Recycling economy from plastic waste to polyethylene and base oil by refinery hydrocracking unit
By mixing waste plastic with petroleum raw materials and sending it to a hydrocracking device for refining, the problems of low plastic regeneration rate and poor fuel quality in the prior art are solved, and plastic regeneration and circular economy with high efficiency and low energy consumption are achieved. The fuel and base oil produced have a low CO2 footprint.
Patent Information
- Application Number
- CN202380031087.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to effectively regenerate disposable plastics, especially polyethylene and polypropylene, resulting in large-scale incineration or landfill of plastic waste. The fuel quality generated by the pyrolysis method is poor and cannot be mixed into the fuel on a large scale, limiting plastic regeneration. application.
By mixing waste plastic with petroleum raw materials, a stable homogeneous mixture is formed, sent to a hydrocracking device for refining, high-quality hydrocarbon fuel and base oil are recovered, and further processed into high-quality ethylene and polyethylene products are realized to achieve plastics efficient regeneration and circular economy.
It improves the regeneration rate and product quality of plastic waste, reduces energy consumption, produces fuel and base oil with a low CO2 footprint, supports the high-quality production of polyethylene polymers, and realizes economic benefits from recycled plastics to products.
Smart Images

Figure CN119032151A_ABST
Abstract
Description
Background Art
[0001] The world's plastic production is growing extremely rapidly. According to Plastics Europe Market Research Group, the world's plastic production was 335 million tons in 2016, 348 million tons in 2017, 359 million tons in 2018, and 367 million tons in 2020. According to McKinsey & Company, if the current trajectory continues, global plastic waste is expected to reach 460 million tons per year by 2030.
[0002] Single-use plastic waste has become an increasingly important environmental issue. Currently, there seem to be few options for recycling polyethylene and polypropylene waste plastics into value-added chemicals and fuel products. Currently, only a small amount of polyethylene and polypropylene is recycled through chemical recycling, where the recycled and clean polymer pellets are pyrolyzed in a pyrolysis unit to make fuels (naphtha, diesel), steam cracker feed or slack wax. The vast majority, more than 80%, is incinerated, landfilled or discarded.
[0003] Current methods of chemical regeneration through pyrolysis have not had much impact on the plastics industry. Current pyrolysis operations produce fuel components (naphtha and diesel series products) of poor quality, but in small enough quantities that these products can be blended into the fuel supply. However, if large amounts of waste polyethylene and polypropylene are to be recycled to address environmental concerns, this simple blending cannot continue. The products produced by pyrolysis units are too poor quality to be blended into transportation fuels in large quantities.
[0004] Methods for converting waste plastics into hydrocarbon lubricants are known. For example, U.S. Pat. No. 3,845,157 discloses the cracking of waste or virgin polyolefins such as ethylene / olefin copolymers to form gaseous products, which are further processed to produce synthetic hydrocarbon lubricants. U.S. Pat. No. 4,642,401 discloses the production of liquid hydrocarbons by heating pulverized polyolefin waste at a temperature of 150-500° C. and a pressure of 20-300 bar. U.S. Pat. No. 5,849,964 discloses a method for depolymerizing waste plastic materials into a volatile phase and a liquid phase. The volatile phase is separated into a gas phase and a condensate. The liquid phase, condensate and gas phase are refined into liquid fuel components using standard refining techniques. U.S. Pat. No. 6,143,940 discloses a process for converting waste plastics into heavy wax compositions. U.S. Pat. No. 6,150,577 discloses a method for converting waste plastics into lubricating oils. EP0620264 discloses a process for producing lubricating oil from waste or virgin polyolefins by thermally cracking the waste in a fluidized bed to form a waxy product, optionally using hydrotreatment, followed by catalytic isomerization and fractionation to recover the lubricating oil.
[0005] U.S. Patent Application Publication No. 2021 / 0130699 discloses a method and system for preparing recycle content hydrocarbons from recycled waste. The recycled waste is pyrolyzed to form a pyrolysis oil composition, at least a portion of which can then be cracked to form a recycle olefin composition.
[0006] Other documents related to methods for converting waste plastics into lubricating oils include U.S. Patent Nos. 6288296, 6774272, 6822126, 7834226, 8088961, 8404912, and 8696994, and U.S. Patent Application Publication Nos. 2019 / 0161683, 2016 / 0362609, and 2016 / 0264885. The aforementioned patent documents are incorporated herein by reference in their entirety.
[0007] Globally, there is a great interest in the recycling or upcycling of plastic waste in order to save resources and the environment. Mechanical recycling of plastic waste is quite limited due to the different types, properties, additives and contaminants of collected plastics. Usually, recycled plastics have degraded quality. Chemical recycling to obtain starting materials or value-added chemicals has become a more desirable route.
[0008] However, to achieve chemical recycling of industrially large quantities of single-use plastics to reduce their environmental impact, more robust approaches are needed. Improved approaches should establish a "circular economy" for waste polyethylene and polypropylene plastics, in which used waste plastics are effectively recycled back into the starting material for polymers or value-added chemicals or fuels. Summary of the invention
[0009] A continuous process for converting waste plastics into recyclables for polyethylene polymerization is provided. The method comprises selecting waste plastics containing polyethylene and / or polypropylene. These waste plastics are then blended with petroleum feedstocks. The resulting blend is typically a stable blend and homogeneous mixture (especially at a temperature below the melting point of the waste plastics). The blend comprises less than about 20% by weight of the selected waste plastics. The blend is then fed to a hydrocracking unit in a refinery along with conventional refinery feeds such as VGO.
[0010] Integration of the process with an oil refinery is an important aspect of the process of the invention and allows the creation of a circular economy using single-use waste plastics such as polyethylene. The blend is thus sent to a refinery hydrocracking unit. The blend is conveyed at a temperature above its pour point so that the blend can be pumped to the refinery hydrocracking unit. Prior to injection into the hydrocracking unit, the blend is heated to above the melting point of the plastic. The C-containing plastic is recovered from the hydrocracking unit.3 -C 4 LPG streams containing hydrocarbons and C 5 -C 8 The C 3 -C 4 The and naphtha streams can be sent to a steam cracker to produce ethylene. A heavy fraction is also recovered from the hydrocracking unit and sent to an isomerization / dewaxing unit. Quality base oils can be recovered from the dewaxing unit and then sent to a hydrofinishing unit for further processing to produce truly premium base oils.
[0011] In another embodiment, LPG and naphtha (C 5 -C 8 ) fraction and sends it to a steam cracker to produce ethylene.
[0012] A refinery will typically have its own hydrocarbon feeds flowing through the refinery units. An important aspect of the process of the present invention is that it does not negatively impact the operation of the refinery. The refinery must still produce valuable chemicals and fuels. Otherwise, combining the process with an oil refinery would not be a viable solution. Therefore, the flow volume must be carefully observed.
[0013] The flow volume of the waste plastic / petroleum blend entering the refinery device may include any actual or adapted volume percentage of the total flow entering the refinery device. Typically, the flow of the blend may be up to about 100% by volume of the total flow, i.e., the blend flow is the entire flow without the refinery flow. In one embodiment, the flow of the blend is an amount that accounts for up to about 50% by volume of the total flow (i.e., the refinery flow and the mixture flow).
[0014] It has been found that, among other factors, by increasing refinery operations, plastic waste can be efficiently and effectively regenerated while also supplementing refinery operations in the preparation of higher value products such as gasoline, jet fuel, base oils and diesel. It has also been found that by increasing refinery operations, clean ethylene can be efficiently and effectively produced from waste plastics for final polyethylene polymer production. The entire process from recycled plastics to polyethylene products having the same product quality as the original polymer achieves positive economic benefits. The inventive method can also regenerate waste plastics to prepare excellent / high quality base oils while also preparing polyethylene products. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 depicts current practices for pyrolyzing waste plastics to produce fuel or wax.
[0016] Figure 2The process of the present invention is described for preparing a hot, homogeneous liquid blend of plastic and petroleum feedstock, and how the blend can be sent to a refinery conversion unit.
[0017] Figure 3 The preparation of a stable blend is described in detail, as well as how the stable blend can be sent to a refinery conversion unit.
[0018] Figure 4 The classification of plastic types for recycling of waste plastics is described.
[0019] Figure 5 The process of the invention is described in which the prepared blend is sent to a refinery hydrocracking unit.
[0020] Figure 6 Graph showing thermogravimetric analysis (TGA) of the thermal stability of polyethylene and polypropylene. DETAILED DESCRIPTION
[0021] In the inventive method, a method for regenerating waste polyethylene and / or polypropylene back to original polyethylene is provided, which establishes a circular economy by combining different industrial processes. And in one embodiment, due to the integration of the method with a refinery, high-quality base oils can be obtained. A large part of polyethylene and polypropylene polymers are used for disposable plastics and are discarded after use. Disposable plastic waste has become an increasingly important environmental problem. At present, the selection of polyethylene and polypropylene waste plastics to be recycled into value-added chemicals and fuel products seems to be few. Currently, only a small amount of polyethylene / polypropylene is regenerated by a chemical regeneration process, wherein the regenerated and cleaned polymer pellets are pyrolyzed in a pyrolysis unit to make fuels (naphtha, diesel), steam cracker feed or slack wax.
[0022] Ethylene is the largest petrochemical base stock produced. Hundreds of millions of tons of ethylene are produced annually by steam cracking. Steam crackers use either gaseous feeds (ethane, propane and / or butane) or liquid feeds (naphtha or gas oil). It is a non-catalytic cracking process that operates at very high temperatures, up to 850°C.
[0023] Polyethylene is used in a wide variety of consumer and industrial products. Polyethylene is the most common plastic, with more than 100 million tons of polyethylene resin produced each year. Its main use is in packaging (plastic bags, plastic films, geomembranes, containers including bottles, etc.). Polyethylene is produced in three main forms: high-density polyethylene (HDPE, ~0.940-0.965 g / cm -3 ), linear low-density polyethylene (LLDPE, ~0.915-0.940g / cm -3 ) and low-density polyethylene (LDPE, <0.930 g / cm -3 ), have the same chemical formula (C2 H 4 ) n But the molecular structures are different. HDPE has low branching and short side chains, while LDPE has very high branching and long side chains. LLDPE is a basic linear polymer with a large number of short branches, usually made by copolymerizing ethylene with short-chain α-olefins.
[0024] Low density polyethylene (LDPE) is produced by free radical polymerization at 150–300°C and ultra-high pressure of 1000-3000 atmospheres. The method uses a small amount of oxygen and / or an organic peroxide initiator to produce a polymer having an average of about 4000–40,000 carbon atoms per polymer molecule and having many branches. High density polyethylene (HDPE) is manufactured at relatively low pressure (10-80 atmospheres) and 80-150°C temperature in the presence of a catalyst. Ziegler-Nat ta organometallic catalysts (titanium (III) chloride and alkyl aluminum) and Phil lips type catalysts (chromium (IV) oxide on silica) are typically used and produced by a slurry process using a loop reactor or by a gas phase process using a fluidized bed reactor. Hydrogen is mixed with ethylene to control the chain length of the polymer. Linear low-density polyethylene (LLDPE) is manufactured under similar conditions to HDPE, except that ethylene is copolymerized with short-chain α-olefins (1-butene or 1-hexene).
[0025] Today, as mentioned above, only a small portion of used polyethylene products are collected for recycling due to ineffective and inefficient recycling efforts.
[0026] FIG. 1 shows a diagram of the pyrolysis of waste plastics into fuel or wax, which is commonly operated in today's industry. Typically, waste plastics are sorted together 1. Cleaned plastic waste 2 is converted into waste gas 4 and pyrolysis oil (liquid product) in a pyrolysis unit 3. The waste gas 4 from the pyrolysis unit 3 is used as fuel for operating the pyrolysis unit. The distillation unit on site separates the pyrolysis oil to produce naphtha and diesel 5 products, which are sold to the fuel market. The heavy pyrolysis oil fraction 6 is recycled back to the pyrolysis unit 3 to maximize the fuel yield. Charcoal 7 is removed from the pyrolysis unit 3. The heavy fraction 6 is rich in long-chain linear hydrocarbons and is very waxy (i.e., paraffin is formed when cooled to ambient temperature). Wax can be separated from the heavy fraction 6 and sold to the wax market.
[0027] However, the method of the present invention does not pyrolyze waste plastics. Instead, a stable blend of petroleum feedstock and waste plastics is prepared. Therefore, the pyrolysis step can be avoided, which greatly saves energy.
[0028] The present blend is prepared in a hot blend preparation unit, wherein the operating temperature is above the melting point of the plastic (about 150-250°C) to form a hot homogenous liquid blend of the plastic and oil. The hot homogenous liquid blend of the plastic and oil can be sent directly to a refinery unit.
[0029] Alternatively, the blend is prepared in a stable blend preparation unit, where the hot homogenous liquid blend is cooled to ambient temperature in a controlled manner to allow for easy storage and transportation. By using this method, a stable blend can be prepared in a facility remote from the refinery and transported to the refinery unit. The stable blend is then heated to above the melting point of the plastic to feed the refinery conversion unit. The stable blend is a physical mixture of finely suspended microcrystalline plastic particles in a petroleum-based oil. The mixture is stable and the plastic particles do not precipitate or agglomerate when stored for long periods of time.
[0030] The meaning of heating the blend to a temperature above the melting point of the plastic is clear when a single plastic is used. However, if the waste plastic contains more than one waste plastic, the melting point of the plastic with the highest melting point is exceeded. Therefore, the melting points of all plastics must be exceeded. Similarly, if the blend is cooled to below the melting point of the plastic, the temperature must be cooled to below the melting points of all plastics that make up the blend.
[0031] Compared to pyrolysis units, these blend preparation units operate at much lower temperatures (~500-600°C vs. 120-250°C). Thus, the process of the present invention is a far more energy efficient method for preparing refinery feedstocks derived from waste plastics than thermal cracking processes such as pyrolysis.
[0032] The use of the waste plastic / petroleum blend of the present invention further increases the total hydrocarbon yield obtained from the waste plastic. This increase in yield is significant. The hydrocarbon yield using the blend of the present invention provides a hydrocarbon yield of up to 98%. In contrast, pyrolysis produces a large amount of light products (about 10-30% by weight) from plastic waste, and about 5-10% by weight of char. As mentioned above, these light hydrocarbons are used as fuel to operate the pyrolysis plant. Therefore, the liquid hydrocarbon yield of the pyrolysis plant is at most 70-80%.
[0033] When the blend of the present invention is fed to a refinery unit such as a hydrocracker, only a small amount of waste gas is generated. The catalytic cracking process used in refinery units such as hydrocrackers is different from the thermal cracking process used in pyrolysis. The production of undesirable light byproducts such as methane and ethane can be minimized by the catalytic process. The refinery unit has efficient product fractionation and can efficiently utilize all hydrocarbon product streams to produce high value materials. The refinery co-feed will only generate about 2% waste gas (H 2 , methane, ethane, ethylene). C 3 and C4 Streams are captured to produce useful products such as recycled polymer products, while other hydrocarbon streams can be captured to produce quality fuel products including premium base oils. Thus, use of the petroleum / plastic blends of the present invention increases hydrocarbons obtained from plastic wastes, as well as providing a more energy efficient regeneration process, compared to thermal processes such as pyrolysis.
[0034] The process of the present invention converts disposable waste plastics in large quantities by integrating the waste plastics blended with petroleum product streams into oil refinery operations. The resulting process produces feedstock for polymers (naphtha or C for ethylene crackers) 3 and C 4 ), high quality gasoline, jet fuel and diesel and / or quality base oils.
[0035] In general, the process of the present invention provides a circular economy for polyethylene plants. Polyethylene is produced by polymerizing pure ethylene. Clean ethylene can be produced by steam cracking. 3 or C 4 The stream is sent to a steam cracker where ethylene is polymerized to form polyethylene.
[0036] By increasing refinery operations, upgrading waste plastics to higher value products (gasoline, jet fuel, diesel, and base oils), and producing clean ethylene for final polyethylene polymer production, positive economic benefits are achieved for the entire process from recycled plastics to polyethylene products (product quality is the same as the original polymer). Moreover, by integrating the regeneration method of the present invention with oil refinery operations, a more energy efficient and effective process is achieved while avoiding any problems with refinery operations.
[0037] The integration of refinery operations becomes very important in another aspect. Waste plastics contain pollutants, such as calcium, magnesium, chlorides, nitrogen, sulfur, dienes and heavy components, and these products cannot be used in large quantities and blended into transportation fuels. It has been found that by passing these products through a refinery unit, pollutants can be captured in a pre-treatment unit, reducing their negative impact. The fuel component can be further upgraded by using a suitable refinery unit of a chemical conversion process, and the quality of the final transportation fuel produced in the integrated process is higher and meets the fuel quality requirements. The integrated process will produce a cleaner and purer ethylene stream for polyethylene production. These large-scale on-spec productions make the "circular economy" of recycled bioplastics possible.
[0038] The carbon going in and out of the refinery operations is “transparent,” meaning that not all molecules in the waste plastic may end up in the exact olefin product that is looped back into the polyolefin plant, but are still considered a “credit” because the net “green” carbon going in and out of the refinery is positive. Through these integrated approaches, the amount of virgin feed required for the polyethylene plant is significantly reduced.
[0039] In some cases, converting waste plastics into clean fuels requires less energy than producing fuels and base oils from virgin petroleum feedstocks. As waste plastic collection and processing improve, energy efficiency gains will continue to increase. Such fuels and base oils produced from blends of waste plastics and oils have a recycled component and a lower carbon footprint than corresponding fuels and base oils made from pure petroleum feedstocks. The method of the present invention can use waste plastics to produce a product containing recycled components and a lower CO 2 Clean gasoline, jet fuel, diesel, and base oils with a (lower carbon) footprint.
[0040] Figure 2 A method for preparing a hot homogeneous blend of plastic and petroleum feedstock is shown, the blend being used for direct injection into a hydrocracking unit in the process of the present invention, wherein a hot homogeneous liquid blend of plastic and oil is prepared in a hot blend preparation unit. The preferred range of the plastic component in the blend is about 1-20% by weight. If high molecular weight polypropylene (average molecular weight of 250,000 or greater) waste plastic or high density polyethylene (density greater than 0.93 g / cc) is used as the main waste plastic, such as at least 50% by weight, the amount of waste plastic used in the blend is more preferably about 10% by weight. The reason is that the pour point and viscosity of the blend will be high.
[0041] Preferred conditions for the preparation of the hot homogeneous liquid blend include heating the plastic to a temperature above the melting point of the plastic while vigorously mixing with the petroleum feedstock. Preferred process conditions include heating to a temperature of 250-550°F, a residence time of 5-240 minutes at the final heating temperature, and 0-10 psig atmospheric pressure. This can be done in an open atmosphere, and preferably in an oxygen-free inert atmosphere.
[0042] With reference to the attached drawings Figure 2, showing a step-by-step preparation method for preparing a hot homogeneous liquid blend. Mixed waste plastics are sorted to produce post-consumer waste plastics 21 comprising polyethylene and / or polypropylene. The waste plastics are cleaned 22 and then mixed with oil 24 in a hot blend preparation unit 23. After mixing in 23, a homogeneous blend of plastic and oil 25 is recovered. Optionally, a filtering device (not shown) can be added to remove any undissolved plastic particles or any solid impurities present in the hot liquid blend. The hot blend of plastic and oil can then be combined with a refinery feedstock (e.g., vacuum gas oil (VGO) 20) to become a mixture of plastic / oil blend and VGO 26, which can then be sent to a refinery unit. In the process of the present invention, the refinery unit in one embodiment is a hydrocracking unit.
[0043] Figure 3 The method for preparing a stable blend of plastic and oil used in the method of the present invention is shown. The stable blend is prepared in a stable blend preparation device by a two-step process. The first step is to produce a hot, homogeneous liquid blend of the plastic melt and the petroleum raw material. This step is similar to Figure 2 The hot blend preparation described in is the same. The preferred range of the plastic component in the blend is about 1-20% by weight. If high molecular weight polypropylene (average molecular weight of 250,000 or more) waste plastic or high density polyethylene (density higher than 0.93 g / cc) is used as the main waste plastic, for example, at least 50% by weight, the amount of waste plastic used in the blend is more preferably about 10% by weight. The reason is that the pour point and viscosity of the blend will be high.
[0044] Preferred conditions for the preparation of the hot homogeneous liquid blend include heating the plastic to above the melting point of the plastic while vigorously mixing with the petroleum feedstock. Preferred process conditions include heating to a temperature of 250-500°F, a residence time of 5-240 minutes at the final heating temperature, and 0-10 psig atmospheric pressure. This can be done in an open atmosphere, and preferably in an oxygen-free inert atmosphere.
[0045] In a second step, the hot blend is cooled to below the melting point of the plastic while continuing to vigorously mix with the petroleum feedstock and then further cooled to a lower temperature, preferably to ambient temperature, to produce a stable blend of plastic and oil.
[0046] It has been found that a stable blend is an intimate physical mixture of plastic and petroleum feedstock. The plastic is in a "depolymerized" state. The plastic remains in a finely dispersed state of solid particles in the petroleum feedstock at temperatures below its melting point, particularly at ambient temperature. The blend is stable, allowing for easy storage and transportation. At the refinery, the stable blend is heated in a preheater to above the melting point of the plastic to produce a hot homogenous liquid blend of the plastic and petroleum. The hot liquid blend can then be sent to the refinery hydrocracking unit as a co-feed with conventional refinery feedstocks.
[0047] exist Figure 3 , more details of the preparation of a stable blend are shown. The stable blend is made in a two-step process in a stable blend preparation device 100. As shown, clean waste 22 is conveyed to a stable blend preparation device 100. The selected plastic waste 22 is heated and mixed with a refinery feedstock oil 24. The plastic waste is heated to a temperature higher than the melting point of the plastic to melt the plastic. The petroleum feedstock is mixed with the heated plastic at 23. The mixing is usually very intense. The mixing and heating conditions can generally include heating at a temperature in the range of about 250-500°F, with a residence time of 5-240 minutes at the final heating temperature. The heating and mixing can be carried out in an open atmosphere or in an oxygen-free inert atmosphere. The result is a hot homogeneous liquid blend 25 of plastic and oil. Optionally, a filtering device (not shown) can be added to remove any undissolved plastic particles or any solid impurities present in the hot homogeneous liquid blend.
[0048] The hot blend 25 is then cooled to below the melting point of the plastic while mixing of the plastic with the petroleum feedstock continues 101. Cooling generally continues, typically to ambient temperature, to produce a stable blend of plastic and oil 102. At the refinery, the stable blend may be sent to a preheater 50, which heats the blend to above the melting point of the plastic to produce a mixture of the plastic / oil blend and VGO 26, which is then sent to a refinery conversion unit, such as a hydrocracking unit.
[0049] The preferred plastic starting material for the process of the present invention is sorted waste plastics containing mainly polyethylene and polypropylene (plastic recycling classification types 2, 4 and 5). The pre-sorted waste plastics are cleaned and shredded or granulated for feeding to the blend preparation device. Figure 4 The classification of plastic types for waste plastic recycling is shown. Classification types 2, 4 and 5 are high density polyethylene, low density polyethylene and polypropylene respectively. Any combination of polyethylene and polypropylene waste plastics can be used. For the method of the present invention, at least some polyethylene waste plastics are preferred. Polystyrene (Class 6) can also exist in a limited amount.
[0050] In order to minimize contaminants such as N, Cl and S, it is very important to sort the waste plastics properly. Plastic wastes containing polyethylene terephthalate (plastic recycling classification type 1), polyvinyl chloride (plastic recycling classification type 3) and other polymers (plastic recycling classification type 7) need to be sorted to less than 5%, preferably less than 1%, and most preferably less than 0.1%. The method of the present invention can tolerate a moderate amount of polystyrene (plastic recycling classification type 6). Waste polystyrene needs to be sorted to less than 20%, preferably less than 10%, and most preferably less than 5%.
[0051] Washing of waste plastics can remove metal contaminants such as sodium, calcium, magnesium, aluminum, and non-metallic contaminants from other waste sources. Non-metallic contaminants include contaminants from Group IV of the periodic table, such as silicon dioxide; contaminants from Group V, such as phosphorus and nitrogen compounds; contaminants from Group VI, such as sulfur compounds; and halide contaminants from Group VII, such as fluoride, chloride, and iodide. Residual metals, non-metallic contaminants, and halides need to be removed to less than 50 ppm, preferably less than 30 ppm, and most preferably less than 5 ppm.
[0052] If cleaning does not adequately remove metals, non-metallic contaminants, and halide impurities, separate guard beds may be used to remove metals and non-metallic contaminants.
[0053] The petroleum blended with waste plastics is generally a petroleum feedstock for a refinery. Preferably, the petroleum blended oil is the same as the petroleum feedstock for a refinery. Petroleum can also include any petroleum-derived oil or petroleum-based materials. In one embodiment, the petroleum feedstock oil can include atmospheric gas oil, vacuum gas oil (VGO), atmospheric residue or heavy materials recovered from other refinery operations. In one embodiment, the petroleum feedstock oil blended with waste plastics includes VGO. In one embodiment, the petroleum feedstock oil blended with waste plastics includes light cycle oil (LCO), heavy cycle oil (HCO), FCC naphtha, gasoline, diesel, toluene and / or petroleum-derived aromatic solvents.
[0054] Figure 5 One embodiment of the integrated process of the present invention is shown wherein the blend is sent to a hydrocracking unit. Figure 5 Zhongyu Figure 2 and Figure 3 Like numbers refer to like items / devices. As shown, the selected waste 21 is cleaned 22 and then sent to the blend preparation unit 23 where the plastic and refinery feedstock 24 are mixed to produce a hot blend of plastic and oil 25. If desired, oil refinery feedstock, such as vacuum gas oil (VGO) 20, can be added to the blend. If the plastic / oil blend is still hot ( Figure 225), it can be mixed immediately with the co-feed oil 20. However, if the plastic / oil stabilized blend requires heating ( Figure 3 102), a preheater is usually used ( Figure 3 The blend is heated to a temperature above the melting point of the plastic in a preheater 50 in the reactor prior to mixing with the co-feed VGO oil. This homogenous plastic / oil blend and VGO oil 26 are then sent to a hydrocracking unit 27 in a refinery. In another embodiment, the heated blend and the refinery feedstock are each sent directly but separately to the hydrocracking unit.
[0055] Refineries will often have their own hydrocarbon feeds flowing through the refinery units. In this case, Figure 5 As shown, the hydrocarbon feed is VGO 20. The flow volume of the blend sent to the refinery unit (here, a hydrocracking unit) can account for any actual or adapted volume % of the total flow sent to the refinery unit. In general, for practical reasons, the flow of the blend can be up to about 50% by volume of the total flow (i.e., the refinery flow and the blend flow). In one embodiment, the flow of the blend is an amount of up to about 100% by volume of the total flow. In another embodiment, the flow volume of the blend is an amount of up to about 25% by volume of the total flow. It has been found that about 50% by volume is a fairly practical amount in terms of its impact on the refinery, while also providing excellent results and being an amount that can be adapted. It is important to avoid any negative impact on the refinery and its products. If the amount of plastic in the final blend (including the plastic / oil blend and the co-feed petroleum) is greater than 20% by weight of the final blend, difficulties in operating the refinery unit may occur. The final blend refers to the plastic / oil blend of the present invention and any co-feed petroleum. The plastic / oil blend may comprise up to 100% by volume of the feed to the refinery unit and may therefore comprise the entire final blend.
[0056] Any suitable hydrocracking operation can be run. The catalyst in the hydrocracker can be selected from any known hydrocracking catalyst. Hydrocracking conditions typically include a temperature range of 175°C to 485°C, a molar ratio of hydrogen to hydrocarbon charge of 1 to 100, a pressure range of 0.5 to 350 bar, and a liquid hourly space velocity (LHSV) range of 0.1 to 30. In the hydrocracking reactor, larger molecules are cracked into smaller molecules. Hydrocracking catalysts typically contain large pore zeolites (such as USY) and various combinations of Group VI and Group VIII base metals (such as nickel, cobalt, molybdenum and tungsten) finely dispersed on alumina or oxide carriers.
[0057] Recovery of LPG C from the hydrocracking unit 27 3 -C 4The feed stream 30, the clean naphtha stream 31 and the heavy fraction 28. The heavy fraction 28 is sent to the isomerization / dewaxing unit 29. In the hydrocracking reactor, the feed can first be contacted with a hydrotreating catalyst under hydrotreating conditions in a hydrotreating zone or a protective layer to provide a hydrotreated feedstock. The hydrotreating catalyst generally contains various combinations of Group VI and Group VIII base metals (such as nickel, cobalt, molybdenum and tungsten) finely dispersed on an alumina or oxide support. The feedstock is contacted with the hydrotreating catalyst in the protective layer, which can effectively hydrogenate the aromatics in the feedstock and remove N and S containing compounds from the feed, thereby protecting the hydroisomerization catalyst of the catalyst system. "Effectively hydrogenate aromatics" means that the hydrotreating catalyst is able to reduce the aromatic content in the feedstock by at least about 20%. The hydrotreated feedstock may generally contain C 10+ normal paraffins and slightly branched isoparaffins, and the wax content is typically at least about 20%.
[0058] The hydroisomerization catalyst that can be used in the process of the present invention typically contains a catalytically active hydrogenation metal. The presence of a catalytically active hydrogenation metal leads to an improvement in the product, particularly VI and stability. Typical catalytically active hydrogenation metals include chromium, molybdenum, nickel, vanadium, cobalt, tungsten, zinc, platinum and palladium. Metallic platinum and palladium are particularly preferred, most particularly preferably platinum. If platinum and / or palladium are used, the total amount of active hydrogenation metal is typically 0.1% to 5% by weight, typically 0.1% to 2% by weight, of the total amount of catalyst. In addition, the hydroisomerization catalyst typically contains a medium pore size zeolite dispersed on an oxide support, such as ZSM-23, ZSM-48, ZSM-35, SSZ-32, SSZ-91.
[0059] The refractory oxide support may be selected from those oxide supports commonly used for catalysts, including silica, alumina, silica-alumina, magnesia, titania, and combinations thereof.
[0060] The conditions in the isomerization / dewaxing reactor unit 29 typically include temperatures in the range of about 390°F to about 800°F (199°C to 427°C). In one embodiment, the hydroisomerization dewaxing conditions include temperatures in the range of about 550°F to about 700°F (288°C to 371°C). In another embodiment, the temperature may be in the range of about 590°F to about 675°F (310°C to 357°C). The total pressure may be in the range of about 500 to about 3000 psig (0.10 to 20.68 MPa), and is typically in the range of about 750 to about 2500 psig (0.69 to 17.24 MPa).
[0061] Dewaxed oil 33 can be recovered from the isomerization / dewaxing unit 29, and the oil can be used as a base oil, and the oil can also be sent to a hydrofinishing unit 34 to prepare a high-quality base oil 35. In the hydrofinishing unit 34, hydrofinishing can be carried out in the presence of a hydrogenation catalyst, as known in the art. The hydrogenation catalyst used for hydrofinishing can include, for example, platinum, palladium, or a combination thereof on an alumina carrier. Hydrofinishing can be carried out at a temperature in the range of about 350°F to about 650°F (176°C to 343°C) and a pressure in the range of about 400 psig to about 4000 psig (2.76 to 27.58 1MPa). Hydrofinishing for the production of lubricating oils is described, for example, in U.S. Pat. No. 3,852,207, the disclosure of which is incorporated herein by reference.
[0062] The LPG stream 30 and the clean naphtha stream 31 may be sent to a steam cracker 40 to produce ethylene 36. The naphtha stream 31 may be sent in whole or in part to the steam cracker 40 because it also contains clean gasoline, jet fuel, and diesel fuel fractions. At least a portion of the naphtha stream 31 may also be sent to a gasoline pool or upgrading process to upgrade the fuel fractions, especially jet fuel. The LPG and naphtha 32 may also be recovered from the dewaxing unit 29 and sent as feedstock to the steam cracker 40 to produce ethylene 36. The ethylene is sent to an ethylene polymerization unit 41 to produce polyethylene, which is further processed to produce various polyethylene products 42 to meet consumer demand.
[0063] Preferably, the steam cracker and ethylene polymerization unit are located near the refinery so that the raw materials (propane, butane, naphtha or ethylene) can be transported by pipeline. For petrochemical plants far from refineries, the raw materials can be transported by truck, barge, rail car or pipeline.
[0064] The benefits of a circular economy and effective and efficient regeneration activities are achieved through the integrated approach of the present invention.
[0065] The following examples are provided to further illustrate the methods of the present invention and their benefits. These examples are for illustrative purposes only and are not intended to be limiting.
[0066] Example 1: Properties of plastic samples and raw materials used for blend preparation
[0067] Four plastic samples were purchased: low density polyethylene (LDPE, Plastic A), high density polyethylene (HDPE, Plastic B), and two polypropylene samples with average molecular weights of ~12,000 (PP, Plastic C) and ~250,000 (PP, Plastic D), and their properties are summarized in Table 1.
[0068] Table 1: Properties of the plastics used
[0069]
[0070] The petroleum feedstocks used to prepare stable blends with plastics include hydrotreated vacuum gas oil (VGO), Aromatic 100 solvent, light cycle oil (LCO) and diesel. Their properties are shown in Table 2 below. Aromatic 100 is a commercially available aromatic solvent made from petroleum-based materials, mainly containing C9-C10 dialkyl and trialkyl benzenes.
[0071] Table 2: Properties of petroleum feedstocks used in blend preparation
[0072]
[0073]
[0074] Thermogravimetric analysis (TGA) was performed on Plastic A (LDPE) and Plastic C (PP) to verify that the plastic materials were thermally stable at temperatures well above the melt preparation temperature. Figure 6 The TGA results shown indicate that the LDPE sample is stable up to 800°F, while the polypropylene sample is stable up to 700°F.
[0075] Example 2: Production of Feedstock C from Waste Plastic / Oil Blend Co-fed to Refinery Hydrocracking Unit 3 -C 4 and / or naphtha
[0076] By feeding the plastic / oil blend of the present invention (with or without co-feed) to a hydrocracking unit, the blend is converted and fractionated into multiple components. A refinery hydrocracking unit produces significant amounts of clean propane, butane, and naphtha streams, as well as other streams for refinery conversion units and for polyethylene production.
[0077] Example 3: Hydrocracking of plastic and petroleum blends to produce a plastic with renewable content and low CO 2 Footprint of fuels and base oils
[0078] Gasoline, jet fuel, diesel and heavy fractions from the hydrocracker effluent distillation column can be sent to the corresponding blending tanks to blend into a fuel with renewable components and low CO 2 The heavy fraction can be further processed in an isomerization / dewaxing unit to produce a product with a renewable component and lower CO 2 Footprint base oil or white oil ( Figure 5 ).
[0079] Example 4: Regeneration product C 3 -C4 and / or naphtha to steam crackers to produce ethylene, and then polyethylene resins and polyethylene consumer products, as well as base oils
[0080] According to Example 2, a propane, butane and naphtha stream produced by co-feeding a plastic / oil blend into a hydrocracking unit is co-fed as a good raw material to a steam cracker to produce ethylene with a recycled component. At least a portion, if not all, of the stream can be fed to a steam cracker. Ethylene can be processed in a polymerization unit to produce polyethylene resins containing some materials derived from recycled polyethylene / polypropylene, and the quality of the newly produced polyethylene is no different from that of virgin polyethylene made entirely from virgin petroleum resources. The polyethylene resin with recycled materials can then be further processed to produce a variety of polyethylene products to meet the needs of consumer products. These polyethylene consumer products now contain chemically recycled recycled polymers, and the quality of the polyethylene consumer products is no different from that of products made entirely from virgin polyethylene polymers. These chemically recycled polymer products are different from mechanically recycled polymer products, the latter of which are not as good as polymer products made from virgin polymers ( Figure 5 ).
[0081] The heavy fraction from the hydrocracking unit can also be sent to the isomerization / dewaxing unit. Dewaxed oil or base oil can be recovered from the unit and can be further sent to the hydrofining unit to prepare high-quality base oil or white oil ( Figure 5 ).
[0082] As used in this disclosure, the words "comprising" or "including" are intended to be open transitional terms, meaning the inclusion of specified elements but not necessarily the exclusion of other unspecified elements. The phrase "consisting essentially of is intended to mean the exclusion of other elements having any significant significance to the composition. The phrase "consisting of is intended to be a transitional term, meaning the exclusion of all elements other than the listed elements, with the exception of minor trace amounts of impurities.
[0083] All patents and publications cited herein are incorporated herein by reference to the extent that they do not conflict with this article. It should be understood that some of the above-mentioned structures, functions and operations of the above-mentioned embodiments are not necessary for practicing the present invention, but are included in the specification only for the completeness of the exemplary embodiments. In addition, it should be understood that the specific structures, functions and operations set forth in the above-mentioned cited patents and publications can be practiced in conjunction with the present invention, but they are not essential for the practice of the present invention. Therefore, it should be understood that the present invention can be implemented in a manner other than the specific description without really departing from the spirit and scope of the present invention as defined by the appended claims.
Claims
1. A continuous process for converting waste plastics into regenerants for polyethylene polymerization, comprising: (a) selecting waste plastics comprising polyethylene and / or polypropylene; (b) preparing a blend of petroleum and a selected waste plastic, wherein the blend comprises about 20% by weight or less of the selected waste plastic; (c) sending the blend to a refinery hydrocracking unit at a temperature above the melting point of the waste plastic in the blend; (d) recovering a liquefied petroleum gas C3-C4 olefin / paraffin mixture from the hydrocracking unit; and (e) sending the C3-C4 mixture to a steam cracker to produce ethylene.
2. The process according to claim 1, wherein a naphtha stream is also recovered from the hydrocracking unit and at least a portion thereof is sent as feed to the steam cracker for producing ethylene.
3. The method of claim 1, wherein the blend of (b) is a hot, intimate blend of waste plastic and petroleum.
4. The method of claim 1, wherein the blend of (b) is a stable blend of waste plastic and petroleum.
5. The method of claim 1, wherein the ethylene is polymerized into polyethylene.
6. The method according to claim 1, wherein the waste plastics selected in (a) comprise plastics from classification groups 2, 4 and / or 5.
7. The process as claimed in claim 1, wherein gasoline is recovered from the refinery hydrocracking unit and sent to a gasoline blending pool.
8. The process of claim 2, wherein a portion of the naphtha stream recovered from the hydrocracking unit is further processed in a refinery into clean gasoline, diesel or jet fuel.
9. The method of claim 8, wherein the jet fuel is recovered from further processing in a refinery.
10. The process of claim 1, wherein the volume flow rate of the blend sent to the refinery hydrocracking unit in (c) accounts for at most 100 volume % of the total hydrocarbon flow rate sent to the hydrocracking unit.
11. The process of claim 1 , wherein the volume flow rate of the blend sent to the refinery hydrocracking unit in (c) accounts for at most 50 volume % of the total hydrocarbon flow rate sent to the hydrocracking unit.
12. The process according to claim 11, wherein the blend flow rate is at most 25% by volume of the total flow rate sent to the hydrocracking unit.
13. The method of claim 1, wherein the blend of petroleum and selected waste plastic in (b) is prepared by heating the waste plastic to a temperature above the melting point of the plastic and mixing with the petroleum, and then cooling the blend to a temperature below the melting point of the waste plastic.
14. The method of claim 1, wherein the petroleum in the blend comprises atmospheric gas oil, vacuum gas oil (VGO), atmospheric residue, petroleum-derived oils, petroleum-based materials, and / or heavy materials recovered from refinery operations.
15. The method of claim 1, wherein the petroleum in the blend comprises light cycle oil (LCO), heavy cycle oil (HCO), FCC naphtha, gasoline, diesel, toluene, and / or aromatic solvents derived from petroleum.
16. The process of claim 1, wherein a heavy fraction is recovered from the hydrocracking unit and sent to an isomerization / dewaxing unit.
17. The process of claim 16, wherein base oil is recovered from the isomerization / dewaxing unit.
18. The process according to claim 17, wherein the recovered base oil is sent to a hydrofinishing unit.
19. The process of claim 16, wherein a naphtha fraction is recovered from the isomerization / dewaxing unit and at least a portion of the naphtha fraction is sent to a steam cracker to produce ethylene.
20. A method for converting waste plastics into chemicals that can be used to prepare polyethylene, comprising: (a) selecting waste plastics containing polyethylene and / or polypropylene; (b) preparing a blend of petroleum and a selected plastic, wherein the blend comprises about 20% by weight or less of the selected plastic; and (c) sending the blend to a refinery hydrocracking unit.
21. A continuous process for converting waste plastics into regenerants for base oil preparation, comprising: (a) selecting waste plastics comprising polyethylene and / or polypropylene; (b) preparing a blend of petroleum and a selected waste plastic, wherein the blend comprises about 20% by weight or less of the selected waste plastic; (c) sending the blend to a refinery hydrocracking unit at a temperature above the melting point of the plastic in the blend; (d) recovering a heavy fraction from the hydrocracking unit and sending the heavy fraction to a refinery isomerization / dewaxing unit; as well as (e) recovering base oil from the isomerization dewaxing unit.
22. The method according to claim 21, wherein the base oil recovered in (e) is sent to a hydrofinishing unit, and a hydrofinished base oil is recovered therefrom.
23. A method of converting waste plastics into regenerants for use in making lower carbon footprint fuels and base oils, comprising: (a) selecting waste plastics containing polyethylene and / or polypropylene; (b) preparing a blend of petroleum and a selected waste plastic, wherein the blend comprises about 20% by weight or less of the selected waste plastic; (c) sending the blend to a refinery hydrocracking unit at a temperature above the melting point of the plastic in the blend; (d) recovering a heavy fraction from the hydrocracking unit and sending the heavy fraction to a refinery isomerization / dewaxing unit; as well as (e) recovering base oil from the isomerization dewaxing unit.
24. The method of claim 23, wherein the lower carbon footprint fuel comprises gasoline, jet fuel, diesel and / or bunker fuel.
Citation Information
Cited By
Method for preparing steam cracking furnace raw material through hydroisomerization of high-boiling-point wax-containing fraction obtained by cracking waste plastics
CN122609269A