Method for manufacturing hot-dip galvanized steel sheet and facility for manufacturing hot-dip galvanized steel sheet

By controlling the plating solution discharge rate and electrode plate design, the problem of non-coating caused by the oxidation and enrichment of Si and Mn during the hot-dip galvanizing process of high-tensile steel plates was solved, achieving uniform coating and high-quality hot-dip coating, thus improving production efficiency and coating quality.

CN119032198APending Publication Date: 2024-11-26JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034287.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-18
Filing Date
2023-01-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the hot-dip galvanizing process of manufacturing high-tensile steel sheets, easily oxidizable elements such as Si and Mn accumulate on the surface of the steel sheet, leading to reduced wettability and the formation of oxides. This results in problems such as no coating or poor coating adhesion, which is particularly pronounced on irregularly shaped steel sheets.

Method used

By controlling the plating solution discharge rate to less than 50% in the electroplating process and forming an iron-based film in the gap between the electrode plate and the steel plate, combined with appropriate electroplating and hot-dip plating processes, the uniform distribution of the plating solution and the straightening force are ensured, thus avoiding non-plating and defects.

Benefits of technology

It enables uniform coating on irregularly shaped high-tensile steel plates, avoiding uncoated areas and defect picking, resulting in a beautiful hot-dip coating and improving production efficiency and coating quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032198A_ABST
    Figure CN119032198A_ABST
Patent Text Reader

Abstract

Provided is a method that makes it possible to produce a steel sheet having a beautiful plating layer without quality defects such as non-plating and pick-up due to irregularity of the shape of the steel sheet when hot-dip galvanizing or further alloying treatment is performed on a steel sheet containing an oxidizable element, in particular, a high-tension steel sheet. Provided is a method for producing a hot-dip galvanized steel sheet, which comprises: a plating step in which an iron-based coating film is formed on the surface of a steel sheet by supplying an iron-based plating solution to the steel sheet in a gap between the steel sheet and an electrode plate disposed facing the steel sheet, while energizing the steel sheet with the electrode plate as an anode and the steel sheet as a cathode; an annealing step for heating the steel sheet subjected to the electroplating step; and a hot-dip plating step in which hot-dip galvanizing is performed on the steel sheet that has undergone the annealing step, and in the electroplating step, the plating solution discharge rate, which is the ratio of the flow rate of the plating solution flowing out to the back surface side of the electrode plate that does not face the steel sheet to the flow rate of the plating solution supplied to the steel sheet, is less than 50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a hot-dip galvanized steel sheet, and in particular to a method for manufacturing a hot-dip galvanized steel sheet using a high-tensile steel sheet as a base material and a manufacturing device for the hot-dip galvanized steel sheet. Background Art

[0002] In recent years, the demand for high-tensile steel sheets (high-strength steel materials) that can be used for lightweight structures, etc., has been increasing in the fields of automobiles, home appliances, building materials, etc. As high-strength steel materials, for example, steel sheets having good hole expandability by containing Si in steel and steel sheets having improved ductility by containing Si, Al, and Mn are known.

[0003] However, when a hot-dip galvanized steel sheet or an alloyed hot-dip galvanized steel sheet is produced using a high-tensile steel sheet containing a large amount (particularly 0.2 mass % or more) of Si and Mn, for example, having a tensile strength of 590 MPa or more as a base material, the following problems arise.

[0004] That is, the hot-dip galvanized steel sheet is manufactured by heating and annealing the base steel sheet at a temperature of about 600 to 900°C in a reducing atmosphere or a non-oxidizing atmosphere, and then hot-dip galvanizing the steel sheet. In addition, the alloyed hot-dip galvanized steel sheet is manufactured by heating and alloying the galvanized steel sheet after the above-mentioned hot-dip galvanizing treatment. Here, Si and Mn in the steel are easily oxidizable elements, and they will be selectively oxidized even in the commonly used reducing atmosphere or non-oxidizing atmosphere, enriched on the surface of the steel sheet, and form oxides. The oxides will reduce the wettability of the molten zinc during the plating treatment, resulting in non-plating without plating. Therefore, as the concentration of Si and Mn in the steel increases, the wettability decreases sharply, and non-plating occurs frequently. In addition, even if non-plating is not achieved, there is also the problem of poor plating adhesion. Furthermore, if Si and Mn in the steel are selectively oxidized and enriched on the surface of the steel sheet, a significant alloying delay will occur in the alloying process after hot-dip galvanizing, and the phenomenon of significantly hindering productivity becomes a problem.

[0005] To solve this problem, Patent Document 1 discloses a method with low manufacturing cost, wherein a 0.2 to 2 g / m 2 The steel is plated with Fe, and then the heat treatment in the direct fire furnace (DFF) and the radiation heating furnace (RTF) is adjusted to the specified conditions, so that Si, Mn or Al contained in the steel, which are difficult-to-plate elements, diffuse on the surface and inhibit the formation of oxides, thereby preventing the non-plating phenomenon and ensuring excellent plating surface quality, plating adhesion and high strength.

[0006] In addition, Patent Document 2 discloses a method in which a predetermined grain boundary oxidation depth is formed on the surface of a steel sheet in a hot rolling process, and then a 3 g / m 2After the above Fe plating, alloying hot-dip galvanizing treatment is performed to produce a hot-dip galvanized steel sheet excellent in spot weldability.

[0007] Furthermore, as a method for producing a plated steel sheet at a high current density, Patent Document 3 discloses spraying a plating solution from a plurality of through holes provided in an electrode toward a space between a steel sheet and an electrode, and discharging the plating solution from the through holes of the electrode.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: WO2013 / 100615

[0011] Patent Document 2: Japanese Patent Application Publication No. 2008-231493

[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 2005-272999 Summary of the invention

[0013] Patent Document 1 does not describe the specific equipment structure of the Fe plating process. However, when using a general horizontal electroplating tank or a vertical electroplating tank, for example, in the case of a high-strength steel plate with a tensile strength of 590 MPa or more, the steel plate has a poor shape after cold rolling. If the plate is passed directly in the electroplating process, a contact failure with the electrode will occur. In addition, even if the above-mentioned contact does not occur, the distance between the electrode and the steel plate will also change. Therefore, the plating unit area weight recorded in the document 1 is 0.2 to 2.0 g / m 2 The target Fe plating thickness will fluctuate greatly. In this way, in the subsequent annealing process, Si and Mn are partially concentrated on the surface, and non-plating defects and pickup defects are generated, so stable production is achieved.

[0014] It is known that in the method described in Patent Document 2, if Fe plating is performed to such an extent that Si and Mn are not partially concentrated on the surface during the annealing process, the weight per unit area must be more than 10 g / m 2 , the equipment length becomes longer, and a significant cost increase becomes a problem. It should be noted that it is also considered to improve the shape of the steel plate through a straightening process and a pre-annealing process, but a significant cost increase is still a problem.

[0015] In the plating electrode corresponding to the high current density described in Patent Document 3, in order to avoid the generation of a large amount of electrolytic gas at high current density and the reduction of electrolytic efficiency, efforts are made to remove bubbles (electrolytic gas) through the gap between the hole 9 and the nozzle 8a and the plating solution outlet 11, thereby improving the removal of bubbles (electrolytic gas), that is, gas release. On the other hand, improving the gas release also means that the jet pressure of the plating solution is not easy to accumulate between the electrode and the steel plate, especially for irregularly shaped steel plates, it is difficult to make the plating adhesion uniform, which needs to be improved.

[0016] The present invention has been accomplished in view of the above-mentioned problems, and an object thereof is to provide a method capable of manufacturing a steel sheet having a beautiful coating layer without quality defects such as non-coating and pickup caused by irregular shapes of the steel sheet, for example, when a steel sheet containing easily oxidizable elements such as Si and Mn, especially a high-tensile steel sheet, is subjected to hot-dip galvanizing or further alloying treatment.

[0017] The gist of the present invention for solving the above-mentioned problems is as follows.

[0018] 1. A method for manufacturing a hot-dip galvanized steel sheet, which is a method for manufacturing a hot-dip galvanized steel sheet through the following steps:

[0019] The electroplating step includes supplying an iron-based plating solution to the steel plate in a gap between the continuously moving steel plate and an electrode plate disposed opposite to the steel plate, and applying electricity to the electrode plate as an anode and the steel plate as a cathode to perform electroplating to form an iron-based film on the surface of the steel plate;

[0020] An annealing process is performed to heat the steel sheet after the electroplating process; and

[0021] The hot-dip galvanizing step is to perform hot-dip galvanizing on the steel sheet after the annealing step.

[0022] In the electroplating step, the ratio of the flow rate of the plating solution flowing out to the back side of the electrode plate not facing the steel plate to the flow rate of the plating solution supplied to the steel plate, that is, the plating solution discharge rate, is less than 50%.

[0023] 2. The method for producing a hot-dip galvanized steel sheet according to item 1 above, wherein the adhesion amount of the iron-based film is 2.0 g / m 2 above.

[0024] 3. The method for producing a hot-dip galvanized steel sheet according to 1 or 2 above, wherein the plating solution discharge rate is 10% or less.

[0025] 4. The method for producing a hot-dip galvanized steel sheet according to any one of 1 to 3 above, wherein the plating solution flow rate Q (m 3 / minute) satisfies the following formula (1).

[0026] Q≥60WLH····(1)

[0027] Here, W is the width of the steel plate (m), L is the length of the electrode plate in the long side direction (m), and H is the distance between the electrode plate and the steel plate (m).

[0028] 5. The method for producing a hot-dip galvanized steel sheet according to any one of 1 to 4 above, wherein the steel sheet has a component composition containing, by mass%, 0.3% or less of C and 1.0 to 6.0% in total of any one or more of Si and Mn.

[0029] 6. A manufacturing equipment for hot-dip galvanized steel sheet, comprising:

[0030] Electroplating device, forming an iron coating on the steel plate continuously moving on the line;

[0031] An annealing device for heating the steel sheet after the electroplating device; and

[0032] A hot-dip galvanizing device is used to perform hot-dip galvanizing on the steel sheet that has passed through the annealing device.

[0033] The electroplating device comprises electrode plates relatively arranged along the travel line of the steel plate and a jet nozzle supplying an iron-based plating solution from the electrode plate side to the travel line, the electrode plate being an anode and the steel plate being a cathode, and the ratio of the flow rate of the plating solution flowing out to the back side of the electrode plate not opposite to the steel plate to the flow rate of the plating solution supplied from the jet nozzle, that is, the plating solution discharge rate, is less than 50%.

[0034] 7. The manufacturing equipment of the hot-dip galvanized steel sheet according to the above-mentioned 6, wherein the above-mentioned electrode plate has at least one through hole extending in a direction intersecting with the above-mentioned travel line and penetrating the electrode plate, and the above-mentioned injection nozzle is arranged in at least one of the above-mentioned through holes.

[0035] 8. A manufacturing device for hot-dip galvanized steel sheets according to 6 or 7 above, wherein a back plate and a jet manifold are provided in sequence on the back side of the electrode plate from the traveling line side, a plurality of jet nozzles extending through the back plate and the electrode plate are connected to the jet manifold, the back plate is connected to the back side of the electrode plate via an electrode connecting portion, and an insulator is arranged in the space between the back plate and the electrode plate generated by the electrode connecting portion.

[0036] 9. The manufacturing equipment of the hot-dip galvanized steel sheet according to the above 8, wherein the equipment is composed of one or more plating tanks, wherein the plating tank is formed by seamlessly combining the above electrode plates as a collection of multiple sheets to one of the back plates.

[0037] 10. The hot-dip galvanized steel sheet manufacturing equipment according to 9 above, wherein in each of the coating tanks, the jet header is divided into a plurality of portions at positions that do not interfere with the electrode connecting portion.

[0038] 11. A manufacturing device for hot-dip galvanized steel sheets according to any one of 8 to 10 above, wherein the jet manifold has a plating liquid piping for supplying plating liquid into the jet manifold, and a ratio Ak / An of a cross-sectional area Ak of ​​the plating liquid piping to a total cross-sectional area An of injection ports of injection nozzles connected to the jet manifold is greater than 2.5.

[0039] 12. The hot-dip galvanized steel sheet manufacturing equipment according to any one of 6 to 11 above, wherein the electroplating device and the annealing device are located on the same line.

[0040] 13. The manufacturing equipment of the hot-dip galvanized steel sheet according to any one of 6 to 11 above, wherein the electroplating device and the annealing device are located on different lines.

[0041] According to the method for producing a hot-dip galvanized steel sheet of the present invention, even when hot-dip galvanizing is performed on a high-tensile steel sheet that is prone to irregular shapes, for example, a steel sheet having a beautiful hot-dip galvanized layer without quality defects such as non-plating and pickup can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is a schematic diagram showing the structure of the manufacturing equipment of the present invention which is provided with an in-line electroplating device.

[0043] Figure 2 This is a schematic diagram showing the configuration of the manufacturing facility of the present invention including plating devices on different lines.

[0044] Figure 3 This is a schematic diagram of a cross section of the electroplating bath of the present invention as viewed from the side.

[0045] Figure 4 It is an enlarged view of the periphery of the circular tube nozzle of the electroplating pool of the present invention.

[0046] Figure 5 This is a schematic diagram of a conventional horizontal flow cell device.

[0047] Figure 6 This is a schematic diagram of the steel plate viewed from the conveying direction. DETAILED DESCRIPTION

[0048] Hereinafter, the method for producing a hot-dip galvanized steel sheet according to the present invention will be described in detail with reference to the drawings.

[0049] The method for manufacturing a hot-dip galvanized steel sheet of the present invention is a method for manufacturing a hot-dip galvanized steel sheet through the following steps: an electroplating step, in which an iron-based plating solution is supplied to the steel sheet in a gap between a continuously moving steel sheet and an electrode plate arranged opposite to the steel sheet, while the electrode plate is used as an anode and the steel sheet is used as a cathode to conduct electroplating, thereby forming an iron-based film on the surface of the steel sheet; an annealing step, in which the steel sheet that has undergone the electroplating step is subjected to a heating treatment; and a hot-dip galvanizing step, in which the steel sheet that has undergone the annealing step is subjected to hot-dip galvanizing. Furthermore, the method is characterized in that, in the electroplating step, the ratio of the flow rate of the plating solution flowing out to the back side of the electrode plate that is not opposite to the steel sheet to the flow rate of the plating solution supplied to the steel sheet, i.e., the plating solution discharge rate, is less than 50%.

[0050] First, refer to Figure 1 One embodiment of a hot-dip galvanized steel sheet manufacturing facility used in the method for manufacturing a hot-dip galvanized steel sheet of the present invention will be described. Figure 1 The embodiment shown is a continuous hot-dip galvanized steel sheet manufacturing equipment having an electroplating device that performs an electroplating process online. Specifically, for example, from the upstream side of the running line of the steel sheet P as a high-tension steel strip, there are an unwinder 51, a coil joint device 52, an inlet looper 53, a degreasing device 54, a pickling device 55, an electroplating device 56, a water washing device 57, an annealing device 58, a hot-dip galvanizing device 59, an alloying treatment device 60 (used when manufacturing alloyed galvanized steel sheets), a temper rolling device 61, a post-processing device 62, an outlet looper 63, and an inspection device 64 in this order.

[0051] in addition, Figure 2 Another embodiment is shown in which the electroplating device is a line different from the hot-dip galvanizing device. That is, Fe plating is performed in a device line including an uncoiler 51, a coil splicer 52, an inlet looper 53, a degreasing device 54, a pickling device 55, an electroplating device 56, a water washing device 57, an outlet looper 63, and an inspection device 64. Then, galvanizing is performed in a conventional continuous hot-dip galvanizing line including an uncoiler 51, a coil splicer 52, an inlet looper 53, a degreasing device 54, an annealing device 58, a hot-dip galvanizing device 59, an alloying treatment device 60, a temper rolling device 61, a post-treatment device 62, an outlet looper 63, and an inspection device 64.

[0052] The former continuous hot-dip galvanized steel sheet manufacturing equipment ( Figure 1 ) and the latter's continuous hot-dip galvanized steel sheet manufacturing equipment ( Figure 2 ) can be any form of a direct fire heating furnace (DFF) + radiation heating furnace (RTF), an IH heating furnace (IHF) + radiation heating furnace and a full-area radiation heating furnace.

[0053] Continuous hot dip galvanized steel sheet manufacturing equipment ( Figure 1 ) is characterized by being able to complete the hot-dip galvanizing process in one line, so the production efficiency is very high. On the other hand, continuous hot-dip galvanized steel sheet manufacturing equipment ( Figure 2 ) is a two-line manufacturing process, so it is similar to the continuous hot-dip galvanized steel sheet manufacturing equipment ( Figure 1 ) is slightly lower in production efficiency. However, since the electroplating Fe device can be used for multiple hot-dip galvanizing lines that do not usually have Fe plating devices, it has the advantages of high production efficiency as a single Fe plating device and the initial investment is also suppressed to a minimum.

[0054] The amount of Fe plated in the electroplating device 56 is preferably 2.0 g / m2 depending on the added elements in the steel and the length of the annealing device. 2 When less than 2.0g / m 2 When the amount of Fe plating is 2.0 g / m 2 The above is to avoid non-plating defects and pick-up defects. On the other hand, the upper limit of the Fe plating amount is not particularly limited, but when it exceeds 8.0 g / m 2 When the running cost becomes too high, the preferred 2 .

[0055] As long as the electroplating of Fe is iron-based plating, there is no particular restriction on its component system. For example, it can be any system of pure Fe, Fe-B, Fe-C, Fe-P, Fe-N or Fe-O, and pure Fe is particularly preferred. As a plating bath composition of pure Fe, pure Fe can be exemplified: iron content is 55 to 65 g / L and sodium is 5 to 7 g / L, and pH is 2.0 to 2.2.

[0056] The Fe electroplating bath may contain Fe ions and at least one element selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V and Co. The total content of these elements in the Fe electroplating bath is preferably such that the total content of these elements in the Fe electroplating layer is 10 mass % or less.

[0057] Next, refer to Figure 3 and Figure 4 The Fe electroplating device 56 of the present invention will be described in detail.

[0058] Figure 31 shows a horizontal electroplating device used in one embodiment of the present invention. In the electroplating device, a steel plate P is moved horizontally on a moving line, and a pair of electrode plates 10 are arranged opposite to each other along the continuously moving steel plate P. The electrode plates 10 are preferably insoluble. In addition, a conductor roller 20 and a support roller 21 for electrifying the steel plate P are respectively arranged on the upstream side and the downstream side of the electrode plate 10 in the moving direction of the steel plate P.

[0059] Here, the conductor roller 20 may be a roller having a copper plating layer or a nickel plating layer having good conductivity as a base on the roller circumference. In addition, the material and thickness of the electrode plate 10 are not particularly limited, but titanium coated with iridium oxide is preferably used as the material, and the thickness is preferably 5 to 100 mm. There is no particular limitation on the interval between the steel plate P and the electrode plate 10, but it is preferably in the range of 2 to 20 mm.

[0060] A back plate 12 is arranged on the back side of each electrode plate 10 (the side of the electrode plate opposite to the steel plate P) via an electrode connecting portion 11, and the current output from the rectifier (not shown) is input into the back plate 12 through a current-carrying rod 16. A nozzle manifold 14 for supplying a plating solution 30 to the steel plate P is arranged on the back side of the back plate 12. In order to make the current distribution uniform, the back plate 12 is preferably formed as an integral body in one pool. On the other hand, considering the replacement operation, etc., it is preferred to appropriately divide the electrode plate 10 opposite to the steel plate in the width direction and the long side direction.

[0061] The nozzle manifold 14 has a plurality of round tube nozzles 15, and the plurality of round tube nozzles 15 are connected through a plurality of through holes 10a (see Figure 4 ) extends from the back plate 12 side to the electrode plate 10 side and stays in the through hole 10a of the electrode plate 10 and is formed of an insulating material. Here, it is preferred to form the round tube nozzle 15 with an insulating material because, by making the entire plating solution supply system with insulating materials, it is effective to avoid unintentional electrolysis in the plating solution flow path or to avoid component damage caused by sparks between the round tube nozzle 15 and the electrode plate 10.

[0062] The circular nozzle 15 is preferably arranged with its axis perpendicular to the surface of the steel sheet P. The plating solution 30 is supplied from the nozzle manifold 14 to the circular nozzle 15 and is sprayed toward the steel sheet P from the spray port at the front end of the circular nozzle 15 .

[0063] In this way, while the steel plate P is moved in the horizontal direction, the plating solution 30 is supplied to the steel plate P in the gap (gap) between the steel plate P and the electrode plate 10. The electrode plate 10 is used as the anode and the steel plate P is used as the cathode. Electricity is passed between the plated surface of the steel plate P and the electrode plate 10 to electroplate the steel plate.

[0064] Figure 4A nozzle manifold 14 and its surroundings in the electroplating device 56 are shown in an enlarged manner. The front end of the round tube nozzle 15 is long enough to stay in the through hole 10a so as not to protrude further toward the steel plate P side than the surface of the electrode plate 10 on the steel plate P side. Furthermore, in order to prevent the plating solution 30 from flowing out from the through hole 10a to the back side of the electrode plate 10, it is necessary to block the space formed between the electrode plate 10 and the back plate 12 due to the presence of the electrode connecting portion 11 with an insulator 13 made of resin, for example.

[0065] That is, in order to prevent the plating solution from flowing out from the steel plate P side to between the electrode plate 10 and the back plate 12, at least the space formed between the electrode plate 10 and the back plate 12 needs to be filled with an insulator 13. It should be noted that if there is a gap between the inner wall of the through hole 10a of the electrode plate 10 and the outer peripheral surface of the circular tube nozzle 15, it is preferably filled with an insulator 13. Here, if the above-mentioned gap in the through hole 10a can be completely filled without any leakage, it is not necessary to fill the gap between the electrode plate 10 and the back plate 12 with an insulator 13. However, it is difficult in terms of technology or cost to completely block the above-mentioned gap in all the multiple through holes 10a of the electrode plate 10 with an insulator. In view of this, it is effective to more simply use an insulator 13 to block the space formed between the electrode plate 10 and the back plate 12.

[0066] In order to make the current flow evenly from the back plate 12 to the multiple electrode plates 10, it is preferred to fasten the back plate 12 and the electrode connecting part 11 with bolts (not shown) after smoothly processing the connecting surface of the back plate 12 and the electrode connecting part 11. The structure with the electrode connecting part 11 is extremely effective in assembling the present device. That is, although the back plate 12 and the electrode plate 10 can be fastened without the electrode connecting part 11 in structure, the back plate 12 and the electrode plate 10 are only tightly fitted around the fastening bolts. In this case, if a small gap is generated at a position slightly away from the fastening bolts, sparks will be generated at the position of the gap when power is turned on, and the back plate 12 and the electrode plate 10 will be damaged. Therefore, this structure without the electrode connecting part 11 is not ideal.

[0067] Furthermore, as described above, by filling the gap between the back plate 12 and the electrode plate 10 with the insulator 13, uneven current flow between the back plate 12 and the electrode plate 10 can be avoided. In the case where the member filling the gap between the back plate 12 and the electrode plate 10 is not an insulator, a current flow portion is formed except for the electrode connecting portion 11, and when the electrode plate is viewed from the steel plate, a non-uniform current distribution is obtained.

[0068] If the above structure is made, the plating solution 30 does not flow out from the through hole 10a to the back side of the electrode plate 10, so the jet of the plating solution from the round tube nozzle 15 is concentrated in the gap between the electrode plates 10, and the spray pressure of the plating solution can be applied to the steel plate P passing through the gap without any residue. As a result, the straightening force acts on the steel plate P from both the upper and lower sides, and the steel plate with poor shape can be flattened while passing the plate and energized. Therefore, even if the cold-rolled material is passed without pre-straightening, it will not be affected by the shape disturbance during plating as described above, so it is possible to achieve a uniform plating adhesion over the entire width, and the surface enrichment of Si and Mn can be suppressed with a minimum Fe plating adhesion.

[0069] Here, in Figure 3 In one section of electroplating (three pools: electrode size of one pool: width 1.5m×length in the through-plate direction 1m), for the case where the electrode plate with discharge holes described in the above-mentioned patent document 3 is used and for the case where the electrode plate of the present invention is used Figure 4 In the case of the electrode plate shown in FIG. 1 , the pressure of the plating solution jet from the round nozzle on the steel plate P was investigated. Figure 3 In one section of the electroplating shown in the figure, 120 inner diameter electrodes are arranged on one side of a pair of electrode plates, 10 in the electrode width direction and 12 in the plate through direction. The total flow rate of the round tube nozzle is 2.5m 3 The plating solution was sprayed into the gap of 20 mm between the electrode and the steel plate at a rate of 1.50 / min. The pressure applied to the steel plate accompanying the spraying was measured. As a result, in the electrode provided with a discharge hole described in Patent Document 3, only the point where the plating solution jet collided with the nozzle became the point where the pressure on the steel plate acted, and the total pressure acting on one side of the steel plate was 290N (1.53N per nozzle). In contrast, Figure 4 In the electrode, the plating solution is discharged only from the inlet and outlet sides of the steel plate P of the electrode plate, so the pressure loss of the plating solution flowing between the electrode plate and the steel plate is applied to the entire electrode surface (the effective area where the steel plate pressing force actually acts is about 50% of the electrode plate area). As a result, the form of pressing the steel plate is realized, and the steel plate pressing force also reaches 3500N, which is more than 12 times.

[0070] As described above, according to the present invention, the straightening force acts on the steel sheet from top to bottom in the coating bath, and the steel sheet with a poor shape can be flattened while the steel sheet is being passed through and current is being supplied.

[0071] In order to obtain the above effects, it is important to make the above-mentioned plating solution discharge rate during electroplating less than 50%. That is, when the plating solution discharge rate is 50% or more, the flow rate of the plating solution flowing between the electrode plate and the steel plate is reduced, so the pressure on the steel plate is reduced. It is preferably less than 10%. It should be noted that the above-mentioned plating solution discharge rate is less than 50% by the above-mentioned structure of the Fe plating device 56 as described above.

[0072] On the other hand, for bubbles (electrolytic gas) generated during plating, it is preferable to set the plating solution flow rate Q (m 3 / min) satisfies the following formula (1). It was found that bubbles are sufficiently discharged by satisfying the formula (1).

[0073] Q≥60WLH····(1)

[0074] Here, W is the width of the steel plate (m), L is the length of the long side of the electrode plate (m), and H is the distance between the electrode plate and the steel plate (m). It should be noted that the distance between the electrode plate and the steel plate refers to the shortest distance between the electrode plate and the steel plate in a direction perpendicular to the traveling direction of the steel plate.

[0075] That is, 60WLH represents a volume 60 times the volume of the space between the steel plate and the electrode plate. If the plating solution flow rate Q is above 60WLH, the plating solution between the steel plate and the electrode plate can be replaced within 1 second, thereby avoiding the reduction in conductivity caused by the electrolytic gas.

[0076] In addition, in Figure 4 In the split jet manifold 14 shown, the ratio Ak / An of the cross-sectional area Ak of ​​the plating liquid pipe 14a supplying the plating liquid 30 to the jet manifold 14 and the total cross-sectional area An of the injection port of the round tube nozzle 15 provided in the jet manifold 14 is preferably 2.5 or more. That is, if Ak / An is less than 2.5, the pressure distribution in the jet manifold tends to become uneven. As a result, there is a risk that the deviation of the injection speed from the round tube nozzle 15 becomes larger, and sometimes there is a problem of uneven adhesion. It should be noted that if Ak / An exceeds 12, a rapid reduction in the cross-sectional area of ​​the flow path from the jet manifold to the round tube nozzle is formed, the pressure loss becomes larger, and the plating liquid feeding pump requires too much capacity. Therefore, from the viewpoint of economy, it is preferably less than 12.

[0077] It should be noted that the cross-sectional areas Ak and An are the minimum areas of the inner cross-sections of the various tubes perpendicular to the axial direction. In addition, in each jet manifold 14, when there are multiple plating solution pipes and circular nozzles, the total cross-sectional areas of the tubes are Ak and An, respectively. Figure 4 In the jet manifold 14 shown, Ak is the cross-sectional area of ​​the plating solution piping 14 a , and An is the total cross-sectional area of ​​three cross-sectional areas of the jet ports of the circular tube nozzle 15 .

[0078] It should be noted that the objects of the above-mentioned Fe electroplating and zinc plating are not particularly limited as long as they are steel plates. As the plating object, for example, in addition to ordinary steel, stainless steel and other steel plates, aluminum plates and the like are the objects. The present invention is effective when applied to steel plates, and is particularly advantageous when applied to high-tensile steel plates. By the way, as a high-tensile steel plate, a steel plate having the component composition shown below is suitable. It should be noted that, unless otherwise specified, the "%" in the following component composition means mass %.

[0079] C: 0.025~0.300%

[0080] C tends to improve workability by forming a retained austenite layer, a martensite phase, etc. as the steel structure, so it is preferably contained at 0.025% or more. On the other hand, if it exceeds 0.300%, weldability deteriorates, so the C content is preferably 0.300% or less.

[0081] Si: 0.2-2.5%

[0082] Si is an element effective in strengthening steel to obtain good material quality, and is added to high-tensile steel sheets at a content of 0.2% or more. When Si is less than 0.2%, expensive alloying elements are required to obtain high strength. On the other hand, when Si exceeds 2.5%, the formation of oxide film during oxidation treatment is inhibited. In addition, the alloying temperature also becomes high, making it difficult to obtain the desired mechanical properties. Therefore, the amount of Si is preferably less than 2.5%.

[0083] Mn: 1.5~3.5%

[0084] Mn is an element effective in increasing the strength of steel. In order to ensure a tensile strength of 590 MPa or more, it is preferably contained at least 1.5%. On the other hand, if it exceeds 3.5%, it is sometimes difficult to ensure weldability, plating adhesion, and strength-ductility balance. Therefore, the Mn content is preferably 1.5 to 3.5%.

[0085] In addition to the above components, the following elements may be contained.

[0086] Al: 0.001~1.000%

[0087] Al is added for the purpose of deoxidation of molten steel, but when its content is less than 0.001%, its purpose cannot be achieved. On the other hand, if it exceeds 1.000%, Al forms oxides on the surface, and the plating appearance (surface appearance) deteriorates. Therefore, the Al content can be 0.001% to 1.000%.

[0088] P: 0.10% or less

[0089] P is one of the elements that are inevitably contained. In order to make it less than 0.005%, there is a concern about the increase in cost, so it is preferably 0.005% or more. On the other hand, the slab manufacturability deteriorates with the increase of P. Furthermore, the inclusion of P inhibits the alloying reaction and causes uneven plating. In order to suppress these, it is necessary to make the content 0.10% or less. Therefore, the P amount can be 0.10% or less. Preferably, it is 0.05% or less.

[0090] S: 0.01% or less

[0091] S is an element that is inevitably contained in the steelmaking process. However, if it is contained in a large amount, weldability deteriorates. Therefore, S may be 0.01% or less.

[0092] When the above components are contained, the remainder is Fe and inevitable impurities.

[0093] Furthermore, one or more elements selected from the group consisting of B: 0.001-0.005%, Nb: 0.005-0.050%, Ti: 0.005-0.080%, Cr: 0.001-1.000%, Mo: 0.05-1.00%, Cu: 0.05-1.00%, Ni: 0.05-1.00%, and Sb: 0.001-0.200% may be contained as needed.

[0094] When these elements are added, appropriate contents and reasons for their limitations are as follows.

[0095] B: 0.001~0.005%

[0096] When B is 0.001% or more, a quenching acceleration effect can be obtained. On the other hand, when it exceeds 0.005%, the chemical treatment property deteriorates. Therefore, when B is contained, the amount of B can be 0.001% to 0.005%.

[0097] Nb: 0.005~0.050%

[0098] When Nb is 0.005% or more, the effect of strength adjustment (strength improvement) can be obtained. On the other hand, when it exceeds 0.05%, it leads to an increase in cost. Therefore, when Nb is contained, the amount can be 0.005% to 0.05%.

[0099] Ti: 0.005~0.080%

[0100] When Ti is 0.005% or more, the effect of strength adjustment (strength improvement) can be obtained. On the other hand, when it exceeds 0.080%, it leads to deterioration of chemical treatment properties. Therefore, when Ti is contained, the amount can be 0.005% to 0.080%.

[0101] Cr: 0.001~1.000%

[0102] When Cr is 0.001% or more, a hardenability effect can be obtained. On the other hand, when it exceeds 1.000%, Cr is concentrated on the surface, so weldability deteriorates. Therefore, when Cr is contained, the amount can be 0.001% to 1.000%.

[0103] Mo: 0.05~1.00%

[0104] When Mo is 0.05% or more, the effect of strength adjustment (strength improvement) can be obtained. On the other hand, when it exceeds 1.00%, it leads to an increase in cost. Therefore, when Mo is contained, the amount may be 0.05% to 1.00%.

[0105] Cu: 0.05~1.00%

[0106] When Cu is 0.05% or more, the effect of promoting the formation of the residual γ phase can be obtained. On the other hand, when Cu exceeds 1.00%, it leads to an increase in cost. Therefore, when Cu is contained, the amount may be 0.05% to 1.00%.

[0107] Ni: 0.05~1.00%

[0108] When Ni is 0.05% or more, the effect of promoting the formation of the residual γ phase can be obtained. On the other hand, when Ni exceeds 1.00%, it leads to an increase in cost. Therefore, when Ni is contained, the amount may be 0.05% to 1.00%.

[0109] Sb: 0.001~0.200%

[0110] Sb can be contained from the viewpoint of suppressing nitridation and oxidation of the steel sheet surface or decarburization of the tens of micrometers of the steel sheet surface caused by oxidation. By suppressing nitridation and oxidation, the amount of martensite generated on the steel sheet surface is prevented from decreasing, and fatigue properties and surface quality are improved. Such an effect can be obtained when the content is 0.001% or more. On the other hand, if it exceeds 0.200%, toughness deteriorates. Therefore, when contained, the amount of Sb can be 0.001% to 0.200%.

[0111] Example

[0112] The following describes embodiments of the present invention. However, the technical scope of the present invention is not limited to the following embodiments.

[0113] Will use Figure 1 or 2, and use in these manufacturing equipment Figure 3 The case of the electroplating device (one pool) shown in FIG. 1 is used as an example of the present invention. That is, in the plating pool constituting the electroplating device, the electrode length in the long side direction in one pool is 2m, and the pool is connected to two pools. In addition, as a comparative example, a general horizontal flow pool ( Figure 5 ) form, a horizontal porous plating pool form with a plating solution discharge hole (according to Patent Document 3 Figure 1 records).

[0114] Here, Figure 5 In the illustrated horizontal flow cell type Fe electroplating apparatus, a passage 43 divided by electrode plates 42a and 42b is formed between two pairs of rollers of a conductor roller 40 and a support roller 41. When a steel plate P passes through the passage 43, a plating solution 30 is supplied from a nozzle manifold 44 along the passage 43 between the steel plate P and the electrode plates 42a and 42b, and the electrode plates 42a and 42b are used as anodes and the steel plate P is used as a cathode, and electricity is passed between the surface of the steel plate P and the electrode plates 42a and 42b, thereby electroplating Fe on the steel plate P.

[0115] The shape of the steel sheet before passing through the electroplating device is measured using a laser shape measuring device installed on the upstream side of the initial plating tank of the electroplating device. Figure 6 Specifically, if the steel plate P is viewed from the traveling direction, Figure 6 As shown in FIG. 1 , if the steel sheet P is warped, when the steel sheet P is placed on a flat plate, a portion Pb having a height higher than the placement portion Pa is formed in the width direction of the steel sheet P. In the steel sheet P before Fe electroplating, the difference in height between the highest portion Pb and the lowest placement portion Pa is measured as the warpage amount.

[0116] Using each example of the hot-dip galvanized steel sheet manufacturing equipment described above, a steel sheet with a thickness of 1.4 mm and a width of 1200 mm was fed at a sheet feeding speed of 1.5 m / s to perform Fe electroplating and hot-dip galvanizing. The component compositions of the steel sheets are shown in Table 1.

[0117] [Table 1]

[0118] (quality%)

[0119] C Si Mn P S 0.12 0.5 2.5 0.01 0.001

[0120] [Fe plating]

[0121] The Fe plating bath is a sulfuric acid bath, and its composition is adjusted to 55-65 g / L of iron, 5-7 g / L of sodium, and pH 2.0-2.2. Other plating conditions are shown in Table 2. The amount of iron plating was measured on the steel sheet after the Fe electroplating treatment. It should be noted that the amount of iron plating was measured based on a pre-made calibration curve, and the deviation of the amount of iron plating was evaluated by continuously measuring five points in the width direction of the steel sheet using an online adhesion meter using fluorescent X-rays.

[0122] [Hot-dip galvanizing]

[0123] The hot-dip galvanizing was carried out by a common method. In the case of alloyed hot-dip galvanizing (GA) bath, the A1 concentration was 0.13%, and in the case of galvanizing (GI) bath, the A1 concentration was 0.20% (the remainder was zinc). The galvanizing adhesion amount was measured on the steel sheet after hot-dip galvanizing. It should be noted that the galvanizing adhesion amount was also measured at three points in the width direction of the steel sheet using an online adhesion meter using fluorescent X-rays based on a pre-made calibration curve, and the average value was obtained.

[0124] In addition, the appearance of the coating after hot-dip galvanizing was evaluated. The coating appearance score was 1 point if non-coating, severe uneven color tone, or waviness defects occurred frequently, 2 points if non-coating, uneven color tone, or waviness defects existed and most of them needed to be removed, 3 points if partial removal was required due to uneven color tone or waviness defects, 4 points if very slight uneven color tone or poor appearance did not need to be removed, and 5 points if no non-coating, uneven color tone, or waviness defects were observed.

[0125] In addition, the rate of discharge of the plating solution to the back of the electrode plate is determined by the plating solution discharge ports 19 (see Figure 3 ) and the total flow rate of the plating solution supplied to the gap between the upper electrode plate and the steel plate P.

[0126] The results of the above measurements and evaluations are shown in Table 2 together with the electroplating conditions.

[0127]

[0128] As shown in Table 2, in the hot-dip galvanized steel sheet obtained according to the present invention, although there are irregular shapes before electroplating, a good galvanized layer is still obtained. Figure 5 In the electroplating Fe device of the horizontal circulation pool shown in FIG. 2 , the plating solution 30 is supplied from the nozzle manifold 44 to the passage 43, so the pressing force applied to the steel plate cannot be increased. Therefore, in conditions 1 and 2, the straightening force on the steel plate in the plating pool is weak, and an excellent plating appearance cannot be obtained. That is, according to the present invention, plating that is not affected by the shape disturbance of the steel plate before plating is achieved. In other words, as can be seen from the results shown in Table 2, the straightening of the steel plate shape in the electroplating of the present invention is fully achieved.

[0129] Explanation of symbols

[0130] P Steel Plate

[0131] 10-electrode plate

[0132] 10a Through hole

[0133] 11Electrode connection part

[0134] 12 Back Panel

[0135] 13 Insulator

[0136] 14 jet header

[0137] 15 round tube nozzle

[0138] 16 power rod

[0139] 20 conductor rollers

[0140] 21 Support roller

[0141] 30 plating solution

[0142] 51 Unwinding Machine

[0143] 52Joining device

[0144] 53 entrance looper

[0145] 54 degreasing device

[0146] 55 Pickling device

[0147] 56Fe electroplating device

[0148] 57 Water washing device

[0149] 58 Annealing device

[0150] 59Hot dip galvanizing device

[0151] 60 Alloying treatment device

[0152] 61Quenching and tempering rolling device

[0153] 62 Post-processing device

[0154] 63 export looper

[0155] 64 Inspection device

[0156] 63 tension coiler

Claims

1. A method for manufacturing a hot-dip galvanized steel sheet, which is a method for manufacturing a hot-dip galvanized steel sheet through the following steps: The electroplating step includes supplying an iron-based plating solution to the steel plate in a gap between the continuously moving steel plate and an electrode plate disposed opposite to the steel plate, and applying electricity to the electrode plate as an anode and the steel plate as a cathode to perform electroplating to form an iron-based film on the surface of the steel plate; an annealing process, heating the steel sheet after the electroplating process; and The hot-dip galvanizing step is to perform hot-dip galvanizing on the steel sheet after the annealing step. In the electroplating step, the ratio of the flow rate of the plating solution flowing out to the back side of the electrode plate not facing the steel plate to the flow rate of the plating solution supplied to the steel plate, that is, the plating solution discharge rate, is set to less than 50%.

2. The method for producing a hot-dip galvanized steel sheet according to claim 1, wherein: The adhesion amount of the iron film is 2.0 g / m 2 above.

3. The method for producing a hot-dip galvanized steel sheet according to claim 1 or 2, wherein: The plating solution discharge rate is less than 10%.

4. The method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 3, wherein: The plating solution flow rate Q on each single side of the electrode plate satisfies the following formula (1), and the unit of the plating solution flow rate is m 3 / minute, Q≥60WLH····(1) Here, W is the width of the steel plate, in m, L is the length of the long side of the electrode plate, in m, and H is the distance between the electrode plate and the steel plate, in m.

5. The method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 4, wherein: The steel sheet has a component composition including, by mass%, 0.3% or less of C and 1.0 to 6.0% in total of one or more of Si and Mn.

6. A manufacturing equipment for hot-dip galvanized steel sheet, comprising: Electroplating device, forming an iron coating on the steel plate continuously moving on the line; an annealing device for heating the steel plate that has passed through the electroplating device; and A hot-dip galvanizing device is used to perform hot-dip galvanizing on the steel sheet that has passed through the annealing device. The electroplating device comprises electrode plates arranged relatively along a travel line of the steel plate and a jet nozzle supplying an iron-based plating solution from the electrode plate side to the travel line, the electrode plate being an anode and the steel plate being a cathode, and the ratio of the flow rate of the plating solution flowing out to the back side of the electrode plate not opposite to the steel plate to the flow rate of the plating solution supplied from the jet nozzle, that is, the plating solution discharge rate, is less than 50%.

7. The manufacturing equipment of hot-dip galvanized steel sheet according to claim 6, wherein: The electrode plate has at least one through hole extending in a direction intersecting the traveling line and penetrating the electrode plate, and the injection nozzle is arranged in at least one of the through holes.

8. The manufacturing equipment of hot-dip galvanized steel sheet according to claim 6 or 7, wherein: A back plate and a jet manifold are provided on the back side of the electrode plate in sequence from the traveling line side, a plurality of injection nozzles extending through the back plate and the electrode plate are connected to the jet manifold, the back plate is connected to the back side of the electrode plate via an electrode connecting portion, and an insulator is arranged in the space between the back plate and the electrode plate generated by the electrode connecting portion.

9. The manufacturing equipment of hot-dip galvanized steel sheet according to claim 8, wherein: The plating tank is composed of one or more plating tanks, wherein the electrode plates are assembled as a plurality of plates and are seamlessly combined with one of the back plates.

10. The manufacturing equipment of hot-dip galvanized steel sheet according to claim 9, wherein: In each of the plating cells, the jet header is divided into a plurality of parts at positions that do not interfere with the electrode connecting portion.

11. The manufacturing facility of the hot-dip galvanized steel sheet according to any one of claims 8 to 10, wherein: The jet manifold has a plating solution pipe for supplying plating solution into the jet manifold, and a ratio Ak / An of a cross-sectional area Ak of ​​the plating solution pipe to a total cross-sectional area An of injection ports of injection nozzles connected to the jet manifold is 2.5 or more.

12. The manufacturing facility of the hot-dip galvanized steel sheet according to any one of claims 6 to 11, wherein: The electroplating device and the annealing device are located on the same line.

13. The manufacturing facility of the hot-dip galvanized steel sheet according to any one of claims 6 to 11, wherein: The electroplating device and the annealing device are located on different lines.