Method and arrangement for producing reduced metallic material
By chemically reacting metal oxide materials with hydrogen-containing reducing agents and using their thermal energy to perform heat treatment, the problem of insufficient heat treatment of reducing agents in the prior art is solved, and efficient production of reducing metal materials that are resistant to reoxidation is achieved, and in the industry Carbon emissions have been reduced on a scale.
Patent Information
- Application Number
- CN202380030290.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2023-04-03
- Publication Date
- 2024-11-26
AI Technical Summary
The existing methods are inefficient and inefficient when reducing metal oxide materials using reducing agents, resulting in insufficient heat treatment of the reducing agent, destroying its reduction potential, and unable to effectively produce reducing metal materials that are resistant to reoxidation.
By chemically reacting the metal oxide material that maintains heat energy with the hydrogen-containing reducing agent, the introduced hydrogen-containing reducing agent is heated or further heated by the thermal energy of the metal oxide material to achieve effective reduction and heat treatment of the metal oxide material, and the introduction is controlled. The temperature-regulating chemical reaction and heat treatment process of hydrogen-containing reducing agents ensures the passivation parameter value of the reduced metal material.
It realizes efficient reduction and heat treatment of metal oxide materials, produces reduced metal materials that are resistant to reoxidation, reduces production costs, and realizes the production of CO2-medium or low emission metal materials on an industrial scale.
Smart Images

Figure CN119032184A_ABST
Abstract
Description
Technical Field
[0001] The present invention generally relates to a method for reducing a metal oxide material retaining thermal energy to a reduced metal material.
[0002] The present invention also relates to a metal material production arrangement suitable for reducing a metal oxide material retaining thermal energy to a reduced metal material.
[0003] The present invention also relates to a data program programmed to control a heat treatment process for heat treating a metal oxide material and / or a reduced metallic material to produce a reduced metallic material that is resistant to reoxidation.
[0004] The present disclosure may be directed to methods and metallic material production arrangements for producing a carbon-free, reoxidation-resistant, reduced metallic material.
[0005] The present invention relates primarily to the mining industry.
[0006] Furthermore, the present invention may also relate to manufacturers and suppliers of metal oxide material supply device units, reduction equipment, steelmaking industries, and the like. Background Art
[0007] Various methods are currently known for passivating reduced metallic materials by means of different types of reducing agents.
[0008] However, current methods and configurations are inefficient and suboptimal with respect to utilizing a reducing agent introduced into a reduction device for reducing metal oxide materials. In order to provide sufficient heat to support the reduction process, the reducing agent is heated intensely, which in turn destroys the reducing potential of the reducing agent. Summary of the invention
[0009] One object is to provide efficient reduction of metal oxide materials while achieving efficient control of the thermal treatment process by maintaining the reduction potential of the reducing agent to achieve efficient production of reduced metal materials that are resistant to reoxidation.
[0010] One objective is to provide a cost effective delivery supply chain of reduced metallic materials to other industries, such as to the steelmaking industry.
[0011] One object is to produce a reduced metallic material that can be used for the cost-effective production of steel using, for example, an electric arc furnace.
[0012] One object is to provide a method for reducing a metal oxide material holding thermal energy to a reduced metal material to produce a reduced metal material by fossil energy-free or at least substantially fossil energy-free.
[0013] One object is to provide a process by which reduced metallic materials can be produced on an industrial scale in a CO 2 -neutral and / or CO 2 -low-emission and / or CO 2 -free manner.
[0014] An object is to provide a carbon-free reduced metallic material by an energy efficient process.
[0015] These purposes or at least one of the purposes have been achieved by a method for reducing a metal oxide material retaining thermal energy to a reduced metal material; wherein the metal oxide material retaining thermal energy is provided by a metal oxide material supply device unit and is loaded into an upper internal part of a reduction device of a metal material production configuration by a metal oxide material loading device; a control circuit is electrically connected to a reducing agent temperature regulating device, the reducing agent temperature regulating device being configured to regulate the temperature of a hydrogen-containing reducing agent to be introduced into the middle part and / or the lower internal part of the reduction device via a reducing agent inlet device; the method is characterized by the following steps: utilizing the thermal energy of the metal oxide material to heat or further heat the introduced hydrogen-containing reducing agent to provide a chemical reaction between the hydrogen-containing reducing agent and the metal oxide material, thereby reducing the metal oxide material in the upper internal part; providing a heat treatment process, the heat treatment process being used to heat treat the metal oxide material undergoing reduction and / or heat treat the reduced metal material before being discharged from the lower internal part; and controlling the temperature of the introduced hydrogen-containing reducing agent to regulate the chemical reaction and / or the heat treatment process to achieve at least one desired passivation parameter value of the reduced metal material.
[0016] In this way it is achieved that the chemical reactivity and / or high driving force of hydrogen is largely maintained. Chemical reactivity and / or high driving force are essential to provide for efficient reduction of metal oxide materials.
[0017] Alternatively, the step of controlling the temperature of the introduced preheated hydrogen-containing reducing agent includes adjusting the temperature to a predetermined temperature for providing sintering of the reduced metal oxide material and / or sintering and / or heat treatment of the reduced metal material to achieve at least one desired passivation parameter value during a predetermined time period.
[0018] Alternatively, the introduced hydrogen-containing reducing agent comprises 80% to 100% hydrogen, preferably 100% hydrogen.
[0019] Alternatively, the control circuit is adapted for a coarse setting of the thermal energy and for a fine setting of the temperature of the introduced (preheated or cooled) hydrogen-containing reducing agent in order to achieve at least one desired passivation parameter value.
[0020] In this way, an effective regulation of the temperature for reducing the metal oxide material is achieved, while at the same time an effective regulation of the temperature for the heat treatment of the reduced metal material is achieved.
[0021] Alternatively, the step of reducing the metal oxide material in the upper inner portion is accomplished by utilizing thermal energy of the metal oxide material and by heating or further heating the introduced preheated hydrogen gas by utilizing the heat content of the partially reduced metal material in the upper inner portion.
[0022] Alternatively, the temperature of the metal oxide material to be loaded into the upper inner portion is controlled within a range of 900°C to 1500°C, preferably 1000°C to 1400°C by a control circuit.
[0023] Alternatively, the temperature of the preheated hydrogen-containing reducing agent is controlled by a control circuit within the range of 100°C to 400°C, preferably 200°C to 300°C; or 0°C to 300°C, preferably 100°C to 200°C; or 50°C to 250°C, preferably 125°C to 175°C.
[0024] Alternatively, the temperature of the metal oxide material to be loaded into the upper inner portion is controlled within a range of 900°C to 1500°C, preferably 1000°C to 1300°C by a control circuit.
[0025] Alternatively, the temperature of the hydrogen-containing reducing agent is controlled by a control circuit within the range of 100°C to 400°C, preferably 200°C to 300°C; or 0°C to 300°C, preferably 100°C to 200°C.
[0026] By directly loading the metal oxide material from the metal oxide material supply device unit into the reduction equipment, the metal oxide material has thermal energy from the thermal process provided by the metal oxide material supply device unit, thereby achieving effective reduction and chemical reaction between the metal oxide material and the reducing agent. At the same time, by introducing a hydrogen-containing reducing agent with an undamaged reduction potential and providing a heat treatment process for producing a reduced metal material resistant to reoxidation, effective control of the process is achieved.
[0027] Alternatively, the metal oxide material is formed into agglomerates, and the heat energy source is provided by a heating process provided by the metal oxide material supply device unit.
[0028] Alternatively, the upper interior portion is adapted to retain thermal energy for reduction of the metal oxide material.
[0029] Alternatively, the control circuit is electrically coupled to a reducing agent temperature regulating device configured to preheat the hydrogen-containing reducing agent to be introduced into the middle inner portion and the lower inner portion of the reduction device.
[0030] Alternatively, the intermediate interior portion and the lower interior portion are configured for introducing a preheated hydrogen-containing reducing agent suitable for reacting with (reducing) the metal oxide material retaining thermal energy.
[0031] Alternatively, a hydrogen-containing reducing agent is introduced into the middle inner portion and into the lower inner portion.
[0032] Alternatively, the bottom section of the upper interior portion is configured for the introduction of a preheated hydrogen-containing reducing agent suitable for reacting with (reducing) the metal oxide material retaining thermal energy.
[0033] Alternatively, the hydrogen-containing reducing agent is introduced into the bottom section of the upper interior portion.
[0034] Alternatively, the reduction apparatus is configured to allow the reduced metal material to descend into the lower inner portion and / or the middle inner portion for providing a heat treatment process for heat treating the reduced metal material using additional heat energy provided by the preheated hydrogen-containing reducing agent.
[0035] Alternatively, the additional thermal energy is defined as thermal energy added to the thermal energy of the metal oxide material that retains the thermal energy and / or as thermal energy added to the thermal energy of the reduced metal material that descends through the intermediate inner portion and / or the lower inner portion.
[0036] Alternatively, the reduction apparatus is configured to allow the reduced metal material to descend into the lower inner portion and / or the middle inner portion for providing a heat treatment process for heat treating the reduced metal material using additional heat energy provided by the preheated hydrogen-containing reducing agent.
[0037] Alternatively, the additional thermal energy is defined as thermal energy added to the thermal energy of the metal oxide material retaining thermal energy and / or as thermal energy added to the still unutilized thermal energy of the reduced metal material descending through the intermediate inner portion and / or the lower inner portion.
[0038] Alternatively, the control circuit is configured to control the additional thermal energy by adjusting the temperature of the introduced preheated hydrogen-containing reducing agent for providing at least one desired passivation parameter value of the reduced metallic material.
[0039] Alternatively, the additional thermal energy provided by the introduced preheated hydrogen-containing reducing agent is regulated by the control circuit by controlling the temperature of the reduced metal oxide material in the middle inner portion and / or the lower inner portion towards a predetermined temperature, for providing sintering and / or sintering and / or heat treatment of the reduced metal oxide material during a predetermined time period.
[0040] Alternatively, the temperature of the introduced preheated hydrogen-containing reducing agent is controlled by the control circuit to maintain the reduced metallic material in the middle interior portion and / or the lower interior portion at an elevated predetermined temperature for an extended period of time for effecting the heat treatment process.
[0041] In this manner, the reduced metallic material resists reoxidation and / or degradation.
[0042] In this way, it is achieved that the reduced metallic material discharged from the reduction device forms an intermediate product which is resistant to reoxidation.
[0043] In this way it is achieved that the intermediate products do not need to be resistant to reoxidation, which in turn facilitates cost-effective delivery to the steel industry.
[0044] In this way it is achieved that the intermediate product can be used for the production of steel using, for example, an electric arc furnace (EAF) for cost-effective production.
[0045] In this way it is achieved that scrap metal can be reused for the production of steel despite the high carbon content of the scrap metal.
[0046] Alternatively, the temperature of the introduced preheated hydrogen-containing reducing agent provides the first thermal energy.
[0047] Alternatively, the control circuit is adapted to control the additional thermal energy by adjusting the temperature of the introduced preheated hydrogen-containing reducing agent.
[0048] Alternatively, the temperature of the introduced preheated hydrogen-containing reducing agent is controlled within the range of 100°C to 400°C, preferably 200°C to 300°C; or 0°C to 300°C, preferably 100°C to 200°C.
[0049] Alternatively, the temperature of the introduced preheated hydrogen-containing reducing agent is controlled within the range of 300°C to 600°C, preferably 400°C to 500°C.
[0050] Alternatively, the control circuit is adapted to control the thermal energy in such a manner that the thermal energy decreases as the metal oxide material descends further in the upper interior portion.
[0051] Alternatively, the control circuit is adapted to control the thermal energy in such a way that the thermal energy decreases as the reduced metallic material descends further in the intermediate inner portion and / or the lower inner portion.
[0052] Alternatively, the control circuit is adapted to control the temperature of the introduced preheated hydrogen-containing reductant in a manner such that the temperature of the introduced preheated hydrogen-containing reductant increases as the introduced preheated hydrogen-containing reductant rises higher in the upper interior portion.
[0053] Alternatively, the control circuit is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent in such a manner that the thermal energy decreases as the reduced metallic material descends further in the intermediate interior portion and / or the lower interior portion.
[0054] Alternatively, the control circuit is adapted to provide additional thermal energy that decreases as the reduced metallic material descends further in the intermediate interior portion and / or the lower interior portion.
[0055] Alternatively, the control circuit is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent and / or the temperature of the thermally retained metal oxide material to achieve that the temperature in the upper interior portion does not drop below a specific temperature required to reduce the metal oxide material in the upper interior portion.
[0056] In this way, it is ensured that the reduction using the thermal energy of the metal oxide material takes place efficiently, wherein the reduction potential of the preheated hydrogen-containing reducing agent is maintained when it is introduced.
[0057] In this way, the thermal energy of the metal oxide material can be used to a large extent due to its high thermal energy content and is advantageously used in the top section of the upper inner part, where the metal oxide material retaining the thermal energy first encounters the preheated hydrogen-containing reducing agent containing a depleted reduction potential (low reducing power), the depletion of the reduction potential of the preheated hydrogen-containing reducing agent being due to the fact that the metal oxide material retaining the thermal energy, which descends through the upper inner part and encounters the upwardly flowing preheated hydrogen-containing gas, undergoes reduction of the depleted reduction potential.
[0058] Alternatively, the control circuit is suitable for controlling the temperature of the preheated hydrogen-containing reductant so that the consumption of the reduction potential of the preheated hydrogen-containing reductant during reduction proceeds to an extent that the preheated hydrogen-containing reductant in the top section contains a low content of hydrogen and a high content of water vapor (meaning that the covalent bonds that hold the hydrogen and oxygen together produce water vapor and the remaining hydrogen of the hydrogen-containing reductant is used to remove oxygen from the metal oxide material).
[0059] Therefore, due to the high temperature of the heat energy retaining metal oxide material initially charged into the top section of the upper inner portion, effective reduction of the heat energy retaining metal oxide material may be provided.
[0060] In this way, pure or substantially pure hydrogen can be used both for energy efficient reduction of charged metal oxide materials by thermal energy, and for energy efficient thermal treatment processes for thermal treatment of reduced metal materials, wherein the hydrogen-containing reducing agent is preheated to a temperature that does not destroy the reduction potential of the hydrogen.
[0061] In this manner, the temperature of the preheated hydrogen-containing reducing agent may be adjusted to provide the temperature required for effective reduction in the upper interior portion.
[0062] In this manner, the temperature of the preheated hydrogen-containing reducing agent may be adjusted to provide a temperature required to effectively regulate the chemical reaction and / or thermal treatment process in the middle and / or lower inner portions to provide at least one desired passivation parameter value of the reduced metallic material.
[0063] Alternatively, the control circuit is configured to adjust the temperature of the preheated hydrogen-containing reducing agent to a predetermined temperature for providing a heat treatment process established in the middle inner part and / or the lower inner part, wherein the predetermined temperature is determined by optimal energy consumption, i.e., actively limiting any excessive heating of the hydrogen-containing reducing agent to save energy.
[0064] Alternatively, the control circuit is configured to adjust the time period required for the heat treatment process with respect to optimal energy consumption in the production of reduced metallic material, which time period may be determined by the actual temperature of the preheated hydrogen-containing reducing agent.
[0065] In this way, energy-efficient production of reduced metallic material is provided.
[0066] In this way, a heat treatment process is provided with regard to an optimal use of energy.
[0067] Alternatively, the direct reduction apparatus comprises a reductant inlet device configured to introduce a hydrogen-containing reductant into the direct reduction apparatus to provide reduction of the metal oxide material to retain thermal energy.
[0068] Alternatively, the introduced preheated hydrogen-containing reducing agent is considered to be a supplement to the hydrogen-containing reducing agent introduced into the reducing agent inlet device (the hydrogen-containing reducing agent being used for reduction in the direct reduction device).
[0069] Alternatively, the volume of the introduced hydrogen-containing reducing agent and / or preheated hydrogen-containing reducing agent is such as to achieve complete reduction of the metal oxide material, and an excess volume of hydrogen-containing reducing agent is provided in the reduction device for providing said reduction of the metal oxide material and / or heat treatment of the reduced metal material.
[0070] Alternatively, during the reduction of the metal oxide material, the metal oxide material retaining thermal energy is formed in the upper inner portion as agglomerates that are further sintered.
[0071] Alternatively, the reduced and sintered agglomerates transferred into the intermediate inner portion and / or the lower inner portion consist of reduced metal particles that are bonded to each other to form pellets of reduced metal material.
[0072] Alternatively, the control circuit is configured to adjust the temperature of the preheated hydrogen-containing reducing agent to provide a predetermined time period for sintering the pellets of reduced metallic material in the middle inner portion and / or the lower inner portion and / or heat treating the pellets to provide at least one desired passivation parameter value of the reduced metallic material.
[0073] In this way, it is achieved that the reduced metallic material can be subjected to a further sintering process and / or heat treatment of the reduced metallic material in the middle inner portion and / or the lower inner portion.
[0074] Alternatively, the reduced iron ore material is discharged from the reduction device in the form of compact iron bodies of reduced iron ore material (iron balls or iron pellets or so-called iron drops), each pellet having a compact and dense structure for producing an intermediate product resistant to reoxidation.
[0075] Alternatively, the metal oxide material retaining thermal energy is allowed to descend substantially continuously in the upper interior portion and contact the preheated hydrogen-containing reducing agent for reduction of the metal oxide material.
[0076] Alternatively, the reduced metallic material is allowed to descend substantially continuously in the intermediate interior portion and / or the lower interior portion and contact the preheated hydrogen-containing reducing agent.
[0077] Alternatively, the preheated hydrogen-containing reducing agent in the middle inner portion and / or the lower inner portion is used to provide a semi-molten melt and / or melt and / or sinter the reduced iron ore material, wherein the iron atoms of the reduced iron ore material are arranged in a body-centered cubic pattern.
[0078] Alternatively, the temperature of the preheated hydrogen-containing reducing agent introduced into the upper interior portion is controlled by the control circuit to provide that the spent reducing fluid resulting from the reduction comprises 100% water vapor or substantially 100% water vapor.
[0079] Alternatively, the direct reduction apparatus further comprises a spent reducing fluid outlet device configured to discharge the spent reducing fluid, such as water vapor and hydrogen, from the reduction apparatus.
[0080] Alternatively, the control circuit is adapted to control a spent reducing fluid outlet means for discharging spent reducing fluid from the reducing device.
[0081] Alternatively, the control circuit is adapted to control the temperature of the chemical reaction by coarsely regulating the thermal energy provided by the metal oxide material supplier unit, and by finely regulating the temperature required for the chemical reaction and / or thermal treatment process by controlling the temperature of the introduced preheated hydrogen-containing reducing agent.
[0082] These purposes or at least one of the purposes have been achieved by a metal material production configuration suitable for reducing a metal oxide material that retains thermal energy into a reduced metal material; the metal material production configuration includes: a metal oxide material supply device unit, which is configured to provide a metal oxide material that retains thermal energy; a metal oxide material loading device, which is configured to load the metal oxide material into the upper internal part of the reduction device; a reducing agent inlet device, which is configured to introduce a hydrogen-containing reducing agent into the middle internal part and / or the lower internal part of the reduction device, thereby heating or further heating the introduced hydrogen-containing reducing agent by utilizing the thermal energy of the metal oxide material to provide a chemical reaction between the hydrogen-containing reducing agent and the metal oxide material, so that the hydrogen-containing reducing agent is suitable for reacting with the metal oxide material that retains thermal energy to reduce the metal oxide material. The metal material production configuration is characterized in that the reduction equipment of the metal material production configuration is configured to provide a heat treatment process, which is used to heat treat the metal oxide material undergoing reduction and / or the reduced metal material; and the control circuit electrically connected to the reducing agent temperature regulating device configured to regulate the temperature of the hydrogen-containing reducing agent is suitable for controlling the temperature of the introduced hydrogen-containing reducing agent to achieve at least one desired passivation parameter value of the reduced metal material.
[0083] Alternatively, the restoration device comprises a passivation parameter detector configured to detect an actual passivation parameter value.
[0084] Alternatively, the passivation parameter detector includes a laser-based surface detector, a density detector, an X-ray detector, and / or other types of detectors, etc.
[0085] Alternatively, the control circuit is electrically coupled to the metal oxide material supplier unit and is adapted to control the temperature of the metal oxide material to be loaded into the upper inner portion to provide a chemical reaction between the preheated hydrogen-containing reducing agent and the metal oxide material.
[0086] Alternatively, the metal oxide material supplier unit is configured to provide a metal oxide material that retains thermal energy, wherein the metal oxide material is formed into agglomerates that retain thermal energy from a heating process provided by the metal oxide material supplier unit.
[0087] Alternatively, the control circuit controls the temperature of the introduced preheated hydrogen-containing reducing agent to provide sintering of the outer surfaces of the individual agglomerates and / or the entire agglomerates.
[0088] Alternatively, the middle inner portion and / or the lower inner portion is configured for receiving reduced metal material and is configured for providing a heat treatment process for hardening the reduced metal material using a hardening process, for heat treating the reduced metal material using additional thermal energy provided by the introduced preheated hydrogen-containing reducing agent.
[0089] Alternatively, the control unit is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent and is configured to adjust the temperature towards a predetermined temperature for providing sintering of the reduced metal oxide material and / or sintering and / or heat treatment of the reduced metal material during a predetermined time period.
[0090] In this way it is achieved that the iron ore oxide material is prevented from having a tendency to revert to an oxidized state when exposed to the elements and the risk of spontaneous combustion processes is reduced.
[0091] Alternatively, the control unit is adapted to control the amount of additional thermal energy by controlling the temperature of the introduced preheated hydrogen-containing reducing agent and / or by controlling the temperature of the metal oxide material charged into the upper inner part by controlling the metal oxide material feeder unit.
[0092] Alternatively, the middle internal portion and / or lower internal portion of the reduction apparatus configured for the thermal treatment process is an independent unit or a single unit of the apparatus connected to the reduction zone having a similar configuration as the upper internal portion and suitable for receiving the metal oxide material to retain heat energy and the introduction of preheated hydrogen-containing reducing agent.
[0093] Alternatively, the control circuit is adapted to control the temperature of the preheated hydrogen-containing reducing agent for controlling the heat treatment process in the reduction apparatus and / or in a separate unit or in a heat treatment zone of a single unit.
[0094] Alternatively, the control circuit is adapted to control the internal gas pressure in the upper inner part and / or the middle inner part and / or the lower inner part of the reduction device.
[0095] Alternatively, the thermal treatment process includes hot briquetting the metal oxide material and / or the reduced metal material by controlling the temperature of the introduced preheated hydrogen-containing reducing agent to provide at least one desired passivation parameter value of the reduced metal material.
[0096] Alternatively, the control circuit is electrically coupled to a passivation parameter value sensor device configured to detect at least one desired passivation parameter value of the reduced metallic material.
[0097] Alternatively, the control circuit is configured to control the temperature of the metal oxide material to be charged into the upper inner portion for controlling the heat treatment process towards a specific heat treatment temperature value, wherein the specific heat treatment temperature value is determined by at least one desired passivation parameter value of the reduced metal material, wherein the control circuit takes into account the actual temperature of the metal oxide material to be charged in order to reach the specific heat treatment temperature value.
[0098] Alternatively, the control circuit is configured to control the temperature of the metal oxide material charged to the direct reduction plant.
[0099] Alternatively, the reduced and sintered agglomerates transferred into the intermediate inner portion and / or the lower inner portion consist of reduced metal particles that are bonded to each other to form pellets of reduced metal material.
[0100] In this way, it is achieved that the reduced iron ore material (e.g., sponge iron, such as pellets, briquettes, balls, iron droplets, etc.) will form a dense body of reduced iron material, which optionally has an external structural feature with a density higher than the core of the pellet body, promoting cost-effective transportation and preventing spontaneous combustion of the reduced iron material.
[0101] The wording "metal" may mean a metal ore or be replaced by "iron ore", which may contain other elements and / or minerals besides iron, such as naturally occurring alloying elements or smaller amounts of minerals that do not constitute an alloy.
[0102] The expression "iron ore" may mean iron ore including introduced additives such as quartzite, silicon, lime and the like.
[0103] The wording "restore the device" can be changed to "restore the device directly".
[0104] The wording "heat treatment" may be changed to the wording "heat hardening".
[0105] The definition of "sintering" may mean a heat treatment process in which agglomerated reduced metallic material is subjected to sufficiently high temperature and / or pressure to provide a dense and solid mass or pellet of reduced metallic material.
[0106] Alternatively, a portion of the hydrogen-containing reducing agent is cooled prior to introduction into the bottom section of the lower interior portion.
[0107] Alternatively, a cold hydrogen-containing reducing agent is introduced into the bottom section of the lower interior portion.
[0108] In this way, it is achieved that the reduced metal material is cooled by the cooling process in the direct reduction device before being discharged from the reduction device, whereas the hydrogen-containing reducing agent used for cooling will be heated, whereas the heat recovered from the reduced metal material can be used again in the reduction and heat treatment process.
[0109] Alternatively, heat recovered from the reduced metallic material by the cooling process is transferred upward in the direct reduction plant to add heat to the reduction and / or thermal treatment process in a recirculating heating system.
[0110] Alternatively, the introduction point of the preheated hydrogen-containing reducing agent into the direct reduction apparatus may be vertically adjustable along the extension of the direct reduction apparatus for controlling the heat treatment process to achieve optimal sintering and produce dense and solid reduced metallic material blocks or pellets.
[0111] Alternatively, the introduced hydrogen-containing reducing agent is introduced into the reduction device via a reducing agent inlet arrangement, which comprises at least one reducing agent inlet of the reduction device.
[0112] Alternatively, the reductant inlet arrangement comprises at least two reductant inlets, at least one of which is configured to introduce supplemental hydrogen-containing reductant into the reduction device to provide the thermal treatment process.
[0113] Alternatively, the heat treatment includes subjecting the reduced metal oxide material and / or the reduced metal material to thermal hardening.
[0114] Alternatively, the heat treatment includes a thermal hardening process including sintering of the reduced metal material and / or shrinking of the reduced metal material and / or densification of the reduced metal material.
[0115] Alternatively, the metal oxide material supplier unit may include a metal oxide granulation device or a metal oxide preheating device.
[0116] Alternatively, reducing the thermally-energy-retaining metal oxide material to a reduced metal material utilizes the thermal energy of the metal oxide material, wherein the thermal energy is used to heat or further heat the introduced hydrogen-containing reducing agent and / or the reduction process to provide a chemical reaction between the hydrogen-containing reducing agent and the metal oxide material.
[0117] Alternatively, the temperature of the chemical process for reduction is above 570°C, or in the range of 600°C to 1500°C, preferably 750°C to 1350°C.
[0118] Alternatively, the temperature of the chemical process for reduction is in the range of 700°C to 1400°C, preferably 800°C to 1300°C.
[0119] Alternatively, the temperature of the introduced hydrogen-containing reducing agent is controlled to provide regulation of the heat treatment process, the temperature of the heat treatment process being adapted to be at a predetermined temperature value to provide the heat treatment process to achieve at least one desired passivation parameter value of the reduced metallic material.
[0120] Alternatively, the predetermined temperature is suitably in the range of 200°C to 600°C, preferably 300°C to 500°C, to provide at least one desired passivation parameter value of the reduced metallic material.
[0121] Alternatively, the predetermined temperature is provided during a predetermined period of time long enough to enable the heat treatment process to be performed to provide at least one desired passivation parameter value of the reduced metallic material.
[0122] Alternatively, at least one desired passivation parameter value may relate to a porosity parameter and / or a size parameter and / or a weight parameter and / or a metal particle structure parameter and / or a sample cutting uniformity parameter and / or a shrinkage parameter and / or a sintering parameter and / or a cold crushing strength parameter and the like.
[0123] Alternatively, the metal oxide material that retains the heat energy is transferred from the upper interior portion to the middle portion and / or the lower portion by gravity.
[0124] Alternatively, the reducing agent temperature regulating device may comprise or be a part of an electrolysis cell adapted to regulate the temperature of the introduced hydrogen-containing reducing agent, the electrolysis cell being electrically coupled to the control circuit.
[0125] Alternatively, the reducing agent temperature regulating device may include a reducing agent preheating device adapted to regulate the temperature of the introduced hydrogen-containing reducing agent, the reducing agent preheating device being electrically coupled to the control circuit.
[0126] Alternatively, the reducing agent temperature regulating device is further configured to cool the hydrogen-containing reducing agent to be introduced into the middle portion and / or the lower inner portion of the reduction device via the reducing agent inlet device.
[0127] Alternatively, the method includes the step of utilizing thermal energy of the metal oxide material to heat or further heat the introduced preheated hydrogen-containing reducing agent to provide a chemical reaction between the preheated hydrogen-containing reducing agent and the metal oxide material, thereby reducing the metal oxide material in the upper inner portion.
[0128] Alternatively, the reducing agent inlet device is configured to introduce the preheated hydrogen-containing reducing agent into the middle internal part and / or the lower internal part of the reduction device, thereby heating or further heating the introduced preheated hydrogen-containing reducing agent by utilizing the thermal energy of the metal oxide material to provide a chemical reaction between the preheated hydrogen-containing reducing agent and the metal oxide material, so that the preheated hydrogen-containing reducing agent is suitable for reacting with the metal oxide material that retains thermal energy to reduce the metal oxide material.
[0129] Alternatively, the control circuit electrically coupled to the reductant preheating device configured to preheat the hydrogen-containing reductant is adapted to control the temperature of the introduced preheated hydrogen-containing reductant to achieve at least one desired passivation parameter value of the reduced metallic material.
[0130] Alternatively, the introduced preheated hydrogen-containing reducing agent (either preheated or cooled) comprises from 80% to 100% hydrogen by volume, preferably from 90% to 95% hydrogen.
[0131] Alternatively, the introduced preheated hydrogen-containing reducing agent (either preheated or cooled) comprises from 70% to 95% hydrogen by volume, preferably from 80% to 90% hydrogen.
[0132] Alternatively, the substantially or completely endothermic chemical reaction may consume heat energy equivalent to about 475°C to 525°C, preferably about 500°C, extracted from the metal oxide material retaining heat energy during the reduction and chemical reaction carried out in the direct reduction unit.
[0133] Alternatively, the control circuit is configured to control the time during which the metal oxide material flows through the middle interior portion and / or the lower interior portion of the reduction device by design of the mechanical device, pressurization, reduction shaft, and heat treatment shaft.
[0134] These or at least one of the objects has been achieved by a data program programmed to cause a metal material production arrangement to perform a method according to the attached claims.
[0135] The benefit of utilizing the present disclosure is demonstrated by the fact that the chemical reactivity and / or high driving force of the hydrogen H of the hydrogen-containing reducing agent is maintained when introduced into a direct reduction plant.
[0136] Alternatively, the reduction device is connected to the metal oxide preheating device for preheating the metal oxide material.
[0137] Iron droplets may be defined as small, round, pear-shaped, droplet-shaped, pellet-shaped, bead-shaped, sphere-shaped or ellipsoidal bodies of passivated reduced iron ore material and / or metallic material having a compact and dense structure, which are used to produce a reoxidation resistant intermediate product.
[0138] Alternatively, the reducing agent to be introduced and / or being introduced into the direct reduction device has a gas temperature predetermined and / or controlled and / or selected by the control circuit to be any temperature in the range of about 600°C to 1000°C, or about 500°C to 900°C, or about 700°C to 1200°C.
[0139] Alternatively, the introduced reducing agent rising upward in the direct reduction plant meets the direct reduced iron ore material and / or the iron ore oxide material undergoing direct reduction descending in the direct reduction plant.
[0140] Alternatively, the gas temperature of the reducing agent is provided to reduce the cooling rate of the direct reduced metal material and / or the metal oxide material undergoing direct reduction descending through the direct reduction apparatus.
[0141] Alternatively, the reduction potential of the reductant rising in the upper internal portion may be lower than the reduction potential of the reductant introduced further down in the direct reduction device (i.e., the middle internal portion and / or the lower internal portion) because the reductant contains a higher level of water vapor in the upper internal portion than in the middle internal portion and / or the lower internal portion.
[0142] Alternatively, the material temperature of the metal oxide material to be charged and / or being charged into the direct reduction apparatus (e.g., any temperature in the range of about 50°C to about 350°C, or about 100°C to about 400°C) meets the reducing agent in the upper interior portion.
[0143] Alternatively, a portion of the hydrogen is used for chemical reactions in the middle inner portion and / or the lower inner portion.
[0144] Alternatively, the heat-retaining metal oxide material provides at least a portion of the heat energy required for said chemical reaction between the metal oxide material and the reducing agent in the upper interior portion of the direct reduction device.
[0145] Alternatively, the metal oxide material, which retains thermal energy at least to some extent, further heats the reducing agent in the upper interior portion.
[0146] This makes possible an energy-saving method for the direct reduction of metal oxide materials by hydrogen and / or a hydrogen-containing reducing agent, wherein the hydrogen can preferably be temporarily stored in a gas storage tank and / or a storage device in a geological reservoir and / or in other buffer devices, so that the hydrogen of the reducing agent is available and can be used when renewable energy cannot be fully generated, for example to cope with fluctuations in the production of renewable generated electrical energy.
[0147] The present invention may relate to a method for producing steel, whereby a metal oxide material is reduced in a direct reduction plant with a reducing agent, such as a hydrogen-containing reducing agent, and the intermediate products and final accompanying materials of the directly reduced metal material thus obtained are subjected to metallurgical processing; the reducing agent is produced by electrolysis of water via an electrolysis unit, such as a high-temperature electrolysis unit, the electrical energy required for the electrolysis may be renewable energy from hydro and / or wind and / or photovoltaic and / or other forms of renewable energy and / or a nuclear power plant, such as a plant including a small modular reactor SMR, wherein if sufficient reducing agent is available, the reduced metal material produced, such as sponge iron (the so-called intermediate product), is produced independently of current demand.
[0148] Alternatively, the metal oxide material is transferred from a metal oxide material supply device, such as a granulation device and / or a preheating device, to a direct reduction device, and the heat energy from the metal oxide material supply device is maintained.
[0149] Alternatively, the direct reduction apparatus is configured to introduce a reducing agent suitable for reacting with a metal oxide material that retains thermal energy, thereby reducing the metal oxide material to an intermediate product by utilizing the thermal energy of the metal oxide material to further heat the introduced reducing agent to achieve a chemical reaction between the metal oxide material and the reducing agent, thereby providing an energy-saving and time-saving process.
[0150] The hydrogen gas containing the hydrogen reducing agent and / or the hydrogen containing reducing agent may be stored in a gas storage tank and / or a storage device in a geological storage reservoir and / or in other buffer devices.
[0151] Gas storage tanks or storage facilities in geological repositories may be located between the electrolysis unit and / or high-temperature electrolysis unit and the direct reduction unit.
[0152] Alternatively, the reducing agent may be preheated prior to introduction into the direct reduction plant so that the reducing agent, in addition to providing direct reduction and / or chemical reaction, also reduces the cooling rate of the directly reduced metal material and / or metal oxide material undergoing direct reduction descending through the direct reduction plant.
[0153] The temperature of the metal oxide material to be charged into the upper interior portion of the direct reduction plant may be higher than the temperature of the reducing agent to be and / or being introduced into the direct reduction plant.
[0154] The temperature of the metal oxide material to be charged into the upper interior portion of the direct reduction apparatus may be lower than the temperature of the reducing agent to be and / or being introduced into the direct reduction apparatus.
[0155] The temperature of the metal oxide material to be charged into the direct reduction device may have a material temperature of about 50°C to about 350°C, or about 100°C to about 400°C, or about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or higher.
[0156] The reducing agent may be preheated to a gas temperature of about 200°C to about 500°C, or about 300°C to about 600°C, or about 400°C to about 700°C, or about 500°C to about 800°C, or about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or higher, before and / or when introduced into the direct reduction device.
[0157] By introducing a reducing agent with a relatively high gas temperature (e.g., about 600°C to 900°C) into a direct reduction apparatus, the metal oxide material retaining heat energy that reaches the middle portion and / or lower inner portion of the direct reduction apparatus and undergoes direct reduction and / or heat treatment is achieved, thereby reducing the cooling rate of the directly reduced metal material and / or the metal oxide material undergoing direct reduction in the middle portion and / or lower inner portion of the direct reduction apparatus.
[0158] Therefore, the heat treatment is effectively performed, and the passivated and reduced metal material having a compact and dense structure provides an intermediate product resistant to reoxidation.
[0159] The intermediate product may be defined as small, round, pear-shaped, droplet-shaped, globule-shaped, bead-shaped, sphere-shaped or ellipsoidal bodies of passivated reduced metallic material having a compact and dense structure, which is used to produce the reoxidation resistant intermediate product.
[0160] Alternatively, the direct reduction apparatus is configured to allow the reduced metal material to descend into the lower internal portion and / or the middle internal portion to provide a heat treatment process for effectively heat treating the reduced metal material using a reducing agent having a higher temperature that provides additional thermal energy (in addition to the thermal energy of the metal oxide material) to reduce the cooling rate of the metal material undergoing direct reduction and / or heat treatment.
[0161] The control circuit is connected to the metal oxide preheating device and / or the heating device and is configured to control the material temperature of the metal oxide material to be charged so that the metal oxide material subjected to reduction and / or heat treatment is maintained (adjusted to increase / decrease) at a predetermined temperature of about 200°C to 600°C, preferably about 300°C to 500°C, during a predetermined time period that is long enough to enable a heat treatment process that provides the desired passivation parameter value of the reduced metal material to be carried out, which in turn obtains that the intermediate product becomes resistant to reoxidation.
[0162] Alternatively, the control circuit is further connected to a reductant preheating device, which is configured to preheat the reductant before it is introduced into the direct reduction device and is configured to control the gas temperature of the reductant so that the metal oxide material subjected to reduction and / or heat treatment is maintained (adjusted to increase / decrease) to a predetermined temperature of about 200°C to 600°C, preferably about 300°C to 500°C, during a predetermined time period that is long enough to enable a heat treatment process that provides the desired passivation parameter value of the reduced metal material to be carried out, which in turn results in the intermediate product becoming resistant to reoxidation.
[0163] Alternatively, the predetermined temperature is about 400°C to 800°C, preferably about 500°C to 700°C.
[0164] Alternatively, the predetermined temperature is about 600°C to 1000°C, preferably about 700°C to 900°C.
[0165] Alternatively, the desired passivation parameter value may be defined as a value for the rate and / or extent and / or grade and / or quota and / or proportion of reoxidation of the intermediate product (sponge iron and / or reduced iron ore material).
[0166] Alternatively, the control circuit may be adapted to control the temperature of the metal oxide material retaining thermal energy towards a predetermined temperature for providing a heat treatment process in a direct reduction device to heat treat the metal oxide material undergoing reduction during a predetermined period of time to achieve desired passivation parameter values with respect to porosity and / or size of sponge iron and / or weight per unit volume of sponge iron produced and / or metal particle structure and / or sample cutting uniformity and / or shrinkage and / or sintering and / or cold crushing strength and the like.
[0167] The desired passivation parameter value for porosity, its definition can be expressed as the ratio of the pore volume of the produced sponge iron to its total volume. The size of the sponge iron can be expressed as the average diameter of the sponge iron agglomerates typically produced. The weight per unit volume can be defined as a measure of the iron concentration of the sponge iron agglomerates typically produced. The metal grain structure can be defined as the final microstructure of the sponge iron agglomerates produced and the distribution of dense and porous areas. The sample cutting uniformity can define the density of the sponge iron agglomerates produced.
[0168] The heat treatment process provided by the control circuit during a predetermined time period to achieve the desired passivation parameters of the sponge iron produced enables the sponge iron or intermediate product to have a dense structure and / or high uniformity of final porosity and / or highly uniform chemical composition in specific areas (such as the central area of the sponge iron agglomerates) for cost-effective and energy-saving production in subsequent steel production in a steel plant, and resistance to reoxidation.
[0169] Alternatively, a high material temperature (e.g., any temperature in the range of about 600°C to about 900°C, or about 700°C to about 1000°C, or about 800°C to about 1100°C, or about 900°C to about 1200°C, or higher) of the metal oxide material to be charged and / or being charged into the direct reduction device encounters a reducing agent.
[0170] Alternatively, a portion of the hydrogen is used for chemical reactions in the middle section and / or the lower inner section.
[0171] Alternatively, the high material temperature of the metal oxide material charged into the upper inner portion of the reduction device provides a part of the heat energy for the chemical reaction and generates a high temperature top gas containing high temperature water vapor to be used in the high temperature electrolysis unit.
[0172] Alternatively, the metal oxide material subjected to direct reduction and / or the direct reduced metal material in the middle portion and / or the lower inner portion is subjected to the heat treatment process.
[0173] In this way, effective treatment and energy-saving recycling of high-temperature water vapor in the top gas produced by the chemical reaction supported by the metal oxide material of the high-temperature charge is achieved, the high-temperature water vapor is fed to the high-temperature electrolysis unit, and thus, due to the effective heat recovery of the high-temperature water vapor and due to the high content of high-temperature water vapor in the top gas discharged from the direct reduction device, energy-efficient operation of the high-temperature electrolysis unit is provided.
[0174] Alternatively, the high temperature electrolysis unit is configured to generate hydrogen, and the metal oxide material supplier unit is configured to provide the metal oxide material that retains thermal energy.
[0175] Alternatively, the direct reduction apparatus comprises a metal oxide material charge inlet means, a reducing agent inlet means configured to introduce a hydrogen-containing reducing agent that retains additional thermal energy.
[0176] Alternatively, the control circuit is configured to control the direct reduction of the metal oxide material by adjusting the temperature of the charged metal oxide material and the introduced hydrogen-containing reducing agent.
[0177] Alternatively, the metal material production configuration is suitable for reducing the metal oxide material by using at least a portion of the thermal energy of the metal oxide material charged into the direct reduction device to further heat the introduced hydrogen-containing reducing agent to a reaction temperature required for the chemical reaction to provide a chemical reaction between the hydrogen-containing reducing agent and the metal oxide material.
[0178] Alternatively, the direct reduction plant comprises a gas outlet arrangement configured for removing high temperature exhaust gas (top gas) from an upper inner portion of the direct reduction plant.
[0179] Alternatively, the metal material production arrangement comprises a first fluid line arrangement configured for fluid communication and adapted to feed high temperature steam of the high temperature exhaust gas to the high temperature electrolysis unit.
[0180] Alternatively, the second fluid line arrangement is configured for fluid communication and is adapted to feed hydrogen (produced by the high temperature electrolysis unit) from the high temperature electrolysis unit to the direct reduction plant.
[0181] In this manner, a high content of high-temperature water vapor in the high-temperature exhaust gas is achieved, which promotes effective utilization of the high-temperature water vapor injected into the high-temperature electrolysis unit.
[0182] Alternatively, the upper interior portion is configured to achieve a desired reaction temperature that is higher than the desired reaction temperature provided by the lower interior portion.
[0183] Alternatively, the heat-retaining metal oxide material charged to the direct reduction apparatus exhibits a temperature of 1000°C to about 1450°C, preferably about 1100°C to about 1300°C.
[0184] Alternatively, the method includes the step of providing high temperature exhaust gas (top gas) from the upper inner portion by charging a metal oxide material retaining heat energy into the upper inner portion to induce a chemical reaction between the metal oxide material and a hydrogen-containing reducing agent.
[0185] In this way, an endothermic chemical reaction can occur in the upper interior portion between the metal oxide material and the hydrogen-containing reducing agent, despite the fact that the hydrogen-containing reducing agent may contain a high content of water vapor generated by the chemical reaction.
[0186] By the high temperature of the charged metal oxide material which retains heat energy, the hydrogen-containing reducing agent which has risen to the upper inner portion is further heated due to the high temperature transfer from the charged metal oxide material, providing the (endothermic) chemical reaction, thereby achieving the high-temperature exhaust gas (top gas) generated in the upper inner portion containing high-temperature water vapor.
[0187] Alternatively, the high-temperature exhaust gas contains high-temperature water vapor in an amount of up to about 80% to 100% by volume, preferably about 85% to 95% by volume.
[0188] Alternatively, the high-temperature exhaust gas contains high-temperature water vapor in an amount of up to about 60% to 90% by volume, preferably about 70% to 80% by volume.
[0189] Alternatively, the high-temperature exhaust gas contains high-temperature water vapor in an amount of up to about 40% to 80% by volume, preferably about 50% to 70% by volume.
[0190] Alternatively, the high-temperature exhaust gas contains high-temperature water vapor in an amount of up to about 20% to 60% by volume, preferably about 30% to 40% by volume.
[0191] Alternatively, the high-temperature exhaust gas contains high-temperature water vapor in an amount of up to about 10% to 30% by volume, preferably about 15% to 20% by volume.
[0192] Alternatively, the high temperature exhaust gas (top gas) contains high temperature water vapor and excess hydrogen.
[0193] Alternatively, excess hydrogen is separated from the high temperature exhaust gas and recycled to and introduced into the direct reduction plant to provide direct reduction in the direct reduction plant.
[0194] Alternatively, the metal material production arrangement comprises a top gas recirculation arrangement adapted to recirculate excess hydrogen from the high temperature exhaust gas and add it to the hydrogen produced by the high temperature electrolysis unit.
[0195] Alternatively, a carbon-containing gas is added to the reducing agent to incorporate carbon into the intermediate product.
[0196] Alternatively, at least such amount of carbon-containing gas is added to the reducing agent that the intermediate product contains carbon.
[0197] Alternatively, the carbon-containing gas comprises methane and / or other carbon-containing gases from biogas production and / or carbon-containing gases from pyrolysis of renewable feedstocks and / or synthesis gas from biomass.
[0198] Alternatively, a reducing agent configured for direct reduction includes at least sufficient carbonaceous gas added thereto to provide an intermediate product comprising carbon.
[0199] Alternatively, the reducing agent comprises hydrogen configured for direct reduction of the metal oxide material and for providing chemical conversion of the metal oxide material to a carbon-free intermediate product.
[0200] Alternatively, the reducing agent (for example consisting of hydrogen and possibly containing a carbonaceous gas) is introduced into the reduction process at a temperature below and / or above the temperature of the metal oxide material charged to the direct reduction plant.
[0201] Alternatively, the reducing agent may be preheated to a certain extent before being introduced into the direct reduction device, wherein the temperature of the introduced reducing agent may be about 300°C to about 700°C, preferably about 400°C to about 650°C.
[0202] Alternatively, the carbon-containing material extracted from the carbon source is added to the directly reduced metal material in a separate carburizing zone of the direct reduction device and / or a separate carburizing reactor, wherein the carburizing zone and / or the carburizing reactor are configured to introduce carbon into the metal oxide material to provide an intermediate product discharged from the direct reduction device or the separate carburizing reactor.
[0203] Alternatively, the carbonaceous material comprises pure carbon or is a molecule such as methane, propane or other hydrocarbon or other element of a molecule.
[0204] Alternatively, the carbon production unit comprises a Sabatier reactor which produces methane CH4 from the reaction between hydrogen H2 and carbon dioxide CO2, said methane CH4 being a carbon-containing gas or a hydrogen-containing gas which is transferred to a separate carburizing zone and / or a separate carburizing reactor.
[0205] Alternatively, the carbon production unit and / or the carbon capture and utilization unit and / or the biogas production unit and / or the synthesis gas production unit are incorporated as an integrated unit of the preheating device and / or the metal production unit and / or the direct reduction plant and / or the electrolysis unit.
[0206] Alternatively, the carbon production unit comprises a Fischer-Tropsch plant configured to produce a carbonaceous product by reducing methane CH4 produced by a Sabatier reactor, said carbonaceous product being transferred to a separate carburizing zone and / or a separate carburizing reactor.
[0207] Alternatively, a carbon capture and utilization unit (CCU) comprises a CO2 capture device CCD configured to capture CO2 from the atmosphere, and the captured CO2 may be transferred to the Sabatier reactor configured to produce carbon-dependent methane CH4.
[0208] Alternatively, a carbon production unit configured for producing non-fossil produced carbon is used by a cement industry plant that manufactures cement from mined calcium minerals.
[0209] Alternatively, the method comprises the steps of: directly reducing the metal oxide material by means of a reducing agent having a hydrogen content of at least 80% by volume; wherein the carbon content in the directly reduced metal material is then increased by means of a carburizing gas, and thereafter at least partially releasing the used carburizing gas while largely avoiding mixing of the carburizing gas with the reducing agent.
[0210] Alternatively, the reducing agent comprises a hydrogen content of at least about 40 vol% to 60 vol%, or about 50 vol% to 70 vol%, or about 60 vol% to 80 vol%, or about 70 vol% to 90 vol%.
[0211] Alternatively, the carburizing zone corresponds to an independent (isolated) carburizing zone configured to prevent the carbonaceous substance from mixing with the reducing agent.
[0212] Alternatively, the carburizing zone constitutes a carburizing space inside the direct reduction device, the carburizing space being configured to reduce the metal oxide material, and being configured to carburize the metal oxide material subjected to reduction by mixing the carbonaceous substance with the reducing agent.
[0213] Alternatively, the carburizing zone constitutes a carburizing space (not shown) inside the direct reduction device, which is configured to reduce the metal oxide material, and is configured to carburize the metal oxide material subjected to reduction, and to mix the carbonaceous substance with the reducing agent.
[0214] By utilizing the thermal energy of the metal oxide material to further heat the introduced reducing agent, a chemical reaction between the metal oxide material and the reducing agent is achieved in an energy efficient manner.
[0215] Alternatively, the control circuit is suitable for controlling the temperature of the metal oxide material transferred to the direct reduction device and / or controlling the internal gas pressure and / or the reducing agent temperature and / or the reducing agent gas pressure of the introduced reducing agent in the direct reduction device to achieve a predetermined temperature of the metal oxide material undergoing reduction and / or heat treatment.
[0216] Alternatively, the direct reduction apparatus is configured to contain the metal oxide material at a temperature in the range of about 600°C to 1500°C.
[0217] Alternatively, the direct reduction apparatus is configured to contain the metal oxide material at a temperature in the range of about 500°C to 1600°C, preferably in the range of about 800°C to 1300°C.
[0218] Alternatively, the reduced metallic material consists of reduced iron particles which are combined with one another to form pellets of heat-treated and / or heat-hardened and / or passivated reduced iron material in the form of iron droplets.
[0219] Thus, an intermediate product (reduced iron material) suitable for the production of steel ("iron drop" or "iron drip") is achieved, thereby enabling environmentally friendly (carbon-free / low-carbon) production while achieving safe transportation to the steel mill (anti-reoxidation).
[0220] The intermediate product produced is advantageous because the optimum amount of carbon can be added more precisely in the EAF to achieve the desired steel quality.
[0221] The present disclosure may not be limited to the examples described above, but many possibilities of modifications or combinations of the examples described herewith will be apparent to a person skilled in the art without departing from the basic idea as defined in the appended claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0222] In the following, the present invention will be described with reference to examples and the accompanying schematic drawings, from which some unimportant details may be omitted for the sake of clarity and understanding of the present invention.
[0223] Figure 1 A metal material production configuration suitable for reducing a metal oxide material according to a first example is shown;
[0224] Figure 2 shows a flow chart provided by a metal material production arrangement according to a second example;
[0225] Figure 3 A metal material production configuration suitable for reducing a metal oxide material according to a third example is shown;
[0226] Figure 4 A phase diagram showing the iron domain as a function of the oxidizing power of hydrogen and temperature;
[0227] Figure 5 The phase diagram of hydrogen / hydrogen + iron Mol / mol versus temperature is shown;
[0228] Figures 6a to 6c The stages of structural transformation of iron ore agglomerates associated with the thermal treatment process are shown;
[0229] Figure 7a to Figure 7b A metal material production configuration suitable for reducing a metal oxide material according to a fourth example is shown;
[0230] Figure 8 shows a closed loop diagram used in a metal material production configuration according to a fifth example;
[0231] Figure 9a to Figure 9b A flow chart showing an exemplary method of reducing a metal oxide material retaining thermal energy to a reduced metal material is shown;
[0232] Fig.10 A control circuit of a metal material production arrangement according to a sixth example is shown; and
[0233] Fig.11 A metal material production arrangement suitable for reducing iron ore oxide material according to a fifth example is shown. DETAILED DESCRIPTION
[0234] Figure 1A metal material production configuration suitable for reducing a metal oxide material according to a first example is shown. Figure 1 A metal material production arrangement 1 suitable for reducing a metal oxide material 5 retaining thermal energy into a reduced metal material 16 is shown.
[0235] The metal material production arrangement 1 includes a metal oxide material supply device unit 3 configured to provide a metal oxide material 5 retaining thermal energy, such as a metal oxide granulation device or a metal oxide preheating device. The metal material production arrangement 1 includes a reduction device 7 configured to reduce the metal oxide material 5 retaining thermal energy. The metal oxide material charging transfer unit (not shown) of the metal material production arrangement 1 is configured to charge the metal oxide material 5 into the upper inner part UP of the reduction device 7.
[0236] The reduction device 7 includes a reducing agent inlet (not shown) configured to introduce a hydrogen-containing reducing agent 6 into a lower inner portion of the reduction device 7, whereby the introduced hydrogen-containing reducing agent 6 is heated or further heated by utilizing the thermal energy of the metal oxide material 5 to provide a chemical reaction between the hydrogen-containing reducing agent 6 and the metal oxide material 5, so that the hydrogen-containing reducing agent 6 is suitable for reacting with the metal oxide material 5 that retains thermal energy to reduce the metal oxide material 5.
[0237] The hydrogen gas of the hydrogen-containing reducing agent 6 may be generated by an electrolysis unit 17 , which includes a reducing agent temperature regulator 18 configured to regulate (preheat or cool) the temperature of the hydrogen-containing reducing agent 6 .
[0238] The reduction device 7 is configured to provide a heat treatment process for heat treating the metal oxide material 5 subjected to reduction and / or the reduced metal material 16. The metal material production arrangement 1 includes a control circuit 50 electrically connected to the reducing agent temperature regulator 18 to preheat the hydrogen-containing reducing agent 6.
[0239] The control circuit 50 is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent 6 to provide at least one desired passivation parameter value of the reduced metal material 16. The control circuit 50 is electrically coupled to the metal oxide material supply device unit 3 and is adapted to control the temperature of the metal oxide material to be loaded into the upper inner portion UP. The reduced metal material 16 exhibiting at least one desired passivation parameter value is discharged from the reduction device 7 and transported to a steel producer (not shown), while the reduced metal material resists reoxidation due to the passivation of the reduced metal material 16.
[0240] The reduction device 7 is also configured to allow the reduced metal material 16 to descend into the lower inner portion LP to provide a heat treatment process for heat treating the reduced metal material using the additional heat energy provided by the hydrogen-containing reducing agent. It has been shown that the chemical reactivity and / or high driving force of the hydrogen gas of the hydrogen-containing reducing agent 6 are maintained.
[0241] Chemical reactivity and / or high driving force are essential to provide effective reduction of the metal oxide material. The introduced hydrogen-containing reducing agent 6 contains 80% to 100% hydrogen, preferably 100% hydrogen. The control circuit 50 is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent 6 toward a predetermined temperature to provide sintering and / or heat treatment of the metal oxide material 5 undergoing reduction during a predetermined period of time.
[0242] Alternatively, the temperature of the metal oxide material to be loaded into the upper inner portion is controlled within a range of 900°C to 1500°C, preferably 1000°C to 1300°C by a control circuit.
[0243] Alternatively, the temperature of the hydrogen-containing reducing agent is controlled by a control circuit within the range of 100°C to 400°C, preferably 200°C to 300°C; or 0°C to 300°C, preferably 100°C to 200°C.
[0244] Figure 2 A flow chart provided by a metal material production configuration 1 according to a second example is shown. A metal oxide material 5 retaining heat energy is loaded into a reduction device 7. The reduction device 7 can be defined as having an upper inner portion UP, an intermediate inner portion IP, and a lower inner portion LP. A hydrogen-containing reducing agent 6 is introduced into the intermediate inner portion IP and flows upward, encountering the metal oxide material 5 retaining heat energy transferred downward, whereby the upper inner portion UP acts as a countercurrent heat exchange zone to provide a chemical reaction between the metal oxide material and the hydrogen-containing reducing agent 6.
[0245] Alternatively, the hydrogen-containing reducing agent 6 is preheated.
[0246] Alternatively, the metal oxide material that retains the heat energy is transferred from the upper interior portion to the middle interior portion and / or the lower interior portion by gravity.
[0247] Alternatively, the temperature of the hydrogen-containing reducing agent 6 introduced into the upper inner portion UP is controlled by a control circuit (not shown) to provide that the spent reducing fluid 4 resulting from the reduction contains 100% water vapor or substantially 100% water vapor.
[0248] Alternatively, the temperature of the hydrogen-containing reducing agent 6 introduced into the upper inner portion UP is controlled by a control circuit (not shown) to provide that the spent reducing fluid 4 produced by the reduction contains more than 90% water vapor and the remainder hydrogen-containing reducing agent. In this way, an excess volume of hydrogen-containing reducing agent is achieved and complete reduction of the metal oxide material is ensured.
[0249] Due to the high temperature of the charged metal oxide material 5, efficient reduction of the metal oxide material 5 is achieved despite the fact that the hydrogen-containing reducing agent 6 contains a large amount of water vapor.
[0250] A preheated hydrogen-containing reducing agent 6' is additionally introduced in the middle inner portion IP and / or the lower inner portion LP. The temperature of the additionally introduced preheated hydrogen-containing reducing agent 6' is controlled by the control circuit to adapt the temperature to a predetermined temperature, thereby achieving sintering and / or heat treatment of the reduced metal material 16 during a predetermined period of time to provide at least one desired passivation parameter value of the reduced metal material 16.
[0251] Alternatively, the introduction position of the introduced preheated hydrogen-containing reducing agent 6' may be adjusted vertically VD along the extension of the direct reduction device 7 to control the heat treatment process to achieve optimal sintering and produce dense and solid reduced metallic material blocks or pellets.
[0252] Figure 3 A metal material production arrangement 1 suitable for reducing a metal oxide material 5 retaining thermal energy into a reduced metal material 16 according to a third example is shown. The metal material production arrangement 1 comprises a metal oxide material supply device unit 3 configured to provide the metal oxide material 5 retaining thermal energy, such as a metal oxide granulation device or a metal oxide preheating device. The metal material production arrangement 1 comprises a reduction device 7 configured to reduce the metal oxide material 5 retaining thermal energy.
[0253] The metal oxide material charging transfer unit 12 of the metal material production configuration 1 is configured to load the metal oxide material 5 into the upper internal part UP of the reduction device 7 via the metal oxide material charging equipment a, and the metal oxide material charging equipment a includes, for example, a transmission fireproof steel belt (not shown) configured to load the metal oxide material 5 retaining thermal energy into the top section of the upper internal part UP.
[0254] The reduction device 7 includes a reducing agent inlet b configured to introduce a preheated hydrogen-containing reducing agent 6 into the middle inner portion IP of the reduction device 7, whereby the introduced preheated hydrogen-containing reducing agent 6 is heated or further heated by utilizing the thermal energy of the metal oxide material 5 for providing a chemical reaction between the preheated hydrogen-containing reducing agent 6 and the metal oxide material 5, so that the preheated hydrogen-containing reducing agent 6 is suitable for reacting with the metal oxide material 5 retaining thermal energy to reduce the metal oxide material 5. The hydrogen of the preheated hydrogen-containing reducing agent 6 may be generated by an electrolysis unit (not shown).
[0255] The metal oxide material 5 retaining heat energy descends through the upper inner portion UP and is subsequently reduced in the upper inner portion UP to be reduced metal material 16. The temperature of the introduced preheated hydrogen-containing reducing agent 6 increases as the introduced preheated hydrogen-containing reducing agent 6 rises higher in the upper inner portion UP, where the metal oxide material 5 retaining heat energy meets the introduced preheated hydrogen-containing reducing agent 6 and the metal oxide material 5 retaining heat energy is cooled. The upper inner portion UP acts as a countercurrent heat exchange zone and promotes the chemical reaction between the metal oxide material and the preheated hydrogen-containing reducing agent 6.
[0256] Furthermore, the intermediate inner portion IP is configured for providing a heat treatment process for heat treating the reduced metal material 16 in the intermediate inner portion IP. The reduced metal material 16 descends from the upper inner portion UP into the intermediate inner portion IP.
[0257] The control circuit 50 is electrically coupled to the reductant preheater 18 configured to preheat the hydrogen-containing reductant 6 to be introduced into the intermediate inner portion IP via the reductant inlet b.
[0258] The control circuit 50 controls the temperature of the reduced metal material 16 toward a predetermined temperature, for example, set within a range of 200°C to 600°C, preferably 300°C to 500°C, during a predetermined time period long enough to enable the heat treatment process to proceed to provide at least one desired passivation parameter value of the reduced metal material.
[0259] In this manner, the temperature of the introduced preheated hydrogen-containing reducing agent 6 is controlled by the control circuit 50 to maintain the temperature of the reduced metallic material 16 in the intermediate inner portion IP at an elevated predetermined temperature for an extended period of time to effectuate the heat treatment process.
[0260] In this way, a heat treatment process for heat treating the reduced metallic material is achieved which utilizes the additional thermal energy provided by the preheated hydrogen-containing reducing agent 6 , wherein the heat treatment process is controlled by the control circuit 50 .
[0261] The control circuit 50 is configured to control the additional thermal energy by adjusting the temperature of the introduced preheated hydrogen-containing reducing agent in such a manner that at least one desired passivation parameter value of the reduced metallic material is achieved.
[0262] The control circuit 50 may be electrically coupled to a further reducing agent preheater 18 ′ configured to preheat the hydrogen-containing reducing agent 6 introduced into the lower interior portion LP of the reduction device 7 .
[0263] The introduced preheated hydrogen-containing reducing agent 6 fed into the lower inner portion LP may contain 80% to 100% hydrogen, preferably 100% hydrogen. The control circuit 50 is adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent 6 fed into the lower inner portion LP toward a predetermined temperature to provide sintering and / or heat treatment of the reduced metallic material 16 during a predetermined period of time.
[0264] Alternatively, the volume of hydrogen-containing reducing agent introduced is such that complete reduction of the metal oxide material is achieved, and an excess volume of hydrogen-containing reducing agent is provided in the reduction device to provide said reduction of the metal oxide material.
[0265] Figure 4 A phase diagram of the iron domain as a function of the oxidizing power of hydrogen and temperature for a gas mixture H2-H2O is shown. As shown in the figure, the reduction of the iron ore oxide material in the form of hematite and / or magnetite and / or wüstite to reduced iron ore material occurs in two or three stages, depending on whether the temperature is above or below 570°C. In this case, the hematite Fe2O3 is first reduced to magnetite Fe3O4 and then to wüstite Fe 1-Y O, and is eventually reduced to iron Fe.
[0266] The preheated hydrogen-containing reducing agent 6 introduced into the reduction device rises through the upper inner portion and contacts the descending iron ore oxide material being reduced, and the preheated hydrogen-containing reducing agent 6 will contain an increasing amount of water as the introduced preheated hydrogen-containing reducing agent 6 rises higher in the upper inner portion UP. As shown in the figure, hematite will be reduced to magnetite at a high temperature (e.g., 1200° C.), and reduction to magnetite can still be achieved despite the high water content (e.g., 90%) of the preheated hydrogen-containing reducing agent 6. The inventive solution to at least one of the target problems utilizes the high temperature of the iron ore oxide material that retains thermal energy and is charged into the upper inner portion from the iron ore oxide material supply device unit. This high temperature of the iron ore oxide material makes reduction possible despite the fact that the preheated hydrogen-containing reducing agent will contain an increasing amount of water when it reaches the upper region of the upper inner portion.
[0267] Figure 5A hydrogen / hydrogen+iron Mol / mol phase diagram from different temperature aspects is shown. The mark O represents the liquid phase, the mark P represents the Bcc / liquid phase, the mark Q represents the Bcc phase, and the mark R represents the Fcc phase. As shown in the figure, the iron Fe will undergo sintering in the Bcc+liquid phase P, that is, the iron of the reduced iron ore material is hardened by a relatively low temperature (e.g., 200°C to 600°C) due to the fact that the introduced hydrogen maintains its chemical reactivity and / or high driving force.
[0268] The hydrogen does not need to be "burned" or intensely heated to, for example, 1200° C., as taught in the prior art, in order to provide heat for the reduction.
[0269] In contrast, by using the thermal energy of the iron ore oxide material charged to the reduction apparatus to provide reduction, the temperature of the introduced hydrogen-containing reducing agent may be controlled and / or adjusted and / or fine-tuned to achieve at least one desired passivation parameter value.
[0270] Therefore, the thermal treatment process can be effectively controlled by the control circuit by controlling the temperature of the introduced hydrogen gas and maintaining high chemical reactivity and / or high driving force.
[0271] Alternatively, the control circuitry is therefore adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent to provide sintering of reduced iron ore material agglomerates over an extended period of time by such relatively low temperatures to achieve a reduced iron ore material that is resistant to reoxidation.
[0272] In this way it is achieved that the intermediate products (eg sponge iron, such as pellets, briquettes etc.) are prevented from having a tendency to revert to an oxidized state when exposed to the elements and the risk of autoignition processes is reduced.
[0273] Alternatively, the control circuit is adapted to control the internal gas pressure in the reduction device and / or the hydrogen temperature and / or the hydrogen pressure of the preheated hydrogen-containing reducing agent.
[0274] The control circuit 50 is adapted to provide sintering of reduced iron ore agglomerates subjected to sintering in the Bcc+ liquid phase P, or preferably exposing the reduced metallic material by temperatures in the range of, for example, 200°C to 600°C and a high hydrogen / hydrogen+iron Mol / mol relationship (shaded area S) of, for example, 0.75 to 1.0. By such relatively low temperatures, over extended periods of time, and by hydrogen having high chemical reactivity and / or high driving force, a reduced iron ore material resistant to reoxidation is provided.
[0275] Figures 6a to 6c The stages of structural transformation of iron ore agglomerates associated with the thermal treatment process are shown. Figure 6aThe agglomerate structure of heat-retaining iron ore oxide material 5 undergoing reduction in the upper interior portion of a reduction apparatus (not shown) is shown. The iron ore oxide particles 10 are shown bonded to each other to form porous agglomerates 20, the porosity of which facilitates contact between the iron ore oxide and the introduced preheated hydrogen-containing reducing agent during reduction. Figure 6b An agglomerate 20 with reduced iron ore oxide material is shown ready for heat treatment. Alternatively, the particles 10 have been sintered in the upper inner portion. Some iron ore oxide material (FeO) may be trapped and / or retained in the pores of the agglomerate 20. In order to provide a reduced iron ore material that is resistant to reoxidation, a heat treatment process is provided for heat treating the reduced iron ore material and / or the iron ore oxide material subjected to reduction. This is achieved by the control circuit 50 being adapted to control the temperature of the introduced preheated hydrogen-containing reducing agent 6 to a predetermined temperature to provide sintering and / or heat treatment of the iron ore oxide material during a predetermined time period. Figure 6c A fully reduced or substantially fully reduced iron ore material is shown wherein the particles 10 of the agglomerates 20 form a denser structure which hides the resulting FeO from contact with the surrounding atmosphere outside the agglomerates 20 as the agglomerates 20 are discharged from the reduction apparatus. Figure 6c The particles 10 of the agglomerates 20 of the reduced iron ore material 16 are shown formed by (eg, combining Figure 5 A denser structure is achieved by sintering (as shown and described).
[0276] Figure 7a to Figure 7b A metal material production arrangement 1 according to a fourth example is shown which is suitable for reducing a metal oxide material 5 retaining thermal energy into a reduced metal material 16. The metal material production arrangement 1 comprises a metal oxide material supply device unit 3 configured to provide the metal oxide material 5 retaining thermal energy, such as a metal oxide granulation device or a metal oxide preheating device.
[0277] The metal material production arrangement 1 comprises a reduction device 7 configured to reduce the metal oxide material 5 retaining thermal energy. The metal oxide material 5 retaining thermal energy is loaded into an upper inner portion UP of the reduction device 7.
[0278] The reducing agent preheater 18 configured to preheat the hydrogen-containing reducing agent is electrically connected to the control unit 50. The preheated hydrogen-containing reducing agent 6 is introduced into the middle inner part IP of the reduction device 7, whereby the introduced preheated hydrogen-containing reducing agent 6 is heated or further heated by utilizing the thermal energy of the metal oxide material 5 for providing a chemical reaction between the preheated hydrogen-containing reducing agent 6 and the metal oxide material 5 retaining the thermal energy, so that the preheated hydrogen-containing reducing agent 6 is suitable for reacting with the metal oxide material 5 retaining the thermal energy to reduce the metal oxide material 5.
[0279] The metal oxide material supplier unit 3 is electrically coupled to a control circuit 50 adapted to coarsely set the thermal energy of the metal oxide material 5. The control circuit 50 controlling the reductant preheater 18 is adapted to finely set the temperature of the introduced preheated hydrogen-containing reductant 6 to achieve at least one desired passivation parameter value.
[0280] Figure 7a The control circuit 50 in is adapted to control the temperature of the chemical reaction by coarsely adjusting the thermal energy provided by the metal oxide material supplier unit 3, and by finely adjusting the temperature required for the chemical reaction and / or heat treatment process by controlling the temperature of the introduced preheated hydrogen-containing reducing agent 6.
[0281] Furthermore, the preheated hydrogen-containing reducing agent may be introduced into the reduction device at different levels and may be introduced at different temperatures, pressures, flow rates, etc.
[0282] For example, the control circuit 50 may be electrically coupled to a further reducing agent preheater 18 ′ configured to preheat the hydrogen-containing reducing agent 6 introduced into the lower interior portion LP of the reduction device 7 .
[0283] In this way, an effective regulation of the temperature for reducing the metal oxide material is achieved, while at the same time an effective regulation of the temperature for the heat treatment of the reduced metal material is achieved.
[0284] The introduced preheated hydrogen-containing reducing agent 6 fed into the lower and / or inner portion LP may contain 80% to 100% hydrogen, preferably 100% hydrogen.
[0285] Alternatively, the temperature of the preheated hydrogen-containing reducing agent 6 introduced into the intermediate inner portion IP is controlled by the control circuit 50 so as to provide the spent reducing fluid 4 produced by the reduction to contain 100% of water vapor or substantially 100% of water vapor and to be discharged. Due to the high temperature of the charged metal oxide material 5, effective reduction of the metal oxide material 5 is achieved despite the fact that the preheated hydrogen-containing reducing agent 6 contains a large amount of water vapor.
[0286] Figure 7b The reduction device 7 is shown in cross section. Preheated hydrogen-containing reducing agent 6 is introduced circumferentially around the middle inner part. Spent reducing fluid 4 is discharged circumferentially from the reduction device 7.
[0287] Figure 8 A closed-loop diagram of a closed-loop algorithm used in a metal material production configuration according to a fifth example is shown.
[0288] The control circuit 50 is electrically connected to the metal oxide material supply device unit 3, such as a metal oxide granulation device or a metal oxide preheating device, and is adapted to adjust the temperature of the metal oxide material retaining heat energy to be charged into the reduction device. The control circuit 50 may be adapted to control the temperature of the metal oxide material retaining heat energy toward a predetermined temperature value PDTV for providing a heat treatment process in the reduction device for heat treating the metal oxide material subjected to reduction and / or the reduced metal material during a predetermined time period, thereby achieving at least one desired passivation parameter value DPPV of the reduced metal material.
[0289] The at least one desired passivation parameter value DPPV may relate to a porosity parameter and / or a size parameter and / or a weight parameter and / or a metal grain structure parameter and / or a sample cutting uniformity parameter and / or a shrinkage parameter and / or a sintering parameter and the like.
[0290] The passivation parameter detector PPD is associated with the reduction device for detecting the actual passivation parameter value APPV. The control circuit 50 may perform calculation and comparison procedures for regulating the temperature of the metal oxide material holding the heat energy through the metal oxide material supplier unit 3 .
[0291] Alternatively, the control circuit 50 may be adapted to control the temperature of the charged metal oxide material in such a way that the predetermined temperature value PDTV for providing the thermal treatment process assumes a temperature value of the thermal treatment process for reaching at least one desired passivation parameter value DPPV.
[0292] The control circuit 50 repeats the closed loop algorithm until at least one desired passivation parameter value DPPV is reached.
[0293] The control circuit 50 is electrically connected to the reducing agent temperature regulating device 18, which is configured to regulate the temperature of the hydrogen-containing reducing agent to be introduced into the reduction device of the metal material production configuration to achieve at least one desired passivation parameter value DPPV of the reduced metal material. The closed loop diagram can use a startup process, in which an input temperature value IN of the preheated hydrogen-containing reducing agent is used.
[0294] The control circuit 50 is adapted to control the reducing agent temperature regulating device 18 in such a way that the temperature of the introduced preheated hydrogen-containing reducing agent is regulated towards a predetermined temperature value PDTV for providing a heat treatment process for heat treating the metal oxide material subjected to reduction and / or the reduced metal material during a predetermined period of time in the reduction device, thereby reaching at least one desired passivation parameter value DPPV of the reduced metal material. When determining the predetermined temperature value PDTV, the control circuit 50 takes into account the at least one desired passivation parameter value DPPV. In view of achieving an effective passivation of the reduced metal material, the at least one desired passivation parameter value DPPV of the reduced metal material is determined.
[0295] The at least one desired passivation parameter value DPPV may relate to a porosity parameter and / or a size parameter and / or a weight parameter and / or a metal grain structure parameter and / or a sample cutting uniformity parameter and / or a shrinkage parameter and / or a sintering parameter and the like.
[0296] The passivation parameter detector PPD is associated with the reduction device and is used to detect the actual passivation parameter value APPV.
[0297] The actual passivation parameter value APPV of the reduced metallic material is detected by a passivation parameter detector PPD electrically coupled to the control circuit 50. The control circuit 50 performs a calculation and comparison routine for adjusting the reducing agent temperature regulating device 18 in such a way that the temperature of the introduced preheated hydrogen-containing reducing agent is adapted to a predetermined temperature value PDTV in order to reach at least one desired passivation parameter value DPPV.
[0298] The control circuit 50 repeats the closed loop algorithm until at least one desired passivation parameter value DPPV is reached.
[0299] The control circuit 50 is configured to compare the actual passivation parameter value APPV with at least one desired passivation parameter value DPPV and control the reductant temperature regulating device 18 to regulate the temperature of the hydrogen-containing reductant until the at least one desired passivation parameter value DPPV is reached.
[0300] The metal oxide material retaining the heat energy may be metal oxide pellets which are preheated to contain the heat energy. The metal oxide pellets may be produced by a granulation device processing a metal mixture and transferred to a reduction device via a conveyor steel belt.
[0301] The upper interior portion of the reduction device is configured for reducing the metal oxide particles, and the reduction device is configured to provide a chemical reaction between the hydrogen-containing reducing agent and the metal oxide pellets.
[0302] The lower portion and / or the middle portion are configured for use in a thermal treatment process for thermally treating the metal oxide material.
[0303] The reduced and thermally hardened metal material is discharged from the lower inner portion through a discharge transport unit coupled to the opening of the lower inner portion.
[0304] The product produced by the method is a reduced metal material (16) consisting of reduced iron ore particles which are bonded to each other to form pellets of heat-treated and / or heat-hardened and / or passivated reduced iron ore material in the form of iron droplets.
[0305] Alternatively, the computer of the control circuit is electrically connected to the metal oxide material charging device for controlling the charging rate into the reduction device.
[0306] The computer may be electrically connected to the metal oxide material supply device unit for controlling the temperature of the metal oxide pellets to be loaded, and / or electrically connected to the reducing agent temperature regulating device for controlling the temperature of the introduced hydrogen-containing reducing agent, and / or electrically connected to the exhaust transmission unit.
[0307] Figure 9a A flow chart showing an exemplary method of reducing a metal oxide material that retains thermal energy into a reduced metal material by a metal material production configuration is shown. The metal material production configuration includes: a metal oxide material supply device unit configured to provide a metal oxide material that retains thermal energy; a metal oxide material charging device configured to charge the metal oxide material into the upper internal portion of the reduction device; a reducing agent inlet device configured to introduce a hydrogen-containing reducing agent into the middle internal portion and / or the lower internal portion of the reduction device, thereby heating or further heating the introduced hydrogen-containing reducing agent by utilizing the thermal energy of the metal oxide material for providing a chemical reaction between the hydrogen-containing reducing agent and the metal oxide material, so that the hydrogen-containing reducing agent is suitable for reacting with the metal oxide material that retains thermal energy to reduce the metal oxide material. The metal material production configuration is configured to provide a heat treatment process for heat-treating the metal oxide material that is subjected to reduction and / or the reduced metal material; and a control circuit electrically connected to a reducing agent temperature regulating device configured to regulate the temperature of the hydrogen-containing reducing agent is suitable for controlling the temperature of the introduced hydrogen-containing reducing agent to achieve at least one desired passivation parameter value of the reduced metal material.
[0308] Figure 9aThe method in begins at step 901. Step 902 includes adapting the method. Step 903 includes stopping the method. Step 902 may include the following steps: heating or further heating the introduced hydrogen-containing reducing agent using the thermal energy of the metal oxide material to provide a chemical reaction between the hydrogen-containing reducing agent and the metal oxide material, thereby reducing the metal oxide material in the upper inner portion; providing a thermal treatment process for thermally treating the metal oxide material undergoing reduction and / or thermally treating the reduced metal material before being discharged from the lower inner portion; and controlling the temperature of the introduced hydrogen-containing reducing agent for adjusting the chemical reaction and / or the thermal treatment process to achieve at least one desired passivation parameter value of the reduced metal material.
[0309] Figure 9b A flow chart showing an exemplary method for reducing a metal oxide material that retains heat energy by a metal material production configuration disclosed herein is shown. The method begins at step 1001. Step 1002 includes preheating of the metal oxide material. Step 1003 includes charging the metal oxide material that retains heat energy into a reduction device. Step 1004 includes introducing preheated hydrogen into the reduction device. Step 1005 includes heating or further heating the introduced hydrogen-containing reducing agent using the heat energy of the metal oxide material to provide a chemical reaction between the hydrogen-containing reducing agent and the metal oxide material, thereby reducing the metal oxide material in the upper internal portion. Step 1006 includes providing a heat treatment process for heat treating the reduced metal material in the middle internal portion and / or the lower internal portion. Step 1007 includes controlling the temperature of the introduced hydrogen-containing reducing agent for adjusting the chemical reaction and / or the heat treatment process to achieve at least one desired passivation parameter value of the reduced metal material. Step 1008 includes discharging the reduced metal material from the reduction device, the reduced metal material having at least one desired passivation parameter value and resisting reoxidation. Step 1009 comprises stopping of the method.
[0310] Alternatively, the reducing agent preheating device is adapted to adjust the temperature of the preheated introduced hydrogen-containing reducing agent.
[0311] Fig.10 A metal material production configuration 1 according to a sixth example is shown, the control circuit 50 including a computer (not shown). The control circuit 50 is configured to control any of the exemplary methods disclosed herein. The control circuit 50 may include a non-volatile memory NVM 1020, which is a computer memory that can retain stored information even when the control circuit 50 or the computer is not powered. The control circuit 50 also includes a processing unit 1010 and a read / write memory 1050.
[0312] The NVM 1020 comprises a first memory unit 1030. A computer program (which may be of any type suitable for any operational database) is stored in the first memory unit 1030 for controlling the functions of the control circuit 50.
[0313] Furthermore, the control circuit 50 comprises a bus controller (not shown), a serial communication port (not shown) providing a physical interface through which information is transmitted in both directions, an I / O module (not shown) of any suitable type providing input / output signal transmission, an A / D converter (not shown) for converting continuously varying signals from the following into binary codes suitable for processing by the computer of the control circuit 50: a passivation parameter detector PPD and / or a temperature sensor device and / or different monitoring units (not shown) for detecting the temperature of the metal oxide material retaining thermal energy and / or the temperature of the hydrogen-containing reducing agent introduced into the reduction device.
[0314] The control circuit 50 also includes an input / output unit (not shown) for adapting the time and date. The control circuit 50 may also include an event counter (not shown) for counting the number of event quantities generated during the adjustment of the chemical reaction and / or thermal treatment process to reach at least one desired passivation parameter value of the reduced metallic material.
[0315] In addition, the control circuit 50 includes an interrupt unit (not shown) for providing multi-tasking performance and real-time calculation. The NVM 1020 also includes a second memory unit 1040 for external control operations.
[0316] The data medium suitable for storing the data program P comprises drive routines suitable for instructing the operation of the metal material production arrangement 1 .
[0317] The data program P is suitable for operating the control circuit 50 to perform any of the exemplary methods described herein. The data program P includes routines for executing instructions under the operation of the metal material production configuration 1. The data program P includes program codes readable on a computer for causing the computer to perform the exemplary methods described herein.
[0318] The data program P may also be stored in the independent memory 1060 and / or in the read / write memory 1050. The data program P in this embodiment is stored in an executable or compressed data format.
[0319] It should be understood that when processing unit 1010 is described as performing specific functions, this involves processing unit 1010 executing specific portions of a program stored in separate memory 1060 or specific portions of a program stored in read / write memory 1050 .
[0320] The processing unit 1010 is associated with a signal (data) port 1099 for communication via the first data bus 1015, which may be adapted to be electrically coupled to electronic control circuitry of an operator station (not shown).
[0321] In this way it is achieved that an operator via the display of the electronic control circuit can control and monitor the metal material production arrangement 1 .
[0322] The non-volatile memory NVM 1020 is adapted to communicate with the processing unit 1010 via the second data bus 1012. The independent memory 1060 is adapted to communicate with the processing unit 1010 via the third data bus 1011. The read / write memory 1050 is adapted to communicate with the processing unit 1010 via the fourth data bus 1014. The signal (data) port 1099 may be connectable to a data link, for example, a network connected to the control circuit 50.
[0323] When the data port 1099 receives data, the data will be temporarily stored in the second storage unit 1040. After temporarily storing the received data, the processing unit 1010 will prepare to execute the program code according to the exemplary method.
[0324] Preferably, the signal (received by the signal (data) port 1099 ) comprises information about the operating status of the metal material production arrangement 1 .
[0325] Signals received at signal port 1099, such as a serial bus, may be used by control circuit 50 for controlling and monitoring the reduction and heat treatment processes.
[0326] The signals received by the signal (data) port 1099 may be used for historical data and data regarding the operation of the metal material production arrangement 1 .
[0327] The metal material production arrangement 1 can be configured to be connected to a data network via a signal bus, which is configured as an electrical interface for explicitly providing electrical compatibility and related data transmission, which data may include information about the status of the metal material production arrangement 1 and the sensor device. Data can also be manually entered into or presented from the computer via a suitable communication device such as a display (not shown).
[0328] Independent sequences of the method may be performed by a computer, wherein the computer runs a data program P stored in the independent memory 1060 or the read / write memory 1050. When the computer runs the data program P, the method steps according to any example disclosed herein will be performed.
[0329] A data program product comprising a program code stored on a data medium may be provided, which product is readable on a suitable computer for executing the exemplary method steps herein when the data program P is run on the computer.
[0330] Fig.11 A metal material production arrangement 1 suitable for reducing an iron ore oxide material 5 retaining thermal energy into a reduced iron ore material 16 is shown. The metal material production arrangement 1 includes an iron ore oxide material supply device unit 3, which is configured to provide the iron ore oxide material 5 retaining thermal energy. The iron ore oxide material charging device a is configured to charge the iron ore oxide material 5 into the upper inner part UP of the reduction device 7. The reducing agent inlet device b is configured to introduce the hydrogen-containing reducing agent 6 into the middle inner part IP and / or the lower inner part LP of the reduction device 7. The hydrogen-containing reducing agent 6 is preheated, and the introduced hydrogen-containing reducing agent 6 is further heated by utilizing the thermal energy of the iron ore oxide material 5 for providing a chemical reaction between the hydrogen-containing reducing agent 6 and the iron ore oxide material 5, thereby being suitable for reacting with the iron ore oxide material 5 retaining thermal energy for reducing the iron ore oxide material 5.
[0331] The reducing agent 6 is preheated and introduced into the direct reduction device 7 so that the reducing agent 6, in addition to providing direct reduction and / or chemical reaction, also reduces the cooling rate of the directly reduced iron ore material RT and / or the iron ore oxide material 5 subjected to direct reduction descending through the direct reduction device 7. The temperature of the iron ore oxide material 5 charged into the upper inner portion UP of the direct reduction device 7 is lower than the temperature of the preheated reducing agent 6 introduced into the direct reduction device 7.
[0332] The reduction potential of hydrogen of the reducing agent (reference numeral 6 a ) moving through the upper inner portion is lower than the reduction potential of hydrogen of the reducing agent introduced further downward in the reducing device 7 .
[0333] The reduction apparatus 7 is configured for providing a thermal treatment process for thermally treating the iron ore oxide material 5 subjected to reduction and / or the reduced iron ore material 16 .
[0334] The direct reduction plant 7 comprises a heat treatment zone HZ configured for a heat treatment process for heat treating the reduced iron ore material by exposing it to heat treatment temperatures required to provide heat treatment of the reduced metallic material to obtain densified reduced iron ore material.
[0335] The metal material production arrangement 1 comprises a control circuit 50 electrically coupled to the reducing agent temperature regulating device 18, said reducing agent temperature regulating device 18 being configured to regulate the temperature of the reducing agent 6. The control circuit 50 is adapted to control the temperature of the introduced reducing agent 6 to achieve at least one desired passivation parameter value of the reduced iron ore material 16.
[0336] The upper inner portion UP is configured to provide a chemical reaction at least to some extent by further heating the reducing agent (reference numeral 6a) moving through the upper inner portion UP to achieve a chemical reaction between the iron ore oxide material 5 and the reducing agent 6a moving through the upper inner portion.
[0337] By introducing the reducing agent 6 with a higher temperature into the direct reduction device, it is achieved that the iron ore oxide material 5 that retains thermal energy, reaches the middle part IP and / or the lower inner part LP and undergoes direct reduction and / or heat treatment is not cooled rapidly in the direct reduction device 7, that is, the cooling rate of the iron ore oxide material 5 that undergoes direct reduction and / or heat treatment is reduced.
[0338] Alternatively, the direct reduction apparatus 7 is configured to allow the reduced iron ore material to descend into the lower inner portion LP and / or the intermediate inner portion IP to provide a thermal treatment process.
[0339] Alternatively, the heat treatment of the reduced iron ore material is achieved by introducing a preheated reducing agent 6 , wherein the reduced iron ore material 16 is contacted with the preheated reducing agent 6 .
[0340] The reducing agent temperature regulating device 18 is configured to maintain a desired heat treatment temperature by introducing the preheated reducing agent 6 .
[0341] Alternatively, the step of maintaining the desired heat treatment temperature is provided to such an extent that the introduction of the preheated (hydrogen containing) reducing agent reduces the cooling rate of the reduced iron ore material 16 so as to maintain the desired heat treatment temperature.
[0342] The direct reduction apparatus 7 includes a metal material discharge device c configured to discharge the reduced metal material 16 that has been subjected to heat treatment.
[0343] The control circuit of the metal material production arrangement 1 is connected to the iron ore oxide material supply device unit 3 and is configured to control the temperature of the iron ore oxide material 5 to be charged so that the iron ore oxide material 5 subjected to reduction and / or heat treatment is turned to a predetermined temperature during a predetermined time period long enough to enable the heat treatment process to proceed to provide the desired passivation parameter value of the reduced iron ore material, thereby providing an intermediate product resistant to reoxidation.
[0344] Alternatively, the control circuit 50 is connected to a reducing agent temperature regulating device 18, which is configured to preheat the reducing agent before introducing the reducing agent into the direct reduction device 7, and is configured to control the temperature of the reducing agent so that the iron ore oxide material subjected to reduction and / or heat treatment is turned to a predetermined temperature.
[0345] Alternatively, the control circuit 50 is electrically coupled to the reducing agent temperature regulating device 18, which is configured to regulate the temperature of the hydrogen-containing reducing agent introduced into the reduction device of the metal material production configuration to achieve at least one desired passivation parameter value.
[0346] Alternatively, the control circuit 50 is electrically coupled to the reducing agent temperature regulating device 18 configured to regulate the temperature of the hydrogen-containing reducing agent introduced into the reduction device for the chemical reaction and / or heat treatment process by controlling the temperature of the introduced preheated hydrogen-containing reducing agent 6 .
[0347] The control circuit 50 is coupled to a material temperature regulator 98 which is adapted to control the temperature of the chemical reaction by regulating the thermal energy provided by the iron ore oxide material supplier unit 3 .
[0348] In this way, effective treatment and energy-saving recycling of high-temperature water vapor of the furnace top gas is achieved, wherein the furnace top gas is produced by a chemical reaction supported by the iron ore oxide material of the high-temperature charge, and the high-temperature water vapor is fed to the high-temperature electrolysis unit 17, and thus due to the effective heat recovery of the high-temperature water vapor and due to the high content of high-temperature water vapor in the furnace top gas discharged from the direct reduction device, the high-temperature electrolysis unit can be operated energy efficiently.
[0349] Alternatively, the high temperature electrolysis unit is configured to generate hydrogen, and the iron ore oxide material supplier unit is configured to provide the iron ore oxide material retaining thermal energy.
[0350] Alternatively, the direct reduction apparatus comprises an iron ore oxide material charge inlet means, a reducing agent inlet means configured to introduce a hydrogen-containing reducing agent retaining additional thermal energy.
[0351] Alternatively, the control circuit is configured to control the direct reduction of the iron ore oxide material by adjusting the temperature of the charged iron ore oxide material and the introduced hydrogen-containing reducing agent.
[0352] Alternatively, by the high temperature of the charged iron ore oxide material which retains heat energy, the hydrogen-containing reducing agent which has risen to the upper inner portion is further heated due to the high temperature transfer from the charged iron ore oxide material, thereby providing the (endothermic) chemical reaction, thereby achieving that the high-temperature exhaust gas (top gas) generated in the upper inner portion contains high-temperature water vapor.
[0353] Alternatively, the high temperature steam is transferred to the high temperature electrolysis unit 17 .
[0354] Alternatively, a carbon-containing gas is added to the reducing agent to incorporate carbon into the intermediate product in a carburizing zone (not shown).
[0355] Alternatively, the carburizing zone corresponds to an independent (isolated) carburizing zone configured to prevent the carbonaceous substance from mixing with the reducing agent.
[0356] Alternatively, the carburizing zone constitutes a carburizing space inside the direct reduction device, the carburizing space being configured for reducing the iron ore oxide material, and being configured for carburizing the iron ore oxide material subjected to reduction by mixing a carbonaceous substance with a reducing agent.
[0357] Of course, the present invention is not in any way limited to the preferred examples described above, but many possibilities of modification or combination of the examples described thereof should be obvious to a person skilled in the art without departing from the basic idea of the invention as defined in the appended claims.
Claims
1. A method for reducing a metal oxide material (5) retaining thermal energy to a reduced metal material (16); in - the metal oxide material (5) retaining heat energy is provided by a metal oxide material supply device unit (3) and is loaded into the upper inner part (UP) of the reduction device (7) of the metal material production arrangement (1) via a metal oxide material charging device (a); - electrically coupling the control circuit (50) to a reducing agent temperature regulating device (17) configured to regulate the temperature of the hydrogen-containing reducing agent (6, 6') to be introduced into the intermediate inner part (IP) and / or the lower inner part (LP) of the reducing device (7) via the reducing agent inlet device (b); The method is characterized by the following steps: - using the thermal energy of the metal oxide material (5) to heat or further heat an introduced hydrogen-containing reducing agent (6, 6') to provide a chemical reaction between the hydrogen-containing reducing agent (6, 6') and the metal oxide material (5), thereby reducing the metal oxide material (5) in the upper inner portion (UP); - providing a heat treatment process for heat treating the metal oxide material (5) subjected to reduction and / or heat treating the reduced metal material (16) before discharge from the lower interior portion (LP); as well as - controlling the temperature of the introduced hydrogen-containing reducing agent (6, 6') to adjust the chemical reaction and / or the thermal treatment process to achieve at least one desired passivation parameter value (DPPV) of the reduced metallic material (16).
2. The method according to claim 1, wherein the reducing agent temperature regulating device (17) comprises a reducing agent preheating device (18) suitable for regulating the temperature of the preheated introduced hydrogen-containing reducing agent (6, 6'), and the reducing agent preheating device (18) is electrically connected to the control circuit (50).
3. A method according to claim 1 or 2, wherein the step of controlling the temperature of the introduced hydrogen-containing reducing agent (6, 6') includes adjusting the temperature towards a predetermined temperature to provide sintering of the metal oxide material (5) subjected to reduction and / or heat treatment of the reduced metal material (16) during a predetermined time period to achieve the at least one desired passivation parameter value (DPPV).
4. The method according to any one of claims 1 to 3, wherein the introduced hydrogen-containing reducing agent (6) comprises 90% to 100% hydrogen by volume, preferably 100% hydrogen.
5. A method according to any one of the preceding claims, wherein the control circuit (50) is suitable for roughly setting the temperature of the metal oxide material that retains thermal energy through the metal oxide material supply device unit (3), and is suitable for finely setting the temperature of the introduced hydrogen-containing reducing agent (6) to achieve at least one desired passivation parameter value (DPPV).
6. A method according to any one of the preceding claims, wherein the volume of the introduced hydrogen-containing reducing agent (6, 6') is such that complete reduction of the metal oxide material (5) is achieved, and an excess volume of the hydrogen-containing reducing agent (6, 6') is provided in the reduction device (7) to provide the reduction of the metal oxide material (5).
7. The method according to any one of the preceding claims, wherein the introduced hydrogen-containing reducing agent (6, 6') is introduced into the reduction device (7) via a reducing agent inlet device (b) of the reduction device (7) comprising at least one reducing agent inlet.
8. A metal material production arrangement (1) suitable for reducing a metal oxide material (5) retaining thermal energy into a reduced metal material (16); the metal material production arrangement (1) comprising: A metal oxide material supply device unit (3), the metal oxide material supply device unit (3) being configured to provide the metal oxide material (5) for retaining thermal energy; a metal oxide material charging device (a), the metal oxide material charging device (a) being configured to charge the metal oxide material (5) into the upper inner part (UP) of the reduction device (7); A reducing agent inlet device (b), wherein the reducing agent inlet device (b) is configured to introduce a hydrogen-containing reducing agent (6) into the middle inner part (IP) and / or the lower inner part (LP) of the reducing device (7), thereby heating or further heating the introduced hydrogen-containing reducing agent (6, 6') by utilizing the thermal energy of the metal oxide material (5) to provide a chemical reaction between the hydrogen-containing reducing agent (6, 6') and the metal oxide material (5), so that the hydrogen-containing reducing agent (6, 6') is suitable for reacting with the metal oxide material (5) retaining thermal energy to reduce the metal oxide material (5); characterized in that The reduction device (7) of the metal material production arrangement (1) is configured to provide a heat treatment process for heat treating the metal oxide material (5) subjected to reduction and / or heat treating the reduced metal material (16); and A control circuit (50) electrically coupled to a reducing agent temperature regulating device (17) configured to regulate the temperature of the hydrogen-containing reducing agent (6, 6') is adapted to control the temperature of the introduced hydrogen-containing reducing agent (6, 6') to achieve at least one desired passivation parameter value (DPPV) of the reduced metallic material (16).
9. A metal material production arrangement (1) according to claim 8, wherein the reduction device (7) comprises a passivation parameter detector (PPD) connected to the control circuit (50) and configured to detect an actual passivation parameter value (APPV).
10. The metallic material production arrangement (1) according to claim 8 or 9, wherein the introduced hydrogen-containing reducing agent (6, 6') comprises 90 to 100% hydrogen by volume, preferably 100% hydrogen.
11. The metal material production arrangement (1) according to any one of claims 8 to 10, wherein the control circuit (50) is configured to control the temperature of the metal oxide material (5) to be charged into the direct reduction device (7).
12. A data program (P) programmed to cause a metal material production arrangement (1) according to any one of claims 8 to 11 to perform a method according to any one of claims 1 to 7, wherein the data program (P) comprises a program code readable on a computer of a control circuit (50) to provide the following steps: - using the thermal energy of the metal oxide material (5) to heat or further heat the introduced hydrogen-containing reducing agent (6, 6') to provide a chemical reaction between the hydrogen-containing reducing agent (6, 6') and the metal oxide material (5), thereby reducing the metal oxide material (5) in the upper inner portion (UP); - providing a heat treatment process for heat treating the metal oxide material (5) subjected to reduction and / or heat treating the reduced metal material (16) before discharge from the lower interior portion (LP); and - controlling the temperature of the introduced hydrogen-containing reducing agent (6, 6') to adjust the chemical reaction and / or the thermal treatment process to achieve at least one desired passivation parameter value (DPPV) of the reduced metallic material (16).
13. A data medium configured for storing a data program (P) according to claim 12, wherein the data medium comprises a computer-readable program code for executing a method according to any one of claims 1 to 7.
14. A product produced by the method according to claims 1 to 7, wherein the reduced metal material (16) consists of reduced iron ore particles which are combined with each other to form pellets of heat-treated and / or heat-hardened and / or passivated reduced iron ore material in the form of iron droplets.