Energy ray-curable film-like transparent adhesive, device comprising same, and method for manufacturing device
By using a combination of epoxy resin, phenoxy resin and antimony photocationic polymerization initiator, the problem of poor reactivity in low temperature areas and reduced adhesion at high temperatures is solved, and high efficiency and transparent energy is achieved The ray-cured film-like adhesive improves the reliability and heat resistance of functional components.
Patent Information
- Application Number
- CN202380034722.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-30
- Filing Date
- 2023-06-28
- Publication Date
- 2024-11-26
AI Technical Summary
The existing film-like adhesive has poor reactivity in the curing components in low-temperature areas, and requires increasing the irradiation of energy rays, and the adhesive force is easily reduced at high temperatures, which affects the reliability and transparency of functional components.
The energy-ray-curing film-like transparent adhesive consisting of epoxy resin, phenoxy resin and photocationic polymerization initiator containing antimony in anionic part is cured by ultraviolet irradiation, with high glass transition temperature and high parallel light transmission. to ensure that the bonding force is not easily reduced at high temperatures.
It realizes efficient curing with less energy ray irradiation, maintains sufficient adhesion and transparency, and improves the reliability and heat resistance of functional components.
Smart Images

Figure BDA0005089501540000191 
Figure BDA0005089501540000201 
Figure HDA0005089501550000011
Abstract
Description
Technical Field
[0001] The present invention relates to an energy ray-curable film-like transparent adhesive, a device including the film-like transparent adhesive, and a method for producing the device. Background Art
[0002] Image sensors (imaging elements) such as CMOS (Complementary Metal Oxide Semiconductor) image sensors and CCD (Charge Coupled Device) image sensors are installed in digital cameras, digital video cameras and other photographic equipment. The image sensor uses a photodiode to perform photoelectric conversion on the incident light and convert it into an electrical signal, and forms a digital image after signal processing. Color filters, microlenses, etc. are arranged on the surface of the photodiode as needed, and a transparent protective film such as a glass plate is usually arranged on the surface of the laminate. Such a transparent protective film is fixed by a film-like adhesive or the like. The adhesive used for bonding and fixing the transparent protective film of the image sensor is required to have transparency that allows light to pass through fully.
[0003] On the other hand, in image display devices, functional elements (organic electroluminescent (organic EL) elements, liquid crystal panels, micro light-emitting diodes (Micro LED), semiconductor elements such as transistors, etc.) are sometimes arranged on a supporting substrate, and functional layers (protective layers, gas barrier layers (sealing layers), hard coating layers, etc.) are arranged on the surface of the functional elements. The adhesive used for bonding / fixing these functional elements and functional layers is sometimes also required to have sufficient transparency.
[0004] Film adhesives are known to have various compositions, and are widely used in manufacturing electronic devices and components thereof, not limited to image sensors and image display devices. For example, film adhesives are used as die-bonding films in the manufacturing process of semiconductor chips.
[0005] Patent Document 1 discloses a sheet adhesive containing a phenoxy resin having a glass transition temperature of 110° C. or higher, a multifunctional epoxy resin, and a photocationic polymerization initiator. In a specific embodiment thereof, 4-(phenylthio)phenyldiphenylsulfonium hexafluorophosphate or the like is used as the photocationic polymerization initiator. It is believed that the sheet adhesive has excellent shape stability under high temperature conditions.
[0006] Patent Document 2 discloses an adhesive having active energy ray curing properties, wherein the adhesive is cured according to CIE 1976L * a * b * The color system specifies a * Value and b *The calculated X value is set to a specific range, and the color difference ΔE before and after curing is specified according to the color system. * a The adhesive contains a dye whose color disappears due to irradiation with active energy rays and a photoinitiator, and further contains a (meth)acrylate polymer, a crosslinking agent, and an active energy ray-curable component. It is believed that the adhesive can easily confirm the curing caused by irradiation with active energy rays.
[0007] Patent Document 3 discloses an organic electroluminescent element sealant, which contains 100 parts by mass of a bisphenol epoxy resin as a photocationic polymerizable compound and 0.1 to 100 parts by mass of a specific sulfonium borate as a photocationic polymerizer. The sealant exhibits excellent photocurability and is suitable for sealing electroluminescent elements.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: International Publication No. 2020 / 196240
[0011] Patent Document 2: Japanese Patent Application Laid-Open No. 2020-26491
[0012] Patent Document 1: Japanese Patent No. 4933751 Summary of the invention
[0013] Problems to be solved by the invention
[0014] Among functional elements, many have low heat resistance. In the manufacture of devices containing such low heat resistance elements, a method of manufacturing without heat treatment is adopted to avoid damage to the elements. In the manufacture of such devices, as adhesives, film adhesives of energy ray curing method that can be cured at room temperature or in a low temperature region near room temperature are mostly used. However, compared with liquid adhesives, film adhesives have lower molecular fluidity, so there is a tendency for the reactivity of the curing component to be poor in low temperature regions.
[0015] In order to cure the film adhesive efficiently in a low temperature region, it is necessary to increase the irradiation amount of energy rays compared to liquid adhesives. For example, Patent Document 1 discloses in its specific embodiment that in order to cure the sheet adhesive, 2000 mJ / cm 2 Ultraviolet (UV) irradiation and further heating at 100°C. In addition, Patent Document 2 discloses in its specific embodiment that: 2 The curing of the adhesive layer is basically completed. In addition, Patent Document 3 discloses in its specific embodiment that in order to cure the sealing material, 2000mJ / cm2 On the other hand, if the irradiation amount of energy rays increases, even if no heat is applied, heat generation will occur as a side reaction accompanying the curing reaction, and as a result, the functional element is sometimes exposed to high temperature. In this case, problems such as poor reliability and reduced transparency caused by the deterioration of the adhesive force of the adhesive itself are likely to occur. Therefore, it is desired to have a film-like transparent adhesive that can be cured with a small amount of energy ray irradiation, is highly reactive, and is not easily reduced in adhesive force at high temperatures.
[0016] In addition, depending on the device, it may be placed in a high-temperature environment during use, or the device itself may become hot due to heat generated from the inside (for example, devices used in vehicles, etc.). Therefore, in order to improve the reliability of the device in such an environment, an adhesive whose bonding strength is not easily reduced at high temperatures is also required.
[0017] Usually, in order to improve the adhesive force, fillers are mostly added to the adhesive. By adding fillers, the bonding reliability of the adhesive can be improved. However, the addition of fillers will reduce the transparency of the adhesive, so when adding fillers, the above-mentioned reliability improvement and the transparency of the adhesive are in a so-called trade-off relationship. It is desired to have a film-like transparent adhesive that can achieve high bonding reliability even without adding fillers.
[0018] The present invention aims to provide an energy-ray-curable film-like transparent adhesive, which can be cured with a small amount of energy-ray irradiation to exert sufficient adhesive force, has excellent transparency after curing, and is not easily reduced in adhesive force at high temperatures. In addition, the present invention aims to provide a device including the above-mentioned energy-ray-curable film-like transparent adhesive and a method for manufacturing a device using the above-mentioned energy-ray-curable film-like transparent adhesive.
[0019] Means for solving problems
[0020] The above-mentioned problems of the present invention are solved by the following means. [1]
[0022] An energy-ray-curable film-like transparent adhesive comprises an epoxy resin, a phenoxy resin, and a photocationic polymerization initiator containing antimony in the anion part. [2]
[0024] The energy-ray-curable film-like transparent adhesive according to [1], wherein the phenoxy resin has a glass transition temperature of 80°C to 120°C. [3]
[0026] The energy-ray-curable film-like transparent adhesive according to [1] or [2], wherein a cured product of the energy-ray-curable film-like transparent adhesive has a glass transition temperature of 80° C. or higher. [4]
[0028] The energy ray-curable film-like transparent adhesive according to any one of [1] to [3], wherein a cured product of the energy ray-curable film-like transparent adhesive has a parallel light transmittance of 80% or more. [5]
[0030] The energy ray-curable film-like transparent adhesive according to any one of [1] to [4], wherein a storage modulus of a cured product of the energy ray-curable film-like transparent adhesive at room temperature is 1.0 GPa or more. [6]
[0032] The energy beam-curable film-like transparent adhesive according to any one of [1] to [5], wherein the epoxy resin has a hydrogenated bisphenol structure or a bisphenol structure. [7]
[0034] The energy ray-curable film-like transparent adhesive according to any one of [1] to [6], comprising a silane coupling agent. [8]
[0036] The energy ray-curable film-like transparent adhesive according to any one of [1] to [7], further comprising a curing retardant. [9]
[0038] The energy ray-curable film-like transparent adhesive according to any one of [1] to [8], further comprising a filler.
[10]
[0040] A device including a structure in which constituent members are bonded together using the energy ray-curable film-like transparent adhesive according to any one of [1] to [9].
[11]
[0042] A device manufacturing method comprising bonding constituent members using the energy ray-curable film-like transparent adhesive according to any one of [1] to [9].
[0043] In the present invention, a numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0044] Effects of the Invention
[0045] The energy-ray-curable film-shaped transparent adhesive of the present invention can exert sufficient adhesive force when cured with a small amount of energy-ray irradiation, has high transparency, and is not easily reduced in adhesive force at high temperatures. In addition, even if the energy-ray-curable film-shaped transparent adhesive of the present invention is used as an adhesive for a component with low heat resistance, damage to the component can be suppressed, and the bonding reliability of the obtained device can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a cross-sectional view schematically showing the structure of a film-like adhesive with a release film prepared in Examples. DETAILED DESCRIPTION
[0047] [Energy ray curing film-like transparent adhesive]
[0048] The energy-ray-curable film-like transparent adhesive of the present invention (hereinafter also referred to as "the film-like adhesive of the present invention") contains an epoxy resin, a phenoxy resin and a photocationic polymerization initiator containing antimony in the anion part. The film-like adhesive of the present invention is in a state before curing, that is, in the state of stage B, and is cured by energy ray irradiation to exert adhesion to the adherend. Therefore, the film-like adhesive of the present invention is a film composed of a curable composition. The film-like adhesive of the present invention can be suitable for bonding or sealing purposes of components of devices. As devices, digital cameras, digital video cameras, organic EL devices, liquid crystal panel devices, micro LED devices, smart phones, personal computers, televisions, etc. can be cited. The film-like adhesive of the present invention is particularly suitable for bonding or sealing purposes of components of optical products requiring high transparency (such as components such as organic EL devices, liquid crystal panels, micro LED devices (such as lenses, transparent protective films, glass substrates, functional elements and functional layers described later, their laminates, etc.)).
[0049] Examples of the energy ray include light such as ultraviolet rays (UV) and ionizing radiation such as electron beams. The energy ray is preferably ultraviolet rays.
[0050] The film-like adhesive of the present invention does not use a thermal polymerization initiator.
[0051] Each component contained in the film-like adhesive of the present invention will be described.
[0052] (Epoxy resin)
[0053] The film-like adhesive of the present invention contains at least one epoxy resin.
[0054] The epoxy resin may be any resin having an epoxy group, and any epoxy resin that can be used in adhesives can be used. The epoxy resin is a resin that forms a crosslinked structure in the resin composition by reacting an epoxy group with a reactive group of another component or by ring-opening polymerization of epoxy groups.
[0055] In the present invention, epoxy resin refers to a resin having an epoxy equivalent of 3000 g / eq or less. It should be noted that in the present invention, epoxy equivalent refers to the number of grams (g / eq) of the resin containing 1 gram equivalent of epoxy groups.
[0056] The epoxy equivalent of the epoxy resin is preferably 100 to 3000 g / eq, more preferably 180 to 1500 g / eq.
[0057] When the epoxy resin has an alicyclic structure, the epoxy equivalent is preferably large, for example, preferably 200 g / eq or more, more preferably 200 to 3000 g / eq, and further preferably 200 to 1500 g / eq.
[0058] On the contrary, when the epoxy resin does not have an alicyclic structure, the epoxy equivalent can be made smaller, for example, preferably less than 200 g / eq, more preferably 100 to 195 g / eq, further preferably 120 to 195 g / eq, further preferably 130 to 195 g / eq.
[0059] From the perspective of improving the flexibility of the cured product of the film-like adhesive of the present invention, an epoxy resin having an alicyclic structure and a small epoxy equivalent (e.g., an epoxy resin having an epoxy equivalent of 500 g / eq or less, preferably an epoxy resin having an epoxy equivalent of 300 g / eq or less) and an epoxy resin having an alicyclic structure and a large epoxy equivalent (e.g., an epoxy resin having an epoxy equivalent of 600 to 1300 g / eq, preferably an epoxy resin having an epoxy equivalent of 900 to 1300 g / eq) can be used in combination.
[0060] As the skeleton of epoxy resin, phenol novolac type, o-cresol novolac type, cresol novolac type, dicyclopentadiene type, biphenyl type, fluorene bisphenol type, triazine type, naphthol type, naphthyl diol type, triphenylmethane type, tetraphenyl type, bisphenol A type, bisphenol F type, bisphenol AD type, bisphenol S type, trimethylolmethane type, etc. can be cited. Among them, from the aspect of obtaining a film-like adhesive with low crystallinity of the resin and good appearance, triphenylmethane type, bisphenol A type, cresol novolac type, and o-cresol novolac type are preferred. They can be used alone or in combination of two or more.
[0061] The epoxy resin is preferably an epoxy resin having a bisphenol structure.
[0062] The epoxy resin is preferably an epoxy resin having an alicyclic structure, more preferably a hydrogenated bisphenol-type epoxy resin (an epoxy resin having a hydrogenated bisphenol structure), and further preferably a hydrogenated bisphenol A-type epoxy resin.
[0063] From the viewpoint of reducing yellowing of the cured product of the film-like adhesive of the present invention and improving transparency, it is preferred to use an epoxy resin having an alicyclic structure, and it is more preferred to use an epoxy resin having a hydrogenated bisphenol structure.
[0064] The epoxy resin may be a liquid epoxy resin or a solid epoxy resin. From the viewpoint of suppressing stickiness and improving handling properties, it is preferred to use a solid epoxy resin alone or to use a solid epoxy resin and a liquid epoxy resin in combination.
[0065] The weight average molecular weight of the epoxy resin is preferably 100 to 3,000, more preferably 200 to 1,500.
[0066] The weight average molecular weight is a value based on GPC (Gel Permeation Chromatography) analysis.
[0067] The content of the epoxy resin in the solid content (components other than the solvent) of the film adhesive of the present invention is preferably 10 to 80% by mass, more preferably 25 to 80% by mass, further preferably 30 to 80% by mass, further preferably 40 to 75% by mass, further preferably 50 to 75% by mass, and most preferably 60 to 70% by mass.
[0068] (Phenoxy resin)
[0069] The film-like adhesive of the present invention contains at least one phenoxy resin.
[0070] The phenoxy resin is a component that suppresses the film viscosity at room temperature (23° C.) when forming a film-like adhesive and imparts film-forming properties (film-forming properties).
[0071] It should be noted that in the present invention, phenoxy resin refers to a resin having an epoxy equivalent (mass of resin per 1 equivalent of epoxy group) exceeding 3000 g / eq. That is, even if it has a phenoxy resin structure, a resin having an epoxy equivalent of 3000 g / eq or less is also classified as an epoxy resin.
[0072] The phenoxy resin can be obtained by a conventional method, for example, by the reaction of a bisphenol or biphenol compound with an epihalohydrin such as epichlorohydrin, or by the reaction of a liquid epoxy resin with a bisphenol or biphenol compound.
[0073] The glass transition temperature (Tg) of the phenoxy resin is preferably 160°C or lower, more preferably 120°C or lower, further preferably less than 110°C, further preferably 100°C or lower, and particularly preferably 90°C or lower. The Tg of the phenoxy resin is preferably 0°C or higher, 10°C or higher, 20°C or higher, 30°C or higher, 40°C or higher, 50°C or higher, 60°C or higher, 70°C or higher, and 80°C or higher. The Tg of the phenoxy resin is preferably 0 to 160°C, 10 to 125°C, 30 to 120°C, 50 to 120°C, 70 to 120°C, 80 to 120°C, 80 to 80°C and less than 110°C, and 80 to 100°C. The Tg of the phenoxy resin is preferably 80°C or higher from the viewpoint of increasing the storage modulus of the cured product of the film adhesive of the present invention at room temperature (23°C). From the viewpoint of further improving the transparency of the cured product of the film-like adhesive of the present invention, the Tg of the phenoxy resin is preferably 10 to 120°C, preferably 80 to 120°C, preferably 80°C or more and less than 110°C, and preferably 80 to 100°C.
[0074] The Tg of the phenoxy resin is the peak top temperature of tan δ in the dynamic viscoelasticity measurement. Specifically, Tg can be determined as follows.
[0075] A solution in which a phenoxy resin is dissolved is applied to a release film and heated and dried to form a film (polymer film) composed of a phenoxy resin on the release film. The release film is peeled off and removed from the polymer film, and the polymer film is measured using a dynamic viscoelasticity measuring device (trade name: Rheogel-E4000F, manufactured by UBM) at a measuring temperature range of 20 to 300°C, a heating rate of 5°C / min, and a frequency of 1 Hz. The obtained tan δ peak temperature (the temperature at which tan δ shows a maximum value) is set to Tg.
[0076] The phenoxy resin generally has a weight average molecular weight of at least 10000. The upper limit is not particularly limited, but is practically 5000000 or less.
[0077] The weight average molecular weight of the phenoxy resin is determined in terms of polystyrene by GPC (Gel Permeation Chromatography).
[0078] Focusing on the skeleton of the phenoxy resin, in the present invention, a bisphenol A type phenoxy resin, a phenoxy resin containing a biphenyl skeleton and a cyclohexane skeleton, or a bisphenol F + 1,6-hexanediol diglycidyl ether type phenoxy resin can be preferably used.
[0079] In the film-like adhesive of the present invention, the content of the phenoxy resin can be, for example, 30 to 500 parts by mass, 30 to 400 parts by mass, 30 to 300 parts by mass, 40 to 250 parts by mass, 40 to 120 parts by mass, and preferably 40 to 80 parts by mass, relative to 100 parts by mass of the epoxy resin.
[0080] (Photocationic polymerization initiator)
[0081] The film adhesive of the present invention contains a photocationic polymerization initiator containing antimony in the anion part (hereinafter also simply referred to as "photocationic polymerization initiator"). "Containing antimony in the anion part" means having an anion containing an antimony atom in the anion part.
[0082] The photocationic polymerization initiator is preferably an onium salt having the above-mentioned anion part and cation part, and is more preferably an aromatic onium salt.
[0083] The anion part of the photocationic polymerization initiator can be any anion containing an antimony atom, preferably SbF4 - and SbF6 - , more preferably SbF6 - .
[0084] The cationic part of the photocationic polymerization initiator is not particularly limited, but is preferably a sulfonium compound ion, an iodonium compound ion, an ammonium compound ion, a phosphonium compound ion, a pyridinium compound ion, and more preferably a sulfonium compound ion and an iodonium compound ion.
[0085] The cationic part is not particularly limited as long as it has a structure that functions as a photocationic polymerization initiator. From the perspective of light absorption, it is preferred to have an aromatic group. As the aromatic group, an aryl group is preferred, and a phenyl group is more preferred.
[0086] When photocationic polymerization initiators are classified according to the type of cationic site, they may also be referred to as sulfonium salt compounds, iodonium salt compounds, ammonium salt compounds, phosphonium salt compounds, and pyridinium salt compounds. These may be used alone or in combination of two or more.
[0087] The photocationic polymerization initiator is preferably a UV cationic polymerization initiator.
[0088] In the film adhesive of the present invention, the content of the photocationic polymerization initiator may be 0.5 to 30 parts by mass, 1 to 20 parts by mass, 1 to 15 parts by mass, preferably 2 to 10 parts by mass, and preferably 2 to 8 parts by mass, based on 100 parts by mass of the epoxy resin.
[0089] (additive)
[0090] The film adhesive of the present invention may contain a silane coupling agent as an additive. By using a silane coupling agent, the adhesion to the adherend can be further improved, and as a result, the bonding reliability can be improved.
[0091] The silane coupling agent has at least one hydrolyzable group such as an alkoxy group or an aryloxy group bonded to the silicon atom, and may also be bonded to an alkyl group, an alkenyl group, or an aryl group. The alkyl group is preferably substituted with an amino group, an alkoxy group, an epoxy group, or a (meth)acryloyloxy group, and more preferably substituted with an amino group (preferably a phenylamino group), an alkoxy group (preferably a glycidoxy group), or a (meth)acryloyloxy group.
[0092] Examples of the silane coupling agent include 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane.
[0093] When the film adhesive of the present invention contains a silane coupling agent, the content of the silane coupling agent can be 0.1 to 20 parts by mass, 0.5 to 10 parts by mass, 1 to 7 parts by mass, preferably 1 to 5 parts by mass, and preferably 1 to 3 parts by mass, based on 100 parts by mass of the epoxy resin.
[0094] The film-like adhesive of the present invention may contain a curing retarder as an additive. By using a retarded curing agent, the adhesion to the adherend is improved and the adhesive force is improved.
[0095] As a curing retarder, a curing retarder commonly used in an adhesive can be used. As a curing retarder, a polyether compound can be mentioned. As the above-mentioned polyether compound, for example, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, calixarene, crown ether compounds, etc. can be mentioned. Among them, crown ether compounds are preferred. As crown ethers, 18-crown-6-ether, 15-crown-5-ether, etc. can be mentioned.
[0096] When the film adhesive of the present invention contains a curing retarder, the content of the curing retarder can be 0.01 to 20 parts by mass, 0.1 to 10 parts by mass, 0.1 to 8 parts by mass, preferably 0.1 to 5 parts by mass, and preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the epoxy resin.
[0097] The film-like adhesive of the present invention may contain a filler. That is, the film-like adhesive of the present invention may be in a form containing a filler or in a form not containing a filler. However, the film-like adhesive of the present invention exhibits suitable adhesive force even if it does not contain a filler.
[0098] The filler is preferably an inorganic filler. Examples of the inorganic filler include ceramics such as silicon dioxide, clay, gypsum, calcium carbonate, barium sulfate, aluminum oxide (alumina), beryllium oxide, magnesium oxide, silicon carbide, silicon nitride, aluminum nitride, boron nitride, and metals such as aluminum, copper, silver, gold, nickel, chromium, lead, tin, zinc, palladium, solder, and alloys, carbon nanotubes, graphene, and other carbons. Various inorganic powders.
[0099] The inorganic filler may be subjected to surface treatment or surface modification. Examples of agents used for such surface treatment or surface modification include silane coupling agents, phosphoric acid or phosphoric acid compounds, and surfactants.
[0100] The shape of the inorganic filler may be flake, needle, fibril, spherical, or scale-like. Spherical particles are preferred from the viewpoint of high filling and fluidity.
[0101] In the case where the film-like adhesive of the present invention contains a filler, the content of the filler in the above-mentioned film-like adhesive is preferably 70% by mass or less, more preferably 60% by mass or less, also preferably 50% by mass or less, and also preferably 40% by mass or less in the solid content of the film-like adhesive. In the case where the film-like adhesive of the present invention contains a filler, the content of the filler in the above-mentioned film-like adhesive can be 1% by mass or more, can be 2% by mass or more, and is also preferably 4% by mass or more. In the case where the film-like adhesive of the present invention contains a filler, the content of the filler in the above-mentioned film-like adhesive can be 71-70% by mass, can be 2-60% by mass, can be 4-50% by mass, can be 4-40% by mass, and is also preferably 10-30% by mass in the solid content of the film-like adhesive.
[0102] The film-like adhesive of the present invention may further contain an organic solvent, an ion trapping agent, a curing catalyst, a viscosity modifier, an antioxidant, a flame retardant, a colorant, etc. For example, other additives described in International Publication No. 2017 / 158994 may be included.
[0103] The total content of the epoxy resin, the phenoxy resin and the photocationic polymerization initiator in the film-like adhesive of the present invention may be, for example, 30% by mass or more, preferably 40% by mass or more, and more preferably 50% by mass or more. The ratio may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more.
[0104] Here, in the present invention, "film" refers to a thin film having a thickness of 200 μm or less. The shape, size, etc. are not particularly limited and can be appropriately adjusted according to the usage.
[0105] The thickness of the film adhesive of the present invention and the cured product obtained by curing the film adhesive is usually 1 to 100 μm, preferably 2 to 80 μm, and more preferably 5 to 50 μm. The thickness can be measured by a contact / linear gauge method (table-type contact thickness measuring device).
[0106] The glass transition temperature (Tg) of the cured product of the film adhesive of the present invention is preferably 64° C. or higher, more preferably 80° C. or higher. The Tg of the cured product of the film adhesive is the peak top temperature of tan δ in the dynamic viscoelasticity measurement. Specifically, Tg can be determined as follows.
[0107] The film adhesive was laminated to a thickness of 0.3 mm using a laminator at 70° C. and the mercury lamp was used at 23° C. and 500 mJ / cm 2 The cured sample was cut into pieces with a width of 5 mm and used as a test sample. The test sample was measured using a dynamic viscoelasticity measuring device RSAIII (manufactured by TA Instruments) at a distance of 20 mm between chucks, a frequency of 10 Hz, a measuring temperature range of -40°C to 250°C, and a heating rate of 5°C / min. The obtained tanδ peak temperature (the temperature at which tanδ shows a maximum) was taken as the Tg of the cured product of the film adhesive.
[0108] Here, the fact that the Tg of the cured product of the film adhesive of the present invention is X°C means that, when the cured product has two or more Tgs, the Tg on the lowest temperature side is X°C. Therefore, for example, the fact that the Tg of the cured product of the film adhesive of the present invention is 80°C or higher means that, when the cured product has two or more Tgs, the Tg on the lowest temperature side is 80°C or higher.
[0109] The Tg of the cured product of the film-like adhesive of the present invention is also preferably 80° C. or higher, more preferably 90° C. or higher, and even more preferably 100° C. or higher.
[0110] The Tg of the cured product of the film-like adhesive of the present invention is preferably 80 to 150° C., more preferably 80 to 140° C., further preferably 90 to 130° C., further preferably 100 to 130° C. The Tg may also be 110 to 125° C.
[0111] The parallel light transmittance of the cured product of the film-like adhesive of the present invention is preferably 70% or more. In the present invention, the above-mentioned parallel light transmittance refers to the parallel light transmittance at 400nm. Film-like adhesives are usually prone to yellowing due to irradiation with energy rays, so the parallel light transmittance of the obtained cured product at the above wavelength can be used as an indicator to evaluate transparency. That is, the parallel light transmittance at 400nm can represent the parallel light transmittance in the visible light region other than 400nm.
[0112] The parallel light transmittance of the cured product of the film-like adhesive of the present invention is preferably 80% or more, more preferably 85% or more, and further preferably 90% or more. The upper limit of the parallel light transmittance is actually 100%. Therefore, the parallel light transmittance of the cured product of the film-like adhesive of the present invention is preferably 80 to 100%.
[0113] The parallel light transmittance can be measured using a spectrophotometer. Specifically, the parallel light transmittance of the cured product is determined as follows. The film adhesive is laminated to a thickness of 0.3 mm using a laminator at 70° C. and heated at 500 mJ / cm 2 The obtained cured sample was cut into 5 cm squares as measurement samples. The parallel light transmittance at a wavelength of 400 nm was determined using a spectrophotometer (UV-1800, manufactured by Shimadzu Corporation) for the measurement sample.
[0114] The storage modulus of the cured product of the film-like adhesive of the present invention at room temperature (23° C.) (hereinafter also referred to as “storage modulus”) is preferably 0.8 GPa or more. The storage modulus of the above-mentioned cured product is more preferably 1.0 GPa or more, and further preferably 1.2 GPa or more. The storage modulus of the above-mentioned cured product is preferably 7.0 GPa or less, more preferably 6.0 GPa or less, further preferably 5.5 GPa or less, and particularly preferably 5.0 GPa or less. The storage modulus of the above-mentioned cured product can be 0.8 to 7.0 GPa, can also be 0.8 to 6.0 GPa, is also preferably 1.0 to 5.5 GPa, is also preferably 1.0 to 5.0 GPa, is also preferably 1.0 to 4.0 GPa, and is also preferably 1.0 to 3.0 GPa.
[0115] The storage modulus of the cured product was determined as follows: The film adhesive was laminated to a thickness of 0.3 mm using a laminator at 70° C. and 500 mJ / cm 2The obtained cured sample was cut into 5 mm wide pieces as the measurement sample. The measurement sample was subjected to a dynamic viscoelasticity measurement apparatus RSAIII (manufactured by TA Instruments) and heated from -40°C to 250°C at a heating rate of 5°C / min under the conditions of a chuck distance of 20 mm and a tensile frequency of 10 Hz to determine the storage modulus at 23°C.
[0116] The storage modulus of the cured product of the film-like adhesive of the present invention can be controlled by the chemical structure (skeleton, type of functional group, etc.), molecular weight, epoxy equivalent and content of the epoxy resin, the chemical structure (skeleton, type of functional group, etc.), molecular weight, glass transition temperature and content of the phenoxy resin, the chemical structure (skeleton, type of functional group, etc.) and content of the photocationic polymerization initiator, the type or content of the filler and other additives in the adhesive, etc.
[0117] A composition (varnish) obtained by mixing the constituents of the film-like adhesive can be prepared, and the composition is applied to a release film or a desired substrate, and dried as needed to obtain the film-like adhesive of the present invention on the release film or substrate. The composition (varnish) obtained by mixing the constituents of the adhesive layer usually contains an organic solvent.
[0118] As the coating method, a known method can be appropriately adopted, and examples thereof include methods using a roll knife coater, a gravure coater, a die coater, a reverse coater, and the like.
[0119] Drying may be performed without substantially causing a curing reaction, as long as the organic solvent can be removed to form a film-like adhesive, and can be performed, for example, by maintaining the mixture at a temperature of 80 to 150° C. for 1 to 20 minutes.
[0120] The film adhesive of the present invention is preferably stored in a light-shielded state before use (before the curing reaction) from the viewpoint of suppressing the curing reaction of the film adhesive (curing reaction of the epoxy resin). The temperature conditions for storage in a light-shielded state are not particularly limited and may be room temperature or refrigerated.
[0121] [Device manufacturing method]
[0122] The method for producing the device of the present invention is not particularly limited as long as it is a method for producing a device using the film-like adhesive of the present invention.
[0123] One embodiment of the method for producing the device of the present invention includes bonding constituent members using the film-like adhesive of the present invention. Therefore, the device of the present invention includes a structure in which constituent members are bonded using the film-like adhesive of the present invention.
[0124] There are no particular restrictions on the constituent components of the device to which the film-like adhesive of the present invention is applied, and examples thereof include the above-mentioned functional elements and functional layers, and laminates thereof. One embodiment of the method for manufacturing the device of the present invention includes bonding these components, such as laminates containing functional elements (laminates of functional elements and various functional layers arranged on one or both sides thereof), between a substrate and a laminate containing functional elements, between a first substrate and a second substrate (a laminate containing functional elements may be further formed on the side opposite to the adhesive layer of either or both of the first and second substrates), etc., using the film-like adhesive of the present invention. Therefore, one embodiment of the method for manufacturing the device of the present invention includes the following steps: configuring the film-like adhesive of the present invention on the surface of a constituent component constituting the device, configuring other constituent components constituting the device with the film-like adhesive sandwiched therebetween, and causing the film-like adhesive to undergo a curing reaction.
[0125] In the method for manufacturing the device of the present invention, the conditions of the curing reaction can be appropriately set in consideration of the type of curing agent, the heat resistance of the functional element, etc. For example, a mercury lamp or the like is used to irradiate 100 to 1500 mJ / cm 2 The ultraviolet rays can fully cure the adhesive layer. From the perspective of reducing the irradiation amount, the upper limit of the irradiation amount is preferably 700mJ / cm 2 Below, more preferably 600mJ / cm 2 the following.
[0126] Example
[0127] The present invention will be described in more detail based on the examples and comparative examples, but the present invention is not limited to the following examples. In addition, room temperature refers to 23° C., MEK is methyl ethyl ketone, PET is polyethylene terephthalate, and UV is ultraviolet light. Unless otherwise specified, "%" and "parts" are based on mass.
[0128] <Preparation of Film Adhesive>
[0129] (Example 1)
[0130] In a 1000 ml separable flask, 70 parts by mass of ST-3000 (trade name, hydrogenated bisphenol A type liquid epoxy resin, epoxy equivalent: 225 g / eq, manufactured by Nippon Steel Chemical Materials Co., Ltd.) as an epoxy resin, 30 parts by mass of YP-50 (trade name, bisphenol A type phenoxy resin, Tg: 84°C, manufactured by Nippon Steel Chemical Materials Co., Ltd.) as a phenoxy resin, and 30 parts by mass of MEK were heated and stirred at a temperature of 110°C for 2 hours to obtain a resin varnish. Furthermore, the resin varnish was transferred to an 800 ml planetary mixer, and WPI-116 (trade name, UV cationic polymerization initiator (iodonium salt type, anion site: SbF6) as a polymerization initiator was added. - ), 2 parts by mass of FUJIFILM-Wako Pure Chemical Industries, Ltd.), stirred and mixed at room temperature for 1 hour, and then vacuum degassed to obtain a mixed varnish. Then, the obtained mixed varnish was applied to a PET film with a thickness of 38 μm and subjected to surface release treatment, and heated and dried at 130° C. for 10 minutes to obtain a film-like adhesive with a release film having a length of 300 mm, a width of 200 mm, and a thickness of 20 μm.
[0131] (Example 2)
[0132] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that the phenoxy resin was changed to 86 parts by mass of YX7200B35 (trade name, phenoxy resin containing a biphenyl skeleton and a cyclohexane skeleton, Tg: 150°C, 35% by mass of non-volatile component, epoxy equivalent: 9000 g / eq, manufactured by Mitsubishi Chemical Corporation) (including 30 parts by mass of phenoxy resin (solid content)).
[0133] (Example 3)
[0134] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that the epoxy resin was changed to 70 parts by mass of 828 (trade name, bisphenol A type epoxy resin, epoxy equivalent: 185 g / eq, manufactured by Nippon Steel Chemical Materials Co., Ltd.).
[0135] (Example 4)
[0136] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that 1 part by mass of KBM-402 (trade name, silane coupling agent (3-glycidoxypropylmethyldimethoxysilane), manufactured by Shin-Etsu Chemical Co., Ltd.) was added as an additive to the mixed varnish.
[0137] (Example 5)
[0138] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that 0.1 parts by mass of 18-crown-6-ether (trade name, curing retarder, manufactured by Tokyo Chemical Industry Co., Ltd.) was added as an additive to the mixed varnish.
[0139] (Example 6)
[0140] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that the epoxy resin was changed to 50 parts by mass of ST-3000 (trade name, hydrogenated bisphenol A type liquid epoxy resin, epoxy equivalent: 225 g / eq, manufactured by Nippon Steel Chemical Materials Co., Ltd.) and 20 parts by mass of YX8040 (trade name, hydrogenated bisphenol A type solid epoxy resin, epoxy equivalent: 1200 g / eq, manufactured by Mitsubishi Chemical Corporation).
[0141] (Example 7)
[0142] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that 33 parts by mass of YC100C-MLA (trade name, silica filler slurry, solid content: 60%, manufactured by Admatechs Corporation) as a filler (including 20 parts by mass of silica filler) was added to the mixed varnish.
[0143] (Example 8)
[0144] The epoxy resin was mixed in an amount of 50 parts by mass, the phenoxy resin was mixed in an amount of 50 parts by mass, and the polymerization initiator was CPI-101A (trade name, UV cationic polymerization initiator (sulfonium salt type, anion site: SbF6 - A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that 2 parts by mass of ) was added.
[0145] (Example 9)
[0146] The polymerization initiator was CPI-101A (trade name, UV cationic polymerization initiator (sulfonium salt type, anion site: SbF6 - A film-like adhesive with a release film was obtained in the same manner as in Example 4 except that 2 parts by mass of ) was added.
[0147] (Example 10)
[0148] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that the compounding amount of the epoxy resin was 30 parts by mass and the compounding amount of the phenoxy resin was 70 parts by mass.
[0149] (Example 11)
[0150] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that the epoxy resin was blended in an amount of 50 parts by mass and the phenoxy resin was YX7180 (trade name, bisphenol F + 1,6-hexanediol diglycidyl ether type phenoxy resin, Tg: 15° C., manufactured by Mitsubishi Chemical Corporation) was used.
[0151] (Example 12)
[0152] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that the phenoxy resin was changed to 30 parts by mass of YX7180 (trade name, bisphenol F + 1,6-hexanediol diglycidyl ether type phenoxy resin, Tg: 15° C., manufactured by Mitsubishi Chemical Corporation).
[0153] (Example 13)
[0154] A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that 67 parts by mass of YC100C-MLA (trade name, silica filler slurry, solid content: 60%, manufactured by Admatechs Corporation) as a filler (including 40 parts by mass of silica filler) was added to the mixed varnish.
[0155] (Comparative Example 1)
[0156] The epoxy resin was mixed in an amount of 40 parts by mass, the phenoxy resin YX7200B35 (trade name, phenoxy resin containing a biphenyl skeleton and a cyclohexane skeleton, Tg: 150° C., non-volatile content 35% by mass, epoxy equivalent: 9000 g / eq, manufactured by Mitsubishi Chemical Corporation) was mixed in an amount of 171 parts by mass (of which phenoxy resin (solid content) was 60 parts by mass), and the polymerization initiator was CPI-100P (trade name, UV cationic polymerization initiator (sulfonium salt type, anion site: PF6 - A film-like adhesive with a release film was obtained in the same manner as in Example 2 except that 2 parts by mass of ) was added.
[0157] (Comparative Example 2)
[0158] The epoxy resin was mixed in an amount of 50 parts by mass, the phenoxy resin YX7200B35 (trade name, phenoxy resin containing biphenyl skeleton and cyclohexane skeleton, Tg: 150° C., non-volatile content 35% by mass, epoxy equivalent: 9000 g / eq, manufactured by Mitsubishi Chemical Corporation) was mixed in an amount of 142 parts by mass (of which phenoxy resin (solid content) was 50 parts by mass), and the polymerization initiator was CPI-200K (trade name, UV cationic polymerization initiator (sulfonium salt type, anion site: PF3(C2F5)3 -A film-like adhesive with a release film was obtained in the same manner as in Example 2 except that 2 parts by mass of ) was added.
[0159] (Comparative Example 3)
[0160] In the same manner as in Comparative Example 1, a film-like adhesive with a release film was obtained.
[0161] (Comparative Example 4)
[0162] The polymerization initiator was CPI-100P (trade name, UV cationic polymerization initiator (sulfonium salt type, anion site: PF6 - A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that 2 parts by mass of ) was added.
[0163] (Comparative Example 5)
[0164] The polymerization initiator was CPI-200K (trade name, UV cationic polymerization initiator (sulfonium salt type, anion site: PF3 (C2F5) 3 - A film-like adhesive with a release film was obtained in the same manner as in Example 1 except that 2 parts by mass of ) was added.
[0165] (Comparative Example 6)
[0166] A film-like adhesive with a release film was obtained in the same manner as in Comparative Example 2, except that 50 parts by mass of SG-708-6 (trade name, acrylic resin, Tg: 5°C, manufactured by Nagase ChemteX Co., Ltd.) was used instead of the phenoxy resin, and 2 parts by mass of TPO (trade name, UV free radical polymerization initiator (2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide), manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the polymerization initiator.
[0167] (Comparative Example 7)
[0168] A film-like adhesive with a release film was obtained in the same manner as in Comparative Example 6 except that 2 parts by mass of benzophenone (UV radical polymerization initiator, manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the polymerization initiator.
[0169] (Comparative Example 8)
[0170] The polymerization initiator was WPI-116 (trade name, UV cationic polymerization initiator (iodonium salt type, anion site: SbF6 - A film-like adhesive with a release film was obtained in the same manner as in Comparative Example 6 except that 2 parts by mass of ) was added.
[0171] Table 1 shows the composition of the film adhesive of each Example and Comparative Example.
[0172] <Preparation of cured product (cured sample) and confirmation of heat generation>
[0173] The release film is peeled off from the film-like adhesive with a release film obtained in each embodiment and comparative example, and the film-like adhesive is laminated to a thickness of 0.3 mm using a laminator at 70°C to obtain a laminated sample. The laminated sample is treated at room temperature (23°C) with the UV irradiation amount recorded in the "UV irradiation amount" column of the "cured sample preparation conditions" in Table 1 to obtain a cured sample (cured product) for the evaluation of the storage modulus and parallel light transmittance described later.
[0174] At this time, the sample surface temperature was measured before and after UV irradiation, and the presence or absence of heat generation due to UV irradiation was also evaluated. The surface temperature was measured using a non-contact surface thermometer (FT3700, manufactured by Hioki Electric Co., Ltd.), and the surface temperature after UV irradiation was measured within 5 seconds after UV irradiation. The surface temperature difference before and after UV irradiation (surface temperature after UV irradiation - surface temperature before UV irradiation) is recorded in Table 1.
[0175] <Determination of Storage Modulus and Glass Transition Temperature of Cured Material>
[0176] As indicators of the curing state of the film adhesive, the storage modulus and glass transition temperature of the cured product of the film adhesive were measured.
[0177] The cured sample prepared above was cut into pieces with a width of 5 mm to prepare a measurement sample.
[0178] Using the measuring device RSAIII (manufactured by TA Instruments), under the tensile conditions of 20 mm between the chucks and a frequency of 10 Hz, the viscoelastic behavior of each measured sample when heated from -40°C to 250°C at a heating rate of 5°C / min was measured, and the storage modulus and Tg at 23°C were obtained. Tg is the temperature at which the maximum value of tanδ is shown. When the maximum value is 2 or more, the temperature at which the maximum value on the low temperature side is shown is set to Tg. The measurement results are shown in Table 1.
[0179] <Parallel Light Transmittance Measurement>
[0180] The transparency of the cured product of the film-like adhesive was evaluated by the parallel light transmittance at a wavelength of 400 nm.
[0181] The cured sample prepared above was cut into 5 cm squares to prepare measurement samples.
[0182] The parallel light transmittance of each obtained measurement sample was measured using a spectrophotometer (UV-1800, manufactured by Shimadzu Corporation) to determine the parallel light transmittance at a wavelength of 400 nm.
[0183] <Adhesion reliability>
[0184] The curing state and adhesive strength of the film adhesive were evaluated using the rate of change in adhesive strength (shear strength) to the adherends (glass plate and dummy chip) bonded by the cured product of the film adhesive as an index.
[0185] 1) Preparation of samples
[0186] The film adhesive with release film obtained in each example and comparative example (before curing) was first thermally pressed onto one surface of a dummy silicon wafer (8-inch size, 350 μm thickness) using a manual laminator (trade name: FM-114, manufactured by Technovision) at a temperature of 70° C. and a pressure of 0.3 MPa. After that, the release film was peeled off from the film adhesive, and a dicing film and a dicing frame (trade name: DTF2-8-1H001, manufactured by DISCO) were pressed onto the surface of the film adhesive on the opposite side to the dummy silicon wafer using the same manual laminator at room temperature and a pressure of 0.3 MPa. Next, a cutting device (trade name: DFD-6340, manufactured by DISCO) equipped with a dual-axis dicing knife (Z1: NBC-ZH2050 (27HEDD), manufactured by DISCO / Z2: NBC-ZH127F-SE (BC), manufactured by DISCO) is used to cut (cut) the dummy silicon wafer side along the thickness direction of the film adhesive to a depth reaching the entire thickness of the film adhesive in such a manner as to form a size of 2mm×2mm, thereby obtaining a dummy chip with adhesive on the cut crystal film.
[0187] Next, using a chip bonding machine (trade name: DB-800, manufactured by Hitachi High-Technologies Corporation), pick up the above-mentioned dummy chip with adhesive from the cut crystal film, and at 80°C, pressure 0.1MPa (load 400gf), time 1.0 second, make the adhesive side of the above-mentioned dummy chip with adhesive bond and the glass plate (thickness 700μm, length 10mm×width 10mm) as the adherend substrate in the center of the glass plate and heat press bond. Next, using a UV irradiator, UV irradiate from the glass plate side with a specified UV irradiation amount (recorded in the "UV irradiation amount" column of the "reliability evaluation" of the table) to cure the adhesive. In this way, a test piece having a dummy chip-cured product of adhesive-glass plate is obtained.
[0188] 2) Determination of shear strength
[0189] The shear strength between the cured product of the adhesive of the test piece obtained above and the glass plate was measured using a universal bonding tester (trade name: Series 4000PXY, manufactured by Nordson Advanced Technology). The test conditions were set to a measurement speed of 100μm / s and a measurement height of 740μm, and the shear strength was measured when the dummy chip in the test piece was horizontally squeezed relative to the test piece. The above shear strength measurement was carried out at two measurement temperatures (normal temperature (23°C) and high temperature (100°C)), the rate of change of the shear strength was calculated, and the evaluation was performed according to the following evaluation criteria. The shear strength was measured after the adherends bonded by the cured product of the film-like adhesive were kept at the above measurement temperature for 1 minute respectively. Evaluations of A or above are qualified.
[0190] It should be noted that each of the film-like adhesives of Examples 1 to 13 exhibited sufficiently high shear strength immediately after being cured by UV irradiation.
[0191] Shear strength change rate = {(shear strength at room temperature - shear strength at high temperature) / shear strength at room temperature} × 100 [%]
[0192] -Evaluation Criteria-
[0193] AA: Shear strength change rate is less than 5%
[0194] A: The change rate of shear strength is 5% or more and less than 10%
[0195] B: The change rate of shear strength is 10% or more and less than 40%
[0196] C: The change rate of shear strength is more than 40%
[0197]
[0198]
[0199] In the above table, the amount of each component of the adhesive is expressed in parts by mass. A blank column means that the component is not contained.
[0200] As shown in the table above, when a photocationic polymerization initiator or a photoradical polymerization initiator having no antimony atom in the anion part is used as a polymerization initiator, the 2 At a low UV irradiation dose, due to poor curing, at least one of the storage modulus and Tg is low, and the bonding reliability is poor (Comparative Examples 1-2, 4-5). Furthermore, the parallel light transmittance of Comparative Examples 1 and 2 is also poor. In addition, if the UV irradiation dose is 2000mJ / cm 2The storage modulus and Tg of the film increase with the usual UV irradiation of 500 mJ / cm2, and the bonding reliability improves. However, heat is generated, and the parallel light transmittance is poor (Comparative Example 3). The reason for the decrease in parallel light transmittance is believed to be the yellowing caused by heat. If an acrylic resin is used instead of a phenoxy resin, regardless of the type of polymerization initiator, the thermal conductivity of the film increases with the temperature of 500 mJ / cm2. 2 The storage modulus, adhesion reliability and transparency were all poor under the low UV irradiation dose (Comparative Examples 6 to 8). Comparative Examples 6 to 8 were cloudy, and it is believed that the low compatibility between the acrylic resin and the epoxy resin was the cause of the poor transparency.
[0201] On the other hand, the film adhesives of Examples 1 to 13 satisfying the requirements of the present invention showed good thermal stability even when the UV irradiation dose was 500 mJ / cm 2 In the case of , the storage modulus and Tg are also high, showing excellent bonding reliability and parallel light transmittance. The film-like adhesive of the present invention can be fully cured with less irradiation, and it is known that the bonding strength, transparency and bonding reliability at high temperature are all excellent. In addition, it is known that by using the film-like adhesive of the present invention for the manufacture of devices, the reliability of the devices can be improved.
[0202] In addition, it was found that when a phenoxy resin having a Tg of 120° C. or less was used as the phenoxy resin, the transparency could be further improved (comparison between Example 1 and Example 2).
[0203] It is found that when an epoxy resin having a hydrogenated bisphenol structure is used as the epoxy resin, the transparency can be further improved (comparison between Example 1 and Example 3).
[0204] It is found that when a phenoxy resin having a Tg of 80°C or higher is used as the phenoxy resin, the adhesive strength of the cured product can be further improved. Specifically, the Tg and storage modulus of the cured product can be further increased, which contributes to the improvement of the adhesive strength (comparison between Example 1 and Examples 11 and 12).
[0205] It is found that if the content of the filler is reduced to about 20% by mass of the solid content of the film adhesive, the parallel light transmittance can be more reliably increased to 80% or more (comparison between Example 7 and Example 13).
[0206] The present invention has been described in conjunction with its embodiments, but the applicant believes that, unless otherwise specified, the present invention is not limited to any details in the description and should be broadly interpreted without violating the spirit and scope of the invention as shown in the appended claims.
[0207] This application claims priority based on Japanese Patent Application No. 2022-105913 filed in Japan on June 30, 2022, the contents of which are incorporated herein by reference as a part of the contents described in this specification.
[0208] Description of Reference Numerals
[0209] 1. Film adhesive
[0210] 2. Substrate (support substrate)
Claims
1. An energy-ray-curable film-like transparent adhesive comprising an epoxy resin, a phenoxy resin, and a photocationic polymerization initiator containing antimony in an anion site.
2. The energy-ray-curable film-like transparent adhesive according to claim 1, wherein The glass transition temperature of the phenoxy resin is 80°C to 120°C.
3. The energy-ray-curable film-like transparent adhesive according to claim 1 or 2, wherein: The glass transition temperature of a cured product of the energy ray-curable film-like transparent adhesive is 80° C. or higher.
4. The energy-ray-curable film-like transparent adhesive according to any one of claims 1 to 3, wherein The parallel light transmittance of the cured product of the energy ray-curable film-like transparent adhesive is 80% or more.
5. The energy-ray-curable film-like transparent adhesive according to any one of claims 1 to 4, wherein The storage modulus of a cured product of the energy ray-curable film-like transparent adhesive at room temperature is 1.0 GPa or more.
6. The energy-ray-curable film-like transparent adhesive according to any one of claims 1 to 5, wherein The epoxy resin has a hydrogenated bisphenol structure or a bisphenol structure. 7 . The energy-ray-curable film-like transparent adhesive according to claim 1 , comprising a silane coupling agent. 8 . The energy-ray-curable film-like transparent adhesive according to claim 1 , further comprising a curing retardant. 9 . The energy-ray-curable film-like transparent adhesive according to claim 1 , further comprising a filler. 10 . A device comprising a structure in which components are bonded together using the energy ray-curable film-like transparent adhesive according to claim 1 . 11 . A method for manufacturing a device, comprising bonding constituent members using the energy ray-curable film-like transparent adhesive according to claim 1 .
Citation Information
Patent Citations
Adhesive, adhesive sheet and display body
JP2020026491A
Film-like adhesive composition, film-like adhesive, film-like adhesive production method, semiconductor package using film-like adhesive, and production method therefor
WO2017158994A1
Sheet-like adhesive agent, sealing sheet, electronic device sealed body, and method for manufacturing electronic device sealed body
WO2020196240A1