus, the shaped article of the present disclosure may be a cover or housing for an electromagnetic source and / or detector, such as a radome. The shaped article of the present disclosure may be a part of a vehicle, such as a bumper, that shields an electromagnetic transmitting and / or receiving device, such as a radar detection system.

[0021] The mechanical properties of the plastic material of the present disclosure are not substantially affected by the amount of inorganic particles (M) included in the plastic material.

[0022] Although multiple embodiments are disclosed, other embodiments will become apparent to those skilled in the art from the following detailed description. Obviously, certain embodiments as disclosed herein can be modified in various obvious aspects without departing from the spirit and scope of the claims presented herein. Therefore, the following detailed description should be regarded as illustrative in nature and not restrictive. DETAILED DESCRIPTION

[0023] In the context of this disclosure;

[0024] - Percentages are expressed by weight unless otherwise stated;

[0025] - unless otherwise stated, the total weight of the compositions adds up to 100%;

[0026] - the term "comprising" in relation to a polymer, plastic material, polymer composition, mixture or blend shall be interpreted as meaning "comprising or consisting essentially of";

[0027] - The term "consisting essentially of" means that in addition to the mandatory components, other components may also be present in the polymer or polymer composition, mixture or blend, provided that the basic characteristics of the polymer or composition, mixture or blend are not substantially affected by their presence. Examples of components that do not substantially affect the characteristics of the polymer or polyolefin composition, mixture or blend when present in conventional amounts are catalyst residues and processing aids;

[0028] - The term "copolymer" refers to a polymer derived from the polymerization of at least two comonomers, ie the term "copolymer" includes binary and ternary copolymers.

[0029] The plastic material preferably comprises or consists of 0.1 wt.% to 7.0 wt.%, more preferably 0.1 wt.% to 4.0 wt.%, still more preferably 0.5 wt.% to 4.0 wt.% of inorganic particles (M) and 93.0 wt.% to 99.9 wt.%, preferably 96.0 wt.% to 99.9 wt.%, more preferably 96.0 wt.% to 99.5 wt.% of the polymer composition (A), wherein the amounts of (M) and (A), calculated on the total weight of the plastic material, total weight being 100%.

[0030] In a preferred embodiment, the inorganic particles (M) are dispersed, more preferably uniformly dispersed in the polymer composition (A), similar to the inorganic particles (M) being embedded in a matrix consisting of the polymer composition (A).

[0031] In the following, the various components of the plastic material are defined in more detail.The various components may be included in the plastic material in any combination.

[0032] The polymer composition (A) preferably comprises up to and including 100 wt. % of at least one polymer (a), which is selected from the group consisting of propylene polymer (a1), ethylene polymer (a2), polybutene-1 (a3), polystyrene (a4), acrylic polymer (a5), acrylonitrile butadiene styrene polymer (a6), acrylonitrile styrene acrylate polymer (a7), polyamide (a8), polyester (a9), polyurethane (a10), polycarbonate (a11) and mixtures thereof, wherein the amount of polymer (a) is calculated by the weight of the polymer composition (A), and the total weight is 100%.

[0033] In one embodiment, the polymer composition (A) consists of at least one polymer (a).

[0034] The propylene polymer (a1) is preferably selected from the group consisting of:

[0035] (a1.1) Propylene homopolymer;

[0036] (a1.2) a propylene copolymer having at least one olefin of formula CH2=CHR, wherein R is hydrogen or a linear or branched C2-C8 alkyl group, the propylene copolymer preferably comprising up to and including 10.0 wt.-%, more preferably from 0.05 wt.-% to 10.0 wt.-%, still more preferably from 0.1 wt.-% to 8.0 wt.-%, based on the weight of (a1.2), of units derived from the olefin;

[0037] (a1.3) an elastomeric propylene copolymer with at least one olefin of formula CH2=CHR, wherein R is hydrogen or a linear or branched C2-C8 alkyl group, the elastomeric propylene copolymer preferably comprising up to and including 85 wt.-%, more preferably from 5 to 85 wt.-%, still more preferably from 20 to 70 wt.-%, based on the weight of (a1.3), of units derived from olefin;

[0038] (a1.4) recycled polypropylene (r-PP), which is waste plastic material derived from post-consumer and / or post-industrial waste; and

[0039] (a1.5) mixtures thereof.

[0040] In one embodiment the propylene copolymer (a1 ) is a heterophasic propylene copolymer comprising:

[0041] (1) up to and comprising 90 wt%, preferably 10 to 80 wt%, more preferably 15 to 70 wt%, of at least one propylene polymer selected from the group consisting of: propylene homopolymers, propylene copolymers having at least one olefin of formula CH2=CHR, wherein R is hydrogen or a linear or branched C2-C8 alkyl group, the propylene copolymers comprising up to and comprising 10.0 wt%, preferably 0.05 to 10.0 wt%, more preferably 0.1 to 8.0 wt%, based on the weight of (1), of units derived from olefins; and mixtures thereof;

[0042] (2) at least 10 wt.-%, preferably from 20 to 90 wt.-%, more preferably from 30 to 85 wt.-%, of an elastomeric propylene copolymer with at least one olefin of formula CH2=CHR, wherein R is hydrogen or a linear or branched C2-C8 alkyl group, the elastomeric propylene copolymer comprising up to and including 85 wt.-%, more preferably from 20 to 85 wt.-%, still more preferably from 25 to 75 wt.-%, based on the weight of (2), of units derived from an olefin,

[0043] The amounts of (1) and (2) are based on the total weight of (1) + (2).

[0044] In the propylene polymer (a1), the olefin is preferably selected from the group consisting of ethylene, butene-1, hexene-1, 4-methyl-1-pentene, octene-1 and combinations thereof, most preferably ethylene and butene-1.

[0045] The propylene polymer (a1) can be sold under the trade names Moplen, Hifax, Adstif, Clyrell, Softell, Hiflex (sold by LyondellBasell) or for example Vistamaxx. TM Vistamaxx 6102 (sold by Exxon Mobil) is commercially available.

[0046] The propylene polymer (a1) can be obtained by polymerizing the relevant monomers in the presence of a metallocene catalyst system or a highly stereospecific Ziegler-Natta catalyst system comprising:

[0047] (1) A solid catalyst component comprising a magnesium halide support and a stereoregular internal donor, on which a Ti compound having at least one Ti-halogen bond is present;

[0048] (2) optionally but preferably containing an Al promoter; and

[0049] (3) Optionally but preferably a further electron donor compound (external donor).

[0050] The solid catalyst component (1) preferably comprises TiCl4 in an amount ensuring the presence of 0.5 to 10 wt% Ti relative to the total weight of the solid catalyst component (1).

[0051] The solid catalyst component (1) comprises at least one stereoregular internal electron donor compound, which is selected from mono- or bidentate organic Lewis bases, preferably selected from esters, ketones, amines, amides, carbamates, carbonates, ethers, nitriles, alkoxysilanes and combinations thereof.

[0052] Preferred donors are esters of phthalic acid, such as those described in EP 45977 A2 and EP 395083 A2, in particular diisobutyl phthalate, di-n-butyl phthalate, di-n-octyl phthalate, diphenyl phthalate, benzyl butyl phthalate and combinations thereof.

[0053] The esters of aliphatic acids may also be selected from esters of malonic acid, such as those described in WO98 / 056830, WO98 / 056833, WO98 / 056834; esters of glutaric acid, such as those disclosed in WO00 / 55215; and esters of succinic acid, such as those disclosed in WO00 / 63261.

[0054] A specific type of diesters are those derived from the esterification of aliphatic or aromatic diols, such as those described in WO 2010 / 078494 and USP 7,388,061.

[0055] In some embodiments, the internal donor is selected from 1,3-diethers such as those described in EP361493, EP728769, and WO02 / 100904.

[0056] Internal donors, in particular specific mixtures of aliphatic or aromatic mono- or dicarboxylic acid esters and 1,3-diethers as disclosed in WO 07 / 57160 and WO 2011 / 061134, can be used as internal donors.

[0057] The preferred magnesium halide support is magnesium dihalide.

[0058] The amount of the internal donor to be held fixed on the solid catalyst component (1) is 5 mol% to 20 mol% relative to the magnesium dihalide.

[0059] A preferred process for preparing the solid catalyst component (1) is described in EP 395 083 A2.

[0060] The preparation of catalyst components according to general methods is described, for example, in European patent applications US 4,399,054, US 4,469,648, WO 98 / 44009 A1 and EP 395 083 A2.

[0061] In some embodiments, the catalyst system comprises an Al-containing co-catalyst (2), the Al-containing co-catalyst (2) being selected from Al-trialkyl, preferably selected from the group consisting of Al-triethyl, Al-triisobutyl and Al-tri-n-butyl. The Al / Ti weight ratio in the catalyst system is 1 to 1000, preferably 20 to 800.

[0062] In an embodiment, the catalyst system comprises an additional electron donor compound (3) selected from silicon compounds, ethers, esters, amines, heterocyclic compounds (particularly 2,2,6,6-tetramethylpiperidine), and ketones (external electron donor).

[0063] Preferred silicon compounds are selected from methylcyclohexyldimethoxysilane (C-donor), dicyclopentyldimethoxysilane (D-donor) and mixtures thereof.

[0064] The polymerization process to obtain the propylene polymer (a1) can be carried out continuously or batchwise in liquid phase or gas phase.

[0065] Liquid phase polymerisation can be slurry, solution or bulk (liquid monomer). The latter technique is most preferred and can be carried out in various types of reactors such as continuous stirred tank reactors, loop reactors or plug flow reactors.

[0066] The gas phase polymerization can be carried out in a fluidized bed or stirred fixed bed reactor or in a multizone circulation reactor, as described in EP1012195.

[0067] The heterophasic propylene polymers may be obtained by melt blending components (1) and (2) or preferably by polymerizing the relevant monomers in at least two polymerization stages, wherein the second and each subsequent polymerization stage is carried out in the presence of the produced polymer and the catalyst used in the immediately preceding polymerization stage or in a multizone circulation reactor as disclosed in WO2011 / 144489 and WO2018 / 177701.

[0068] The reaction temperature is preferably in the range from 40 to 90° C., and the polymerization pressure is preferably 3.3 to 4.3 MPa for the process in the liquid phase and 0.5 to 3.0 MPa for the process in the gas phase.

[0069] The ethylene polymer (a2) is preferably selected from the group consisting of:

[0070] (a2.1) Thermoplastic ethylene polymers, such as ultra-high molecular weight polyethylene (UHMWPE), high density polyethylene (HDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE);

[0071] (a2.2) having at least one compound of the formula CH2=CHR 1 Elastomeric ethylene copolymers of alpha-olefins, wherein R 1 is a linear or branched C1-C8 alkyl group, the elastomeric ethylene copolymer preferably comprising at least 20% by weight, more preferably from 20% to 50% by weight, based on the weight of (a2.2), of units derived from α-olefins;

[0072] (a2.3) recycled polyethylene (r-PE), which is waste plastic material derived from post-consumer and / or post-industrial waste; and

[0073] (a2.4) mixtures thereof.

[0074] In the ethylene polymer (a2), the α-olefin is preferably selected from propylene, butene-1, hexene-1, octene-1 and combinations thereof.

[0075] Ethylene polymers (a2.1) are commercially available, for example, under the trade names Alathon, Lucalen and Luflexen, sold by LyondellBasell, and can be prepared by known polymerization processes using Ziegler or Phillips catalysts in solution or in the gas phase.

[0076] Ethylene polymers (a2.2) can be obtained, for example, under the trade name Engage, such as Engage TM 8100 or Engage TM 8150 was purchased from are commercially available and can be obtained by known polymerization processes using metallocene-based catalyst systems.

[0077] The polybutene-1 (a3) ​​is preferably selected from the group consisting of butene-1 homopolymers, polybutene-1 having a monomer selected from ethylene and CH2=CHR 2 Butene-1 copolymer of at least one olefin of the group consisting of α-olefins (wherein R 2 is methyl or a linear or branched C3-C8 alkyl), and combinations thereof.

[0078] Ethylene and propylene are preferred comonomers in the butene-1 copolymer (a3). Preferably, ethylene and / or α-olefin is included in the butene-1 copolymer (a3) ​​in the range of 0.1 wt% to 20 wt% based on the weight of the butene-1 copolymer (a3).

[0079] Butene-1 polymers (a3) ​​are commercially available, for example, under the trade name Koattro, sold by LyondellBasell, and can be prepared by known polymerization processes (typically using solution polymerization) using Ziegler-Natta or metallocene-based catalyst systems.

[0080] The polystyrene (a4) is preferably selected from thermoplastic homopolymers of styrene or α-methylstyrene (a4.1), saturated or unsaturated styrene or α-methylstyrene block copolymers (a4.2) (which preferably comprise up to and including 30 wt. % polystyrene, more preferably 10 wt. % to 30 wt. % polystyrene, based on the weight of (a4.2)), recycled styrene block copolymers (r-SBC) (a4.3) (which are waste plastic materials derived from post-consumer and / or post-industrial waste); and mixtures thereof.

[0081] The saturated or unsaturated styrene or α-methylstyrene block copolymer (a4.2) is preferably selected from the group consisting of polystyrene-polybutadiene-polystyrene (SBS), polystyrene-poly(ethylene-butylene)-polystyrene (SEBS), polystyrene-poly(ethylene-propylene)-polystyrene (SEPS), polystyrene-polyisoprene-polystyrene (SIS), polystyrene-poly(isoprene-butadiene)-polystyrene (SIBS) and mixtures thereof.

[0082] Styrene and α-methylstyrene block copolymers (a4.2) are prepared by ionic polymerization of the relevant monomers and are available under the trade name Kraton TM Commercially available and sold by Kraton Polymers.

[0083] The acrylic polymer (a5) is preferably selected from the group consisting of poly(methacrylate) (PMA), poly(methyl methacrylate) (PMMA), poly(ethyl methacrylate) (PEMA), poly(2-hydroxyethyl methyl acrylate) (poly-HEMA) and mixtures thereof.

[0084] The polyamide (a8) is preferably selected from aliphatic polyamides, polyphthalamides, aromatic polyamides, polyamide-imides and mixtures thereof.

[0085] Among aliphatic polyamides, nylon PA6 and nylon PA66 are most preferred.

[0086] Polyamide (a8) is commercially available and can be produced by polycondensation processes well known in the art.

[0087] The polyester (a9) is preferably selected from the group consisting of polyethylene terephthalate (PET), ethylene glycol-modified polyethylene terephthalate (PETG), polybutylene terephthalate (PBT), polylactic acid (PLA), polyglycolic acid (PGA), polycaprolactone (PCL) and mixtures thereof.

[0088] Based on the total weight of polymer (a) (total weight is 100%), polymer (a) optionally includes a conventional amount (preferably up to and including 5.0 wt. %, more preferably 0.01 to 5.0 wt. %) of at least one additive selected from the group consisting of a nucleating agent, an antistatic agent, an antioxidant, a light stabilizer, a slip agent, an antacid, a melt stabilizer and a combination thereof.

[0089] In one embodiment, the polymer composition (A) comprises up to and including 50 wt %, preferably 2 to 50 wt %, of at least one additional component (b), the at least one additional component (b) being selected from the group consisting of fillers, pigments, flame retardants, compatibilizers and combinations thereof, wherein the amounts of (a) and (b) are calculated on the total weight of the polymer composition (A), and the total weight is 100%.

[0090] The filler is preferably selected from the group consisting of mineral fillers, preferably talc, mica, glass fibers, glass beads, carbon fibers, carbon black, natural fibers, carbon nanotubes, fullerenes, and combinations thereof.

[0091] Pigments and flame retardants are of the type used in the polyolefin field.

[0092] The compatibilizer is preferably a modified olefin polymer functionalized with a polar compound, preferably polypropylene and / or polyethylene. The modified olefin polymer is selected from graft copolymers, block copolymers and mixtures thereof. Preferably, the compatibilizer is a polyolefin functionalized with a compound selected from the group consisting of, more preferably selected from polyethylene, polypropylene and mixtures thereof: maleic anhydride, C1-C10 straight or branched maleic acid dialkyl esters, C1-C10 straight or branched fumaric acid dialkyl esters, itaconic anhydride, C1-C10 straight or branched itaconic acid, dialkyl esters, maleic acid, fumaric acid, itaconic acid and mixtures thereof. In a preferred embodiment, the compatibilizer is polyethylene and / or polypropylene (MAH-g-PP and / or MAH-g-PE) grafted with maleic anhydride.

[0093] An example of a modified polyolefin suitable for use as a compatibilizer is the commercial product Amplify TM TY, ExxonMobil Chemical Company's Exxelor TM、Byk (Altana Group) TPPP, Polyram Group and Chemtura and combinations thereof. The modified polymers can be produced by functionalization processes carried out in solution, in the solid state or preferably in the melt, for example, by reactive extrusion of the polymer in the presence of a grafting compound and a free radical initiator. For example, EP0572028A1 describes the functionalization of polypropylene and / or polyethylene with maleic anhydride.

[0094] Preferably, the polymer composition (A) comprises or consists of the following:

[0095] - up to and comprising 100 wt%, preferably 50 to 98 wt% of a polymer (a) according to any one of the above embodiments, and

[0096] - up to and including 50 wt. %, preferably 2 to 50 wt. %, of a component (b) selected from the group consisting of fillers, pigments, flame retardants and combinations thereof,

[0097] The amounts of (a) and (b) are based on the total weight of the polymer composition (A), and the total weight is 100%.

[0098] The metal element included in the inorganic particles (M) is preferably selected from the group consisting of magnesium, calcium, strontium, barium, aluminum, titanium, vanadium, chromium, iron, copper, zinc, ruthenium, rhodium, palladium, silver, tin, platinum, gold, titanium, zirconium, alloys of the metals and combinations thereof, particularly preferably aluminum.

[0099] The inorganic particles (M) preferably include or consist of metal particles, inorganic compound particles, and mixtures thereof.

[0100] The metal particles preferably consist of at least one of the above-mentioned metals or at least one alloy thereof and are preferably in the form of metal flakes. Aluminum flakes are particularly preferred.

[0101] The inorganic compound is preferably selected from metal oxides and mixed metal oxides (eg Al2O3, TiO2), titanates and zirconates of the above metals (eg BaTiO3, Ca2ZrO4), ceramic particles comprising the above metals, zeolites and combinations thereof.

[0102] The inorganic particles (M) preferably have an average particle size D50 of 200 microns or less, more preferably 150 microns or less, more preferably 100 microns or less. In one embodiment, for all the upper limits above, the lower limit of the average particle size is 1 micron.

[0103] Preferably, the inorganic particles (M) also have a particle size equal to or greater than 0.2 micrometers.

[0104] The plastic material is obtained by dry blending or preferably melt blending the polymer composition (A) and the inorganic particles (M) in a conventional melt blending device, preferably a twin-screw extruder, by feeding them sequentially or simultaneously into the device.

[0105] In one embodiment, polyolefin composition (A) comprises polymer (a) and other component (b).Before polyolefin composition (A) and inorganic particles (M) melt blending to obtain plastic material, polymer (a) and other component (b) can be dry blended or preferably mixed in melt blending equipment.Or, polymer (a), other component (b) and inorganic particles (M) are dry blended or preferably fed to melt blending equipment respectively to obtain plastic material.

[0106] The presence of inorganic particles (M) in the plastic material in an amount up to and including 7 wt. % has limited effect on the mechanical properties of the polymer composition (A), and the mechanical properties of the plastic material are not significantly different from the mechanical properties of the polymer composition (A) without added inorganic particles (M).

[0107] The plastic material of the present disclosure is suitable for forming shaped articles, preferably structural parts of shaped articles.

[0108] The shaped articles of the present disclosure are obtained / obtainable by known processes for shaping plastic materials, preferably by injection molding.

[0109] In one embodiment, the shaped article of the present disclosure is obtained or obtainable by shaping a plastic material as described above, preferably by injection molding.

[0110] When the molded article is irradiated with electromagnetic waves having a frequency of 1 GHz to 300 GHz, preferably with electromagnetic waves having a frequency in the range of from 70 GHz to 130 GHz, more preferably in the range of from 76 GHz to 81 GHz, the molded article has a thickness d satisfying the following equation (I):

[0111]

[0112] in

[0113] - d is the thickness of the shaped article measured at the point of incident electromagnetic wave;

[0114] -λ0 is the vacuum wavelength corresponding to the frequency of the electromagnetic wave irradiating the molded article;

[0115] -ε r is the relative dielectric constant of the plastic material determined as described in the experimental section, and

[0116] -m is a positive integer equal to or greater than 1.

[0117] The thickness d of the shaped article ranges from 0.5 mm to 20 mm, preferably from 0.5 mm to 15 mm, more preferably from 1 mm to 10 mm.

[0118] λ0 is a known value determined by the radiation irradiating the molded product.

[0119] Preferably, m is an integer ranging from 1-20, preferably from 1-16, more preferably from 1-10, still more preferably from 1-6.

[0120] The shaped articles of the present disclosure allow for the transmission of electromagnetic waves, including but not limited to radar frequencies, with minimal or no attenuation of the incident waves.

[0121] In a preferred embodiment, the shaped article is a vehicle bumper, a cover or a housing of a device for transmitting and / or receiving electromagnetic waves, such as a radome.

[0122] The shaped articles of the present disclosure are suitable for at least partially, preferably completely, covering a device that emits and / or receives electromagnetic waves, such as a radar detection system for an autonomous vehicle.

[0123] Therefore, the present disclosure also relates to a device configured to emit and / or receive electromagnetic waves, the device being at least partially, preferably completely, covered by a shaped article as described above. In a preferred embodiment, the device is a radar detection system for an autonomous vehicle.

[0124] The present disclosure also provides the use of a plastic material for optimizing the transmission of electromagnetic waves with a frequency in the range from 1 GHz to 300 GHz through a molded article with a thickness d in the range from 0.5 mm to 20 mm, the plastic material comprising up to and including 7 wt%, preferably 0.05 wt% to 7.0 wt%, of inorganic particles (M) containing metal elements and at least 93.0 wt%, preferably 93.0 wt% to 99.95 wt% of a polymer composition (A), wherein the amounts of (A) and (M) are calculated by weight of the plastic material, and the total weight is 100%.

[0125] The use according to the present disclosure comprises forming the plastic material into an article having a thickness d satisfying equation (I), preferably by injection molding, wherein d, λ0, ε r The values ​​of and m are as defined above.

[0126] The present disclosure also provides a method for optimizing the transmission of electromagnetic waves having a frequency in the range of from 1 GHz to 300 GHz through a shaped article, the method comprising:

[0127] - providing a plastic material comprising at most and including 7 wt%, preferably 0.05 to 7.0 wt%, of inorganic particles (M) containing a metal element and at least 93.0 wt%, preferably 93.0 to 99.95 wt%, of a polymer composition (A), wherein the amounts of (A) and (M) are 100 wt% based on the weight of the plastic material; and

[0128] - forming the plastic material into a product having a thickness d ranging from 0.5 mm to 20 mm and satisfying the following equation

[0129]

[0130] in

[0131] d is the thickness of the molded product;

[0132] λ0 is the vacuum wavelength corresponding to the frequency of the electromagnetic wave irradiating the molded article, and the frequency range is from 1 GHz to 300 GHz;

[0133] ε r is the relative dielectric constant of the plastic material, and

[0134] m is a positive integer equal to or greater than 1.

[0135] Composition of plastic materials and d, λ0, ε r and the values ​​of m are as described above.

[0136] Optimizing the transmission of electromagnetic waves through the shaped article makes it possible to optimize the emission and / or detection of waves by an emitting and / or detecting device shielded by the shaped article (such as a radar detection system of an autonomous vehicle).

[0137] The features describing the subject matter of the present disclosure are not inextricably linked to one another. Thus, a preferred range for one feature may be combined with a more preferred range or a less preferred range for a different feature, regardless of their order of preference.

[0138] Examples

[0139] The following examples are illustrative only and are not intended to limit the scope of the present disclosure in any way.

[0140] Characterization methods

[0141] The following methods were used to determine the properties indicated in the specification, claims and examples.

[0142] Melt flow rate: determined according to method ISO 1133 (230°C, 2.16 Kg for thermoplastic polyolefins; 190°C / 2.16 Kg for compatibilizers).

[0143] Solubility in xylene at 25°C: 2.5 g of a polymer sample and 250 ml of xylene were introduced into a glass flask equipped with a cooler and a magnetic stirrer. The temperature was raised to 135°C over 30 minutes. The clear solution obtained was kept at reflux and stirred for another 30 minutes. The solution was cooled in two stages. In the first stage, the temperature was reduced to 100°C in air under stirring for 10 to 15 minutes. In the second stage, the flask was transferred to a thermostatically controlled water bath at 25°C for 30 minutes. The temperature was reduced to 25°C without stirring during the first 20 minutes and maintained at 25°C for the last 10 minutes under stirring. The formed solid was filtered on a fast filter paper (e.g., Whitman (Whatman n ) filter paper grade 4 or 541). 100 m The filtered solution (S1) of l was poured into a pre-weighed aluminum container, which was heated to 140°C on a hot plate under a nitrogen flow to remove the solvent by evaporation. The container was then kept in an oven at 80°C under vacuum until constant weight was reached. The amount of polymer soluble in xylene at 25°C was then calculated. XS(I) and XS were experimentally determined. A The fraction of component (B) soluble in xylene at 25°C (XS B ) can be calculated by the following formula:

[0144] XS=W(A)×(XS A )+W(B)×(XS B )

[0145] Wherein W(A) and W(B) are the relative amounts of components (A) and (B), respectively, and W(A)+W(B)=1.

[0146] C2 content in propylene-ethylene copolymer (II): collected on a Bruker AV-600 spectrometer equipped with a cryoprobe 13 CNMR spectroscopy, operating at 160.91 MHz at 120 °C in Fourier transform mode. ββ The carbon peak (according to the nomenclature of CJ Carman, RA Harrington and CE Wilkes, Macromolecules, 10, 3, 536 (1977)) at 2.8 ppm was used as an internal reference. The samples were dissolved in 1,1,2,2-tetrachloroethane-d2 at 8% wt / v at 120°C. Each spectrum was collected with 90° pulses with a 15 second delay between pulses and CPD was used to remove 1 H- 13C coupling. 512 transient data were stored in 32K data points using a spectral window of 9000 Hz. The spectra were assigned according to Kakugo [M. Kakugo, Y. Naito, K. Mizunuma and T. Miyatake, Macromolecules, 16, 4, 1160 (1982)] and the triad distribution and composition were evaluated. Due to the low amount of propylene inserted as a regio-random unit, the ethylene content was calculated according to Kakugo [M. Kakugo, Y. Naito, K. Mizunuma and T. Miyatake, Macromolecules, 16, 4, 1160 (1982)] using only triad sequences with P inserted as a regular unit.

[0147] PPP=100T ββ / S

[0148] PPE=100T βδ / S

[0149] EPE=100T δδ / S

[0150] PEP=100Sββ / S

[0151] PEE=100Sβ δ / S

[0152] EEE=100(0.25S γδ +0.5S δδ ) / S

[0153] Where S = T ββ +T βδ +T δδ +S ββ +S βδ +0.25S γδ +0.5S δδ

[0154] The molar contents of ethylene and propylene were calculated from the triad using the following equations:

[0155] [E]mol=EEE+PEE+PEP

[0156] [P]mol=PPP+PPE+EPE

[0157] The weight percent ethylene content (E% wt) was calculated using the following equation:

[0158]

[0159] in

[0160] [P]mol = molar percentage of propylene content;

[0161] MWE = molecular weight of ethylene

[0162] MWP = molecular weight of propylene.

[0163] The total ethylene content C2(tot) and the ethylene content C2(A) of component (A) were measured; the ethylene content C2(B) of component (B) was calculated using the following formula:

[0164] C2(tot)=W(A)×C2(A)+W(B)×C2(B)

[0165] Wherein W(A) and W(B) are the relative amounts of components (A) and (B) (W(A)+W(B)=1).

[0166] Flexural Modulus: Determined according to ISO 178 / A:2019-04 on Type 1 injection molded specimens according to ISO 20753.

[0167] Relative dielectric constant ε r and attenuation: The relative permittivity was measured using the radome measurement system RMS-D-77 / 79G from perisens GmbH, which measures amplitude and phase in the frequency range of 76 GHz to 81 GHz via free-space transmission (S21) for determining the relative permittivity of a material. The device sends radar waves in a specific frequency band through a material sample. One measurement is performed without the sample and one with it, from which the damping of the signal is calculated. To calculate the permittivity, the damping between the two measurements and the thickness of the sample (measured with a Mitutoyo digital sheet metal micrometer IP65) are used.

[0168] Particle size and particle size distribution: measured by laser diffraction, for example using a Mastersizer Hydro 3000 (15 sec test, stirring speed 3500 rpm).

[0169] Raw materials:

[0170] HECO : A heterophasic polyolefin composition comprising 60 wt% of a propylene homopolymer (1) and 40 wt% of a propylene-ethylene copolymer (1) containing 68 wt% of ethylene based on the weight of the copolymer (b), wherein the amounts of (a) and (b) are based on the total weight of the HECO. The HECO is a reactor blend of components (a) and (b) obtained as described in Examples 1 to 2 of patent application WO2005 / 014715A1.

[0171] talc: Sold by Imerys PerformanceAdditives 3CA.

[0172] Inorganic particles (M): Metaflake Ltd. sells Pellex A32-30LW, a pellet containing 30% by weight of polyethylene wax and 70% by weight of aluminum flakes having an average particle size D50 of 32 microns.

[0173] Comparative Examples CE1 to CE2 and Example E3

[0174] The plastic material having the composition of Table 1 was prepared by compounding in a twin-screw extruder having a rotation speed of 300 rpm, a mass flow rate of 40 kg / hour, and a temperature of 220° C. (zone 1=200° C., zone 2=210° C., zone 3=220° C., zone 3=zone 4=zone 5=zone 6). The article was obtained by molding the plastic material having the composition of Table 1 into a 2.42 mm thick plate using an injection molding machine having a clamping force of 1600 kN and a screw diameter of 50 mm. The extruder was operated under the following conditions:

[0175] Melting temperature: 225℃;

[0176] Mold temperature: 30℃;

[0177] Average injection speed: 100 mm / s;

[0178] Cavity pressure switching point: 150 bar;

[0179] Maintaining pressure (hydraulic): 50 bar;

[0180] Keep pressure time: 30 seconds;

[0181] Cooldown time: 28 seconds.

[0182] The test specimen was illuminated with a radar frequency of 77 GHz (corresponding to a λ0 vacuum wavelength of 3.89 mm), and equation (I) was satisfied for m = 2. The value of the relative dielectric constant εr was determined experimentally.

[0183] The composition of the plastic materials and the tested properties of the shaped articles are reported in Table 1.

[0184] Table 1

[0185] CE1 CE2 E3 HECO weight% 100 89,5 88,7 talc weight% - 10,5 9.9 Inorganic particles (M) weight% - - 1.4 MFR(230℃ / 2.16Kg) g / 10 minutes 12 10,3 11 Flexural modulus MPa 1100 1534 1569 Relative dielectric constant εr 2.2 2.36 2.6 attenuation dB 0.13 0.06 0.02

Claims

1. A shaped article comprising a plastic material, the plastic material comprising up to and including 7 wt. % of inorganic particles (M) containing a metal element and at least 93.0 wt. % of a polymer composition (A), wherein the thickness d of the shaped article ranges from 0.5 mm to 20 mm, and when the shaped article is irradiated with an electromagnetic wave having a frequency of 1 GHz to 300 GHz, the thickness d satisfies equation (I) in d is the thickness of the molded product; λ0 is the vacuum wavelength corresponding to the frequency of the electromagnetic wave irradiating the molded product; ε r is the relative dielectric constant of the plastic material, and m is a positive integer equal to or greater than 1, and wherein the amounts of (A) and (M) are based on the total weight of the plastic material, the total weight being 100%.

2. The molded article according to claim 1, wherein the plastic material comprises 0.1 wt% to 7.0 wt%, more preferably 0.1 wt% to 4.0 wt%, more preferably 0.5 wt% to 4.0 wt% of the inorganic particles (M) and 93.0 wt% to 99.9 wt%, preferably 96.0 wt% to 99.9 wt%, more preferably 96.0 wt% to 99.5 wt% of the polymer composition (A), the amounts of (A) and (M) being calculated based on the total weight of the plastic material, the total weight being 100%.

3. The shaped article according to claim 1 or 2, wherein the polymer composition (A) comprises up to and including 100 wt. %, preferably 50 wt. % to 98 wt. % of at least one polymer (a), the at least one polymer (a) being selected from the group consisting of propylene polymers, ethylene polymers, polybutene-1, polystyrene, acrylic polymers, acrylonitrile butadiene styrene polymers, acrylonitrile styrene acrylate polymers, polyamides, polyesters, polyurethanes, polycarbonates and mixtures thereof, wherein the amount of the polymer (a) is based on the weight of the polymer composition (A), and the total weight is 100%.

4. The shaped article according to claim 3, wherein the polymer (a) is a heterophasic propylene polymer comprising: (1) up to and including 90 wt%, preferably 10 to 80 wt%, more preferably 15 to 70 wt% of at least one propylene polymer selected from the group consisting of: - propylene homopolymer, a propylene copolymer having at least one olefin of formula CH2=CHR, wherein R is hydrogen or a linear or branched C2-C8 alkyl group, said propylene copolymer comprising up to and including 10.0 wt.-%, preferably 0.05 to 10.0 wt.-%, more preferably 0.1 to 8.0 wt.-%, based on the weight of (1), of units derived from α-olefins, and - mixtures thereof; as well as (2) at least 10 wt.-%, preferably from 20 to 90 wt.-%, more preferably from 30 to 85 wt.-%, of an elastomeric propylene copolymer having at least one olefin of formula CH2=CHR, wherein R is hydrogen or a linear or branched C2-C8 alkyl group, said elastomeric propylene copolymer comprising up to and including 85 wt.-%, more preferably from 20 to 85 wt.-%, still more preferably from 25 to 75 wt.-%, based on the weight of (2), of units derived from said α-olefin, The amounts of (1) and (2) are based on the total weight of (1) + (2).

5. The shaped article according to any one of claims 1 to 4, wherein the polymer composition (A) further comprises up to and including 50 wt. %, preferably 2 wt. % to 50 wt. %, of at least one additional component (b), the at least one additional component (b) being selected from the group consisting of fillers, pigments, flame retardants, compatibilizers and combinations thereof, wherein the amount of component (b) is based on the total weight of the polymer composition (A), the total weight being 100%.

6. The shaped article according to any one of claims 1 to 5, wherein the metal element contained in the inorganic particles (M) is selected from the group consisting of magnesium, calcium, strontium, barium, aluminum, titanium, vanadium, chromium, iron, copper, zinc, ruthenium, rhodium, palladium, silver, tin, platinum, gold, titanium, zirconium, alloys of the metals, and combinations thereof.

7. The shaped article according to any one of claims 1 to 6, wherein the inorganic particles (M) are metal flakes, preferably aluminum flakes.

8. The shaped article according to any one of claims 1 to 7, wherein the inorganic particles (M) have an average particle size D50 measured by laser diffraction of equal to or lower than 200 microns, preferably equal to or lower than 150 microns, more preferably equal to or lower than 100 microns.

9. The shaped article according to any one of claims 1 to 8, wherein when the shaped article is irradiated with electromagnetic waves having a frequency in the range of from 70 GHz to 130 GHz, preferably from 76 GHz to 81 GHz, equation (I) is satisfied. 10 . The shaped article according to claim 1 , wherein m ranges from 1 to 20, preferably from 1 to 16, more preferably from 1 to 10, still more preferably from 1 to 6.

11. The shaped article according to any one of claims 1 to 10, wherein the thickness d of the shaped article ranges from 0.5 mm to 20 mm, preferably from 0.5 mm to 15 mm, more preferably from 1 mm to 10 mm.

12. The shaped article according to any one of claims 1 to 11, wherein the article is a vehicle bumper, a cover or a housing of a device for emitting and / or receiving electromagnetic waves.

13. Use of a shaped article according to any one of claims 1 to 12 for at least partially covering a device for emitting and / or receiving electromagnetic waves, preferably a radar detection system for an unmanned vehicle.

14. Use of a plastic material according to any one of claims 1 to 11 for optimizing the transmission of electromagnetic waves with a frequency in the range from 1 GHz to 300 GHz through a shaped article having a thickness d in the range from 0.5 mm to 20 mm.

15. A method of optimizing the transmission of electromagnetic waves having a frequency in the range from 1 GHz to 300 GHz through a shaped article, the method comprising: - Providing a plastic material according to any one of claims 1 to 11; as well as - forming said article having a thickness d ranging from 0.5 mm to 20 mm and satisfying the equation in d is the thickness of the shaped article; λ0 is a vacuum wavelength corresponding to the frequency of the electromagnetic wave irradiating the molded article, the frequency ranging from 1 GHz to 300 GHz; ε r is the relative dielectric constant of the plastic material, and m is a positive integer equal to or greater than 1.

16. A device configured to emit and / or receive electromagnetic waves, the device being at least partially covered by the shaped article according to any one of claims 1 to 12.

17. The device of claim 16, wherein the device is a radar detection system for an unmanned vehicle.