Catalyst coated ion conducting membranes comprising conductive polymers for water electrolysis
By introducing conductive polymer and polyelectrolyte multi-layer coating technology into the water electrolytic membrane, the problems of high cost and unstable performance in PEM-WE and AEM-WE systems are solved, and efficient and low-cost hydrogen production is achieved.
Patent Information
- Application Number
- CN202380033038.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-10
- Filing Date
- 2023-05-04
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing water electrolysis technology, the high capital cost of the PEM-WE system and the insufficient membrane hydroxyl ion conductivity and stability of the AEM-WE system lead to high cost of producing high-purity hydrogen, and unstable catalyst integration and performance.
New catalyst-coated ion conductive films have been developed, including anode or cathode catalyst coatings of conductive polymers, to improve the conductivity of the catalyst coatings through conductive polymers, and to improve the proton conduction of the membrane using polyelectrolyte multilayer coating technology. and stability, reducing high-frequency resistance and system costs.
Higher electrolytic cell efficiency and lower system cost are achieved, lower cost green hydrogen is produced, while improving the mechanical strength and chemical thermal stability of the membrane and reducing the cross-permeability of H2 and O2.
Smart Images

Figure CN119032201A_ABST
Abstract
Description
[0001] Priority declaration
[0002] This application claims priority to U.S. application No. 17 / 662,675, filed on May 10, 2022, which is incorporated herein in its entirety. Background Art
[0003] Hydrogen plays an important role in the path towards an environmentally friendly, low-carbon energy structure as an energy carrier for grid balancing or power-to-gas and power-to-liquid processes. Water electrolysis produces high-quality hydrogen by electrochemically decomposing water into hydrogen and oxygen; the reaction is given by the following equation 1. The water electrolysis process is an endothermic process, and electricity is the energy source. When the method is operated by renewable energy such as wind, solar or geothermal energy, water electrolysis has a zero carbon footprint. The main water electrolysis technologies include alkaline electrolysis, proton exchange membrane (PEM) water electrolysis (such as Figure 1 PEM-WE as shown), anion exchange membrane (AEM) water electrolysis (such as Figure 2 AEM-WE) and solid oxide water electrolysis as shown.
[0004] like Figure 1 As shown, in the PEM-WE system 100, the anode 105 and the cathode 110 are separated by a solid PEM electrolyte 115, such as that manufactured by the Chemours company under the trademark A fluorinated copolymer based on sulfonated tetrafluoroethylene is sold. The anode and cathode catalysts typically contain IrO2 and Pt, respectively. At the positively charged anode 105, pure water 120 is oxidized to produce oxygen 125, electrons (e - ) and protons; the reaction is given by Equation 2. Protons are transported from the anode 105 to the cathode 110 through the proton-conducting PEM 115. At the negatively charged cathode 110, a reduction reaction occurs in which electrons from the cathode 110 are given to protons to form hydrogen 130; the reaction is given by Equation 3. The PEM 115 not only conducts protons from the anode 105 to the cathode 110, but also separates the H2 gas 130 and O2 gas 125 produced in the water electrolysis reaction. PEM water electrolysis is one of the advantageous methods for converting renewable energy into high-purity hydrogen, with the advantages of compact system design at high pressure difference, high current density, high efficiency, fast response, small footprint, low temperature (20°C-90°C) operation, and high-purity oxygen byproduct. However, one of the main challenges of PEM water electrolysis is the high capital cost of the cell stack, including expensive acid-resistant stack hardware (such as Pt-coated Ti bipolar plates), expensive precious metal catalysts required for electrodes, and expensive PEMs.
[0005] Water electrolysis reaction: 2H2O→2H2+O2(1)
[0006] Anodic oxidation reaction of PEM-WE: 2 H2O → O2 + 4 H + + 4 e (2)
[0007] Cathodic reduction reaction of PEM-WE: 2 H + + 2 e - → H2 (3)
[0008] AEM-WE is a developing technology. Figure 2 As shown, in the AEM-WE system 200, the anode 205 and the cathode 210 are separated by a solid AEM electrolyte 215. Typically, a water feed 220 with an added electrolyte (such as diluted KOH or K2CO3 or deionized water) is fed to the cathode side. The anode and cathode catalysts typically include Ni-based or Ni alloy catalysts that do not contain platinum group metals. At the negatively charged cathode 210, water is reduced to form hydrogen 225 and hydroxyl ions by adding four electrons; the reaction is given by Equation 4. The hydroxyl ions diffuse from the cathode 210 to the anode 205 through the AEM 215 that conducts hydroxyl ions. At the positively charged anode 205, the hydroxyl ions recombine into water and oxygen 230; the reaction is given by Equation 5. The AEM 215 not only conducts hydroxyl ions from the cathode 210 to the anode 205, but also separates the H2 225 and O2 230 produced in the water electrolysis reaction. The AEM 215 allows the production of hydrogen 225 with a very high purity of at least 99.9% at high pressures of up to 35 bar.
[0009] Cathodic reduction reaction of AEM-WE: 4 H2O + 4 e - → 2 H2 + 4 OH - (4)
[0010] Anodic oxidation reaction of AEM-WE: 4 OH - → 2 H2O + O2 + 4 e - (5)
[0011] AEM-WE has advantages over PEM-WE because it allows the use of cheaper platinum group metal-free catalysts, such as Ni and Ni alloy catalysts. In addition, much cheaper stainless steel bipolar plates can be used in the gas diffusion layer (GDL) of AEM-WE instead of the expensive Pt-coated Ti bipolar plates currently used in PEM-WE. However, the biggest obstacle to the development of AEM systems is the membrane hydroxyl ion conductivity and stability, as well as the lack of understanding of how to integrate catalysts into AEM systems. Research on AEM-WE in the literature focuses on developing electrocatalysts, AEMs, and understanding the operating mechanism, with the general goal of obtaining efficient, low-cost and stable AEM-WE technology.
[0012] In the PEM-WE and AEM-WE systems, several components are integrated to produce green H2, including a collector plate, a bipolar plate (BP), two porous transport layers (PTL), a three-layer membrane electrode assembly (MEA) consisting of a membrane, an anode layer, and a cathode layer. In some cases, when the catalyst is coated on one surface of the PTL, a five-layer MEA including a membrane, an anode layer, a cathode layer, and two PTL layers is used in the PEM-WE and AEM-WE systems. Among the main components, the MEA is the most important component because the electrochemical water electrolysis reaction occurs in the MEA. There are two main MEA manufacturing methods, including catalyst-coated substrates (CCS) and catalyst-coated membranes (CCM). Different MEA manufacturing technologies and different catalyst loadings on the anode and / or cathode coatings generally result in different performances.
[0013] Membrane is one of the key components in MEA and is an important driver of safety and performance. Some important properties of membranes used for membrane electrolysis include high conductivity, high ion permeability, high ion exchange capacity (for ion exchange membranes), high ion / H2 and O2 selectivity (low H2 and O2 permeability / crossover), low price, low area resistance to minimize efficiency loss caused by ohmic polarization, high tolerance to oxidizing and reducing conditions, chemically inert over a wide pH range, high thermal stability, and high proton conductivity and high mechanical strength (thickness, low swelling).
[0014] The anode in the MEA for electrochemical cells on one surface of the membrane coated on one surface of the PTL is an electrode whose main reaction is an oxidation reaction (e.g., a water oxidation / oxygen evolution reaction electrode for a water electrolyzer). The cathode in the MEA for electrochemical cells on the other surface of the membrane coated on one surface of the PTL is an electrode whose main reaction is a reduction reaction (e.g., a proton reduction / hydrogen evolution reaction electrode for a water electrolyzer). Both the anode and cathode are key components in the MEA. Typically, for PEM-WE, unloaded or loaded rare platinum group electrocatalysts based on iridium (Ir) are used for oxygen evolution reaction (OER) on the anode, and carbon-loaded platinum electrocatalysts (Pt / C) are used for hydrogen evolution reaction (HER) on the cathode. With the increase in GW-scale PEM-WE installation projects, it is necessary to significantly reduce the amount of platinum group catalyst loading on the catalyst coating. Methods for reducing the loading of platinum group catalysts include: loading platinum group metals or metal oxides (such as IrO2) on high surface area support materials, designing catalysts with unique structures such as nanostructured films, nanowires or core-shell structures, using advanced catalyst layer coating techniques, and reducing the thickness of the catalyst coating. However, reducing the Ir-based catalyst loading in the anode coating will generally result in a loss in the oxygen evolution reaction (OER) kinetics of the PEM-WE. Research on CCM manufacturing methods has focused on the impact of catalyst inks on the manufacture and performance of CCMs in water electrolysis. Catalyst inks used to form anode and cathode coatings on the membrane surface or on the PTL are important for providing high catalyst activity, high proton or hydroxide conductivity, and high conductivity in the catalyst layer to the MEA.
[0015] For water electrolysis to have widespread application in renewable energy systems, significant advances are needed in cost-effective, high-performance, and stable catalysts, catalyst ink formulations, membrane materials, and other stack components. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is a diagram of one embodiment of a PEM-WE cell.
[0017] Figure 2 is a diagram of one embodiment of an AEM-WE battery.
[0018] Figure 3 is a graph comparing the polarization curves of individual water electrolysis cells.
[0019] Figure 4 is a graph comparing the high frequency resistance (HFR) versus current density for a single water electrolysis cell.
[0020] Figure 5 is a graph comparing the polarization curves of individual water electrolysis cells. DETAILED DESCRIPTION
[0021] A novel membrane electrode assembly (MEA) incorporating a novel catalyst-coated ion-conducting membrane has been developed. The catalyst-coated ion-conducting membrane comprises an ion-conducting membrane and an anode catalyst coating or a cathode catalyst coating or both, wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer. The conductive polymer comprises a conductive organic polymer. Incorporating the conductive polymer into the catalyst coating improves the conductivity of the catalyst coating in the MEA, which results in improved electrolysis performance with lower high frequency resistance and lower cell voltage at the same current density compared to an MEA without the conductive polymer in the catalyst coating. The improved electrolysis performance enables higher electrolyzer efficiency and lower system cost compared to current prior art MEAs for water electrolysis, thereby producing lower cost green hydrogen.
[0022] MEA is the center of PEM-WE and AEM-WE system. The catalyst coated membrane (CCM) and catalyst coated substrate (CCS) method for making MEA usually use catalyst ink on the surface of the membrane for CCM or on the surface of PTL to coat the catalyst layer. Usually, the catalyst ink includes catalyst, polymer ionomer and solvent, such as a mixture of organic solvent and water. Catalyst allows hydrogen evolution and oxygen evolution reaction to occur. Catalyst should have good conductivity, good electrocatalytic activity and stability.
[0023] In the novel catalyst-coated ion-conducting membrane, the anode catalyst coating or the cathode catalyst coating or both contain a conductive polymer in addition to the catalyst and the polymer ionomer. The conductive polymer is added to the catalyst ink to improve the conductivity of the catalyst coating in the MEA. The conductive polymer has high conductivity, high chemical, oxidative and thermal stability, and good dispersibility in the catalyst ink. Conductive polymers suitable for the present application include, but are not limited to, poly(3,4-ethylenedioxythiophene) (PEDOT), blends of PEDOT and polystyrene sulfonate (PSS), polyacetylene (PA), polyaniline (PANI), polypyrrole (PPy), polythiophene (PTH), polyparaphenylene (PPP), polyparaphenylene vinylene (PPV) and polyfuran (PF).
[0024] One aspect is a novel catalyst-coated ion-conducting membrane. In one embodiment, the catalyst-coated ion-conducting membrane comprises: an ion-conducting membrane; and an anode catalyst coating on a first surface of the ion-conducting membrane, or a cathode catalyst coating on a second surface of the ion-conducting membrane, or both; wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer.
[0025] Suitable cathode catalysts include, but are not limited to, platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, nickel, molybdenum, iron, copper, chromium, alloys thereof, oxides thereof, carbides thereof, phosphides thereof, or combinations thereof.
[0026] Suitable anode catalysts include, but are not limited to, iridium, platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, copper, nickel, molybdenum, iron, chromium, alloys thereof, oxides thereof, carbides thereof, phosphides thereof, or combinations thereof.
[0027] The cathode and / or anode catalysts may be supported or unsupported.
[0028] Suitable high surface area support materials for preparing supported catalysts include titanium oxide, aluminum oxide, silicon dioxide, zirconium dioxide, yttrium oxide, cerium oxide, ceria, lanthanum oxide, tin oxide, tungsten oxide, molybdenum oxide, niobium oxide, tantalum oxide, tin oxide, and anion- and cation-doped variations of these oxides, including but not limited to fluorine-doped tin oxide, indium-doped and antimony-doped tin oxide, and mixtures thereof.
[0029] The polymer ionomer, acting as a binder for the catalyst particles, generates protons (H) between the membrane and the reaction sites within the electrode catalyst coating. + ) or hydroxide (OH - ) transport path. Polymer ionomers improve the utilization of electrocatalyst particles while reducing internal resistance. Polymer ionomers are ideally insoluble in water and have high H + or OH - conductivity, high chemical, oxidative and thermal stability and high solubility or dispersibility in solvents. The polymer ionomer may be a fluorinated ionomer such as Non-fluorinated ionomers or hydroxide conductive polymer ionomers, or combinations thereof. In some embodiments, the chemical structure of the polymer ionomer is similar to the membrane in the MEA, which allows low interfacial resistance and similar swelling in contact with water to avoid delamination, but higher O2 and H2 permeability than the membrane.
[0030] Suitable proton conducting fluorinated polymer ionomers include, but are not limited to, perfluorosulfonic acid (PFSA) polymers such as Sulfonated trifluorostyrene-trifluorostyrene copolymers, sulfonated polystyrene-poly(vinylidene fluoride) copolymers, or combinations thereof. Suitable proton-conducting non-fluorinated polymer ionomers include, but are not limited to, sulfonated polysulfones, cross-linked sulfonated polysulfones, sulfonated poly(phenylene sulfones), sulfonated phenylated poly(phenylenes), sulfonated polystyrene, sulfonated polyethersulfones, cross-linked sulfonated polyethersulfones, sulfonated polyetheretherketones, cross-linked sulfonated polyetheretherketones, or combinations thereof. Suitable hydroxide-conducting polymer ionomers include, but are not limited to, alkylammonium polyfluorene ionomers, poly(arylpiperidinium) ionomers, high-density polyethylene functionalized with benzyltrimethylammonium, polyphenylenes based on N-heterocycles and alkylammonium, poly(ethylene-co-tetrafluoroethylene) functionalized with benzyltrimethylammonium, or combinations thereof.
[0031] Solvents may be used to disperse the catalyst particles, polymer ionomer, and conductive polymer to form a uniform catalyst ink. Solvents ideally have a low boiling point so that they can be easily removed during or after the ink coating process. Suitable solvents include, but are not limited to, alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, or tert-butanol; acetone; ethers; water; or combinations thereof.
[0032] The ion-conducting membrane may be a proton exchange membrane (PEM) or an anion exchange membrane (AEM). The ion-conducting membrane may be a polyelectrolyte multilayer-coated PEM, comprising a PEM and a polyelectrolyte multilayer coating on the surface of the PEM, wherein the polyelectrolyte multilayer coating comprises alternating layers of polycationic polymer layers and polyanionic polymers, and wherein the polycationic polymer layers are in contact with the PEM. The ion-conducting membrane may also be a polyelectrolyte multilayer-coated AEM, comprising an AEM and a polyelectrolyte multilayer coating on the surface of the AEM, wherein the polyelectrolyte multilayer coating comprises alternating layers of polycationic polymer layers and polyanionic polymers, and wherein the polycationic polymer layers are in contact with the AEM.
[0033] The polyelectrolyte multilayer coated PEM includes a polycationic polymer layer deposited on the PEM and in contact with the PEM. There may be one, two, three, four, five or more groups of alternating polycationic polymer layers and polyanionic polymer layers on one or both sides of the PEM. The polyelectrolyte multilayer coated AEM includes a polyanionic polymer layer deposited on the AEM and in contact with the AEM. There may be one, two, three, four, five or more groups of alternating polycationic polymer layers and polyanionic polymer layers on one or both sides of the AEM. The top layer of the polyelectrolyte multilayer coating may be a polycationic polymer layer or a polyanionic polymer layer. See U.S. Serial No. 17,451,227, entitled "Polyelectrolyte Multilayer Coated Proton Exchange Membrane for Electrolysis and Fuel Cell Application", filed on October 18, 2021, which is incorporated herein in its entirety.
[0034] The polyelectrolyte multilayer coating can be formed using a layer-by-layer self-assembly method. For example, the layer-by-layer self-assembly can be achieved by adsorption, electrostatic interaction, covalent bonding, hydrogen bonding, van der Waals forces, hydrophobic interactions, or a combination thereof. The method for forming the polyelectrolyte multilayer coating via layer-by-layer self-assembly can be selected from, but not limited to, dip coating, spray deposition, centrifugal deposition, electrodeposition, meniscus / slit die coating, brush coating, roller coating, metering rod / Meyer rod coating, knife casting, etc.
[0035] The choice of manufacturing method depends on the polycations and polyanions to be assembled, the time required for layer-by-layer self-assembly, and the shape of the cation exchange membrane on which the polyelectrolyte multilayer coating will be deposited. The first polyelectrolyte layer is formed by adsorbing (for example) polycations or polyanions on one or both surfaces of the PEM or AEM with opposite charges. Subsequently, a second layer of polyelectrolyte with opposite charge to the first layer of polyelectrolyte is deposited on the first layer of polyelectrolyte to form a set of alternating layers on the PEM or AEM. Nanostructured polyelectrolyte multilayer coatings with n sets of alternating layers on one or both surfaces of the PEM produce PEM (or AEM) / (polycation-polyanion) respectively. n or (polyanion-polycation) n / PEM (or AEM) / (polycation-polyanion) nA novel proton exchange membrane. The increase in the thickness of the polyelectrolyte multilayer depends on the number of layers deposited and can be linear or nonlinear. During the layer-by-layer self-assembly process, several parameters such as ionic strength, pH, temperature, polyelectrolyte structure, concentration and charge density can be adjusted. Oppositely varying polyelectrolyte layers are deposited on the surface of a PEM or AEM. The polyelectrolyte multilayer is insoluble and is thermally and chemically stable.
[0036] The polyanionic polymer in the polyelectrolyte multilayer coating may be different from the ion exchange polymer in the PEM or AEM.
[0037] The PEM comprises a cation exchange polymer or a mixture of a cation exchange polymer and an inorganic filler comprising covalently bonded acidic functional groups. The PEM in the novel polyelectrolyte multilayer coated PEM comprises -SO3 - 、-COO - , –PO3 2- or-PO3H - Cation exchange functional groups. The cation exchange polymer in the PEM can be selected from, but not limited to, perfluorosulfonic acid (PFSA) polymers such as FS, or Cross-linked perfluorinated cation exchange polymers, partially fluorinated polymers, cross-linked partially fluorinated cation exchange polymers, non-fluorinated hydrocarbon polymers, cross-linked non-fluorinated hydrocarbon cation exchange polymers or their combination. PEM has high mechanical strength, good chemical and thermal stability and good proton conductivity. However, when thin films with lower cost and lower area specific resistance are used for electrolysis and fuel cell applications, PEM usually has high cost, high area specific resistance and high H2 and O2 cross. Compared with PEM without polyelectrolyte multilayer coating, the PEM of novel polyelectrolyte multilayer coating has low membrane area specific resistance, low swelling, significantly reduced H2 and O2 cross and enhanced proton conductivity.
[0038] The PEM used to prepare the polyelectrolyte multilayer coated PEM can be a composite proton conducting membrane described in U.S. Patent Application No. 17 / 162,421, entitled “Composite Proton Conductive Membranes” filed on January 29, 2021, which is incorporated herein by reference in its entirety. The application discloses a novel composite proton conducting membrane comprising a covalently bonded acidic functional group and at least 150 m 2 / g of high surface area inorganic filler, and water-insoluble ion-conducting polymer. Compared with the composite proton conducting membrane without polyelectrolyte multilayer coating, the deposition of polyelectrolyte multilayer coating on the composite proton conducting membrane leads to reduced membrane swelling, significantly reduced H2 and O2 crossover and enhanced proton conductivity.
[0039] The inorganic filler containing covalently bonded acidic functional groups in the cation exchange membrane can be selected from but not limited to silica gel, precipitated silica, fumed silica, colloidal silica, alumina, silica-alumina, zirconia, molecular sieves, metal organic frameworks, zeolitic imidazolate frameworks, covalent organic frameworks or combinations thereof, and wherein the filler can contain covalently bonded acidic functional groups and 150 m 2 / g or higher, or 300m 2 / g or higher, or 400m 2 / g or higher high surface area. Molecular sieve has a framework structure, which can be characterized by a unique wide-angle X-ray diffraction pattern. Zeolite is a subclass of molecular sieves based on aluminosilicate compositions. Non-zeolitic molecular sieves are based on other compositions, such as aluminophosphates, silicoaluminophosphates and silicon dioxide. Molecular sieves can have different chemical compositions and different framework structures. Molecular sieves can be microporous or mesoporous molecular sieves, and need to be stable in aqueous solutions with a pH less than 6. The acidic functional groups covalently bonded to the inorganic filler can be selected from, but not limited to -H2PO3, -R-H2PO3, -SO3H, -R-SO3H, -COOH, -R-COOH, -C6H5OH, -R-C6H5OH or combinations thereof, wherein R represents a linear alkyl group, a branched alkyl group, a cycloalkyl group, an organic amino group, an organic amino group substituted with an acid group or an aryl group, and the number of carbon atoms in these groups is preferably 1 to 20, more preferably 1 to 10. The inorganic filler may be in the form of, but not limited to, particles, beads, thin plates, rods or fibers. The size of the inorganic filler is in the range of 2 nm to 200 μm, or in the range of 10 nm to 100 μm, or in the range of 50 nm to 80 μm. In some embodiments, the inorganic filler is aminopropyl-N,N-di(methylphosphonic acid) functionalized silica gel such as AMPA, aminopropyl-N,N-di(methylphosphonic acid) functionalized fumed silica, n-propylphosphonic acid functionalized silica gel, n-propylphosphonic acid functionalized fumed silica, p-toluenesulfonic acid functionalized silica gel, p-toluenesulfonic acid functionalized fumed silica, 4-ethylbenzenesulfonic acid functionalized silica gel such as Toluenesulfonic acid, 4-ethylbenzenesulfonic acid functionalized fumed silica, n-propylsulfonic acid functionalized silica gel, n-propylsulfonic acid functionalized fumed silica, or a combination thereof.
[0040] Suitable cation exchange polymers include, but are not limited to, perfluorinated sulfonic acid polymers, perfluorinated carboxylic acid polymers, sulfonated aromatic polymers, crosslinked sulfonated aromatic polymers, or combinations thereof. Suitable cation exchange polymers include, but are not limited to, copolymers of tetrafluoroethylene and perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid, copolymers of tetrafluoroethylene and perfluoro-5-oxa-6-heptene-sulfonic acid, copolymers of tetrafluoroethylene and perfluoro-4-oxa-5-hexene-sulfonic acid, copolymers of tetrafluoroethylene and perfluoro-3-oxa-4-pentene-sulfonic acid, copolymers of perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid and perfluoro(2,2-dimethyl-1,3-dioxole), copolymers of perfluoro-5-oxa-6-heptene-sulfonic acid and perfluoro(2,2-dimethyl-1,3-dioxole). copolymers of perfluoro-4-oxa-5-hexene-sulfonic acid and perfluoro(2,2-dimethyl-1,3-dioxole), copolymers of perfluoro-3-oxa-4-pentene-sulfonic acid and perfluoro(2,2-dimethyl-1,3-dioxole), copolymers of perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid and perfluoro(2-methylene-4-methyl-1,3-dioxolane), copolymers of perfluoro-5-oxa-6-heptene-sulfonic acid and perfluoro(2-methylene-4-methyl-1,3-dioxolane), copolymers of perfluoro-4-oxa-5-hexene-sulfonic acid and perfluoro(2-methylene-4-methyl-1,3 -dioxolane), copolymers of perfluoro-3-oxa-4-pentene-sulfonic acid and perfluoro(2-methylene-4-methyl-1,3-dioxolane), copolymers of perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid and 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, copolymers of perfluoro-5-oxa-6-heptene-sulfonic acid and 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, copolymers of perfluoro-4-oxa-5-hexene-sulfonic acid and 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, copolymers of perfluoro-3-oxa-4-pentene-sulfonic acid and perfluoro(2-methylene-4-methyl-1,3-dioxolane), copolymers of perfluoro-3,6-dioxa-4-methyl-7-octene-sulfonic acid and 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, copolymers of perfluoro-5-oxa-6-heptene-sulfonic acid and 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, copolymers of perfluoro-4-oxa-5-hexene-sulfonic acid and 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, -pentene-sulfonic acid and 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole copolymers, sulfonated poly(etheretherketone) (SPEEK), sulfonated polyethersulfone, sulfonated polyphenylsulfone, sulfonated poly(2,6-dimethyl-1,4-phenylene oxide), sulfonated poly(4-phenoxybenzoyl-1,4-phenylene), sulfonated polyphenylene oxide, sulfonated poly(phenylene), sulfonated poly(phthalazinone), cross-linked SPEEK, cross-linked sulfonated polyethersulfone, cross-linked sulfonated polyphenylsulfone, cross-linked (polyphenylene sulfide sulfone nitrile), sulfonated polystyrene, sulfonated poly(vinyltoluene), cross-linked sulfonated polystyrene, cross-linked sulfonated poly(vinyltoluene), or a combination thereof.
[0041] The first layer deposited on one or both surfaces of the PEM with negative ionic charge should be a polycationic polymer layer with positive ionic charge, opposite to those on the cation exchange membrane, which results in the formation of a stable coating as the first part of the first polyelectrolyte bilayer via electrostatic interactions between the cation exchange polymers of the PEM and the polycations deposited on the surface of the PEM. A polyanionic polymer with an opposite charge is then deposited on the surface of the first polycationic polymer coating via electrostatic interactions to form the second part of the first polyelectrolyte bilayer. PEM / (polycation-polyanion) n or (polyanion-polycation) n / PEM / (polycation-polyanion) n The polyelectrolyte multilayer can be formed after the same alternating deposition process. The thickness of each layer of polyanion or polycation is less than 50nm, or less than 20nm, or less than 10nm, or less than 5nm. The polyanionic polymer in the polyelectrolyte multilayer has a negative charge and can be the same or different from the cation exchange polymer in the PEM, but the polyanionic polymer cannot be the first polyelectrolyte layer deposited on the surface of the PEM with a negative charge. The polyanionic polymer suitable for preparing the PEM coated with polyelectrolyte multilayer has a proton conductivity similar to or higher than that of the PEM, and has a H2 and O2 permeability similar to or lower than that of the PEM. However, polyanionic polymers and polycationic polymers are soluble in aqueous solution, which makes the membrane prepared by polyanionic polymers or polyanionic polymers unsuitable for water electrolysis or fuel cell applications. Compared with PEMs for water electrolysis or fuel cell applications, the polyelectrolyte multilayer deposited on one or both surfaces of the PEM via layer-by-layer self-assembly is not only insoluble and thermally and chemically stable, but also has significantly reduced swelling of the cation exchange membrane and H2 and O2 crossover, as well as enhanced proton conductivity.
[0042] Polycationic polymers suitable for preparing polyelectrolyte multilayer coated PEMs or AEMs include, but are not limited to, protonated chitosan; amine-based linear, highly branched or dendritic polycationic polymers selected from the group consisting of polybiguanide, quaternary ammonium polyethyleneimine, quaternary ammonium polypropyleneimine, quaternary ammonium polyamidoamine (PAMAM), poly(vinylamine hydrochloride) (PVH), poly(allylamine hydrochloride) (PAH), poly(amidoamine hydrochloride), poly(N-isopropylallylamine hydrochloride), poly(N-tert-butylallylamine hydrochloride), poly(N-1,2-dimethylpropylallylamine hydrochloride), poly(N-methylallylamine hydrochloride), poly(N,N-dimethylallylamine hydrochloride), poly(2-vinylpiperidine hydrochloride), poly(4-vinylpiperidine hydrochloride), poly(diallyldimethylammonium chloride), poly(acrylamide-co-diallyldimethylammonium chloride), poly(diallyl) methylamine hydrochloride), copolymers of 2-propylene-1-amine hydrochloride and N-2-propylene-2-propylene-1-amine hydrochloride, poly(N-alkyl-4-vinylpyridinium) salts, polylysine, polyornithine, polyarginine, poly(ethylene oxide)-block-poly(vinylbenzyltrimethylammonium chloride), poly(ethylene oxide)-block-poly(l-lysine), poly(2-methacryloyloxyethyl phosphorylcholine methacrylate)-block-poly(vinylbenzyl trimethylammonium chloride), poly[2-(dimethylamino)-ethyl methacrylate, poly[3-(dimethylamino)-propyl methacrylate], poly[2-(dimethylamino)-ethyl methacrylamide], poly[3-(dimethylamino)propyl methacrylamide], poly[2-(trimethylamino)ethyl methacrylate chloride], poly[2-(diethylamino)ethyl methacrylate], poly[2-(dimethylamino)ethyl acrylate]; or a combination thereof.
[0043] Polyanionic polymers suitable for preparing polyelectrolyte multilayer coated PEM or AEM include, but are not limited to, sulfonated hydrocarbon polymers, poly(acrylic acid), poly(sodium phosphate), or negatively charged polysaccharide polyanionic polymers, or combinations thereof. Suitable sulfonated hydrocarbon polymers include, but are not limited to, sulfonated poly(ether ether ketone), sulfonated polyether sulfone, sulfonated polyphenyl sulfone, sulfonated poly(2,6-dimethyl-1,4-phenylene oxide), sulfonated poly(4-phenoxybenzoyl-1,4-phenylene), sulfonated polyphenylene oxide, sulfonated poly(phenylene), sulfonated poly(phthalazinone), sulfonated polystyrene, sulfonated poly(vinyl toluene), poly(acrylic acid), poly(sodium vinyl sulfonate), poly(sodium phosphate), or combinations thereof. Suitable negatively charged polysaccharide polyanionic polymers include, but are not limited to, sodium alginate, potassium alginate, calcium alginate, ammonium alginate, alginic acid, sodium hyaluronate, potassium hyaluronate, calcium hyaluronate, ammonium hyaluronate, hyaluronic acid, kappa-carrageenan, lambda-carrageenan, iota-carrageenan, carboxymethyl curdlan, sodium carboxymethyl curdlan, potassium carboxymethyl curdlan, calcium carboxymethyl curdlan, ammonium carboxymethyl curdlan, carboxymethyl cellulose, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, calcium carboxymethyl cellulose, ammonium carboxymethyl cellulose, or combinations thereof.
[0044] Another aspect is a membrane electrode assembly incorporating a catalyst-coated ion-conducting membrane. In one embodiment, the membrane electrode assembly includes: an ion-conducting membrane; a first porous transport layer adjacent to a first side of the ion-conducting membrane; and a second porous transport layer adjacent to a second side of the ion-conducting membrane. There is an anode between the first side of the ion-conducting membrane and the first porous transport layer, the anode including an anode catalyst coating on a first side of the ion-conducting membrane adjacent to the first porous transport layer, or on a first side of the first porous transport layer adjacent to the first side of the ion-conducting membrane, or on both; and there is a cathode between the second side of the ion-conducting membrane and the second porous transport layer, the cathode including a cathode catalyst coating on a second side of the ion-conducting membrane adjacent to the second porous transport layer, or on a first side of the second porous transport layer adjacent to the second side of the ion-conducting membrane, or on both. The anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer. By "adjacent," it is meant that the layers are adjacent to each other, but not necessarily directly adjacent to each other. For example, the first porous transport layer is adjacent to one side of the ion-conducting membrane, but there is a catalyst coating between them, the catalyst coating being on the membrane, on the porous transport layer, or on both.
[0045] The conductive polymer, catalyst, polymer ionomer and ion conducting membrane are as described above.
[0046] In some embodiments, the membrane electrode assembly further includes a pair of bipolar plates, one plate adjacent to an outer side of the first porous transport layer and one plate adjacent to an outer side of the second porous transport layer.
[0047] Another aspect is an electrolysis system. In one embodiment, the electrolysis system includes: at least one cell forming a cell stack, the at least one cell including: a membrane electrode assembly, wherein the membrane electrode assembly includes: an ion-conducting membrane; a first side of a first porous transport layer adjacent to a first side of the ion-conducting membrane; a first side of a second porous transport layer adjacent to a second side of the ion-conducting membrane; an anode between the first side of the ion-conducting membrane and the first side of the first porous transport layer, the anode including an anode catalyst coating on a first side surface of the ion-conducting membrane adjacent to the first porous transport layer, on a first side of the first porous transport layer adjacent to the first side of the ion-conducting membrane, or on both; A cathode between the second side of the ion-conducting membrane and the first side of the second porous transport layer, the cathode comprising a cathode catalyst coating on the second side of the ion-conducting membrane adjacent to the second porous transport layer, or on the first side of the second porous transport layer adjacent to the second side of the ion-conducting membrane, or on both; wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer; a pair of bipolar plates, the first bipolar plate being adjacent to the second side of the first porous transport layer, and the second bipolar plate being adjacent to the second side of the second porous transport layer; and a pair of current collectors, the first current collector being adjacent to the first end of the battery stack, and the second current collector being adjacent to the second end of the battery stack.
[0048] The bipolar plate can be any bipolar plate known to those skilled in the art. Suitable bipolar plates include, but are not limited to, Pt-coated Ti bipolar plates, stainless steel bipolar plates, Ti-coated stainless steel bipolar plates, Ti and C-coated stainless steel bipolar plates, stainless steel bipolar plates, graphite bipolar plates, or combinations thereof. The bipolar plate needs to have a high electrical resistance to inhibit the diffusion of harmful ions from the bipolar plate and to inhibit hydrogen adsorption embrittlement. The bipolar plate also needs to have a low and stable electrical contact resistance over the life cycle of the stack.
[0049] In some embodiments, there is a pair of gaskets, with a first gasket between the first porous transport layer and the first bipolar plate, and a second gasket between the second porous transport layer and the second bipolar plate.
[0050] The electrolysis system typically comprises more than one cell. For example, the number of cells may be in the range of 2 cells to several thousand cells, or in the range of 2 cells to 3000 cells, or in the range of 2 cells to 2000 cells, or in the range of 2 cells to 1500 cells, or in the range of 2 cells to 1000 cells, or in the range of 2 cells to 750 cells, or in the range of 2 cells to 500 cells, or in the range of 10 cells to 3000 cells, or in the range of 10 cells to 2000 cells, or in the range of 10 cells to 1500 cells. In one embodiment, the present invention relates to a battery pack having a plurality of batteries, wherein the battery pack has a plurality of batteries, and the plurality of batteries are stacked together to form a battery stack. The current collector is positioned at each end of the battery stack, and the end plates are on the outside of the current collectors at each end.
[0051] The current collector can be any current collector known to those skilled in the art. Suitable current collectors can be made of materials including, but not limited to, nickel, steel, aluminum, copper, titanium, platinum, and gold.
[0052] The end plate may be any end plate known to those skilled in the art. Suitable end plate materials include, but are not limited to, aluminum alloys, stainless steel, Ti, and Pt-coated Ti.
[0053] Example
[0054] Example 1. Preparation of (SPEEK-PAH) 3 / -212 / (PAH-SPEEK)3 membrane, Three-layer MEA of PEDOT conductive polymer in ionomer and IrO2 anode catalyst coating (referred to as IrO2-PEDOT-1 / M-1 / PtMEA)
[0055] Poly(allylamine hydrochloride) (PAH) and sulfonated poly(etheretherketone) (SPEEK) polyelectrolyte multilayer coatings were prepared as follows: 212 membrane: A poly(allylamine hydrochloride) (PAH) polycation solution with 1 M NaCl and 0.02 M PAH was prepared by dissolving NaCl and PAH in DI H2O and adjusting the pH to 2.3 using 0.1 M HCl aqueous solution. An aqueous solution of SPEEK polyanion with 0.5 M NaCl and 0.02 M SPEEK was prepared by dissolving NaCl and sulfonated poly(etheretherketone) (SPEEK) in deionized (DI) H2O at 100 °C. After cooling to room temperature, the solution was filtered and the pH was adjusted to 5.8. A sheet of The 212 membrane was immersed in the PAH polycation solution for 5 minutes and the membrane was rinsed 3 times with deionized (DI) H2O. The membrane was then immersed in the SPEEK polyanion solution for 5 minutes. The membrane was rinsed 3 times with DI H2O and a PAH / SPEEK polyelectrolyte bilayer was deposited on 212 on both surfaces of the membrane. Repeat this process to Three groups of PAH / SPEEK polyelectrolyte double layers were deposited on the two surfaces of the 212 membrane to form (SPEEK-PAH)3 / -212 / (PAH-SPEEK)3 membrane.
[0056] By mixing Pt Black, The cathode catalyst ink was prepared by mixing the ionomer. The mixture was finely dispersed using an ultrasonic bath. The cathode catalyst ink was sprayed onto (SPEEK-PAH) 3 / -212 / (PAH-SPEEK)3 membrane. Pt loading is 0.08 mg / cm 2 .
[0057] By mixing IrO2, poly(3,4-ethylenedioxythiophene) (PEDOT) and poly(styrene sulfonate) (PSS) and The ionomers were mixed in H2O and ethanol to prepare the anode catalyst ink. The weight ratio of ionomer to the blend of PEDOT and PSS was 1.3 / 1. The anode catalyst ink was sprayed on (SPEEK-PAH) 3 / -212 / (PAH-SPEEK)3 membrane to form a three-layer MEA containing PEDOT conductive polymer in the IrO2 anode catalyst coating (referred to as IrO2-PEDOT-1 / M-1 / Pt MEA). The IrO2 loading was 0.8 mg / cm 2 .
[0058] Example 2. Preparation of (SPEEK-PAH) 3 / -212 / (PAH-SPEEK)3 membrane, Three-layer MEA of PEDOT conductive polymer in ionomer and IrO2 anode catalyst coating (abbreviated as IrO2-PEDOT-2 / M-1 / PtMEA)
[0059] The procedure of Example 1 was used to prepare a mixture comprising (SPEEK-PAH)3 / -212 / (PAH-SPEEK)3 membrane, The three-layer MEA of PEDOT conductive polymer in the ionomer and IrO2 anode catalyst coating (abbreviated as IrO2-PEDOT-2 / M-1 / Pt MEA) is different from The weight ratio of ionomer to the blend of PEDOT and PSS is 2.5 / 1. The Pt loading is 0.08 mg / cm 2 , and the IrO2 loading is 0.8 mg / cm 2 .
[0060] Example 3. Preparation comprising FS-990-PK membrane, Three-layer MEA of PEDOT conductive polymer in ionomer and IrO2 anode catalyst coating (abbreviated as IrO2-PEDOT-1 / M-2 / Pt-C)
[0061] Using the procedure of Example 1, a FS-990-PK membrane, The three-layer MEA of PEDOT conductive polymer in the ionomer and IrO2 anode catalyst coating (abbreviated as IrO2-PEDOT-1 / M-2 / Pt-C) is different from that used for the catalyst coating. FS-990-PK membrane, and the cathode catalyst is Pt / C with Pt nanoparticles on a carbon support. The Pt loading is 0.08 mg / cm 2 , and the IrO2 loading is 0.8 mg / cm 2 .
[0062] Comparative Example 1. Preparation of (SPEEK-PAH) 3 / -212 / (PAH-SPEEK)3 membrane, Three-layer MEA with IrO2 anode catalyst coating without PEDOT conductive polymer (abbreviated as IrO2 / M-1 / Pt)
[0063] The procedure of Example 1 was used to prepare a mixture comprising (SPEEK-PAH)3 / -212 / (PAH-SPEEK)3 membrane, Three-layer MEA with IrO2 anode catalyst coating without PEDOT conductive polymer (referred to as IrO2 / M-1 / Pt), except that PEDOT was not used. Pt loading was 0.08 mg / cm 2 , and the IrO2 loading is 0.8 mg / cm 2 .
[0064] Comparative Example 2. Preparation of FS-990-PK membrane, Three-layer MEA with IrO2 anode catalyst coating without PEDOT conductive polymer (referred to as IrO2 / M-2 / Pt-C MEA)
[0065] Using the procedure of Example 1, a FS-990-PK membrane, The three-layer MEA with IrO2 anode catalyst coating without PEDOT conductive polymer (abbreviated as IrO2 / M-2 / Pt-C) is different from that of the membrane used for catalyst coating. FS-990-PK membrane, the cathode catalyst is Pt / C with Pt nanoparticles on a carbon support, and no PEDOT is used. The Pt loading is 0.08 mg / cm 2 , and the IrO2 loading is 0.8 mg / cm 2 .
[0066] Example 4. Evaluation of the water electrolysis performance of IrO2 / M-1 / Pt, IrO2-PEDOT-1 / M-1 / Pt MEA and IrO2-PEDOT-2 / M-1 / PtMEA
[0067] Evaluation using a proton exchange membrane (PEM) water electrolysis test station (Scribner 600 electrolyzer test system)
[0068] IrO2 / M-1 / Pt (a), IrO2-PEDOT-1 / M-1 / Pt (b) and IrO2-PEDOT-2 / M-1 / Pt (c) MEA with an active membrane area of 5 cm 2 The water electrolysis performance in a single electrolyzer cell of . The test station includes an integrated power supply, a potentiostat, an impedance analyzer for electrochemical impedance spectroscopy (EIS) and high frequency resistance (HFR), and real-time sensors for product flow rate and permeation monitoring. The MEA was sandwiched between carbon paper (as cathode PTL) and Pt-Ti felt (as anode PTL). The test was carried out at 80°C and atmospheric pressure. Ultrapure water was supplied to the anode of the MEA at a flow rate of 100 mL / min. Polarization curves were collected at 80°C (each data point was held for 1 minute) and the results are shown in Figure 3The high frequency resistance (HFR) versus current density of a single water electrolysis cell was collected at 80°C and the results are shown in Figure 4 middle.
[0069] from Figure 3 From the polarization curves in Figure 2, it can be observed that IrO2-PEDOT-1 / M-1 / Pt (b) MEA and IrO2-PEDOT-2 / M-1 / Pt (c) MEA both show lower cell voltage than IrO2 / M-1 / Pt (a) MEA without PEDOT conductive polymer at the same current density, especially at ≥2 A / cm 2 at high current density. IrO2-PEDOT-2 / M-1 / Pt(c)MEA with a weight ratio of 2.5 / 1 of ionomer to PEDOT and PSS blends showed a The IrO2-PEDOT-1 / M-1 / Pt(b)MEA with a weight ratio of 1.3 / 1 for the blend of ionomer to PEDOT and PSS showed a greater voltage drop. Figure 4 It can also be seen that both IrO2-PEDOT-1 / M-1 / Pt(b)MEA and IrO2-PEDOT-2 / M-1 / Pt(c)MEA show lower high frequency resistance (HFR) than IrO2 / M-1 / Pt(a)MEA without PEDOT conductive polymer, indicating that IrO2-PEDOT-1 / M-1 / Pt(b)MEA and IrO2-PEDOT-2 / M-1 / Pt(c)MEA containing PEDOT conductive polymer have higher conductivity than IrO2 / M-1 / Pt(a)MEA without PEDOT conductive polymer. These results indicate that IrO2-PEDOT-1 / M-1 / Pt(b)MEA and IrO2-PEDOT-2 / M-1 / Pt(c)MEA containing PEDOT conductive polymer have improved electrolysis performance due to the improved conductivity of the anode catalyst coating.
[0070] Example 5. Evaluation of the water electrolysis performance of IrO2 / M-2 / Pt-C MEA and IrO2-PEDOT-1 / M-2 / Pt-C MEA
[0071] A PEM water electrolysis test station (Scribner 600 electrolyzer test system) was used to evaluate the performance of IrO2 / M-2 / Pt-C (a) MEA and IrO2-PEDOT-1 / M-2 / Pt-C (b) MEA at an active membrane area of 5 cm 2The water electrolysis performance in a single electrolyzer cell of . The test station includes an integrated power supply, a potentiostat, an impedance analyzer for EIS and HFR, and real-time sensors for product flow rate and permeation monitoring. The MEA is sandwiched between two Pt-Ti felts PTL. The test is performed at 90°C and at atmospheric pressure. Ultrapure water is supplied to the anode of the MEA at a flow rate of 100 mL / min. Polarization curves are collected at 90°C (each data point is held for 1 minute) and the results are shown in Figure 5 In. From Figure 5 It can be observed from the polarization curves that the IrO2-PEDOT-1 / M-2 / Pt-C MEA with PEDOT conductive polymer (b) has a high current density (>2.5A / cm 2 ) showed a lower cell voltage than that of IrO2 / M-2 / Pt-C MEA without PEDOT conductive polymer (a), indicating that the electrolysis performance was improved using IrO2-PEDOT-1 / M-2 / Pt-C MEA (b).
[0072] Specific implementation plan
[0073] While the following is described in conjunction with specific embodiments, it should be understood that this description is intended to illustrate and not to limit the scope of the foregoing description and the appended claims.
[0074] A first embodiment of the invention is a catalyst-coated ion-conducting membrane comprising an ion-conducting membrane; and an anode catalyst coating on a first surface of the ion-conducting membrane, or a cathode catalyst coating on a second surface of the ion-conducting membrane, or both; wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer. An embodiment of the invention is one, any, or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the conductive polymer comprises a conductive organic polymer. An embodiment of the invention is one, any, or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the conductive organic polymer comprises poly(3,4-ethylenedioxythiophene) (PEDOT), a blend of PEDOT and polystyrene sulfonate, polyacetylene, polyaniline, polypyrrole, polythiophene, polyparaphenylene, polyparaphenylene vinylene, polyfuran, or a mixture thereof. An embodiment of the invention is one, any, or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the anode catalyst coating or the cathode catalyst coating or both comprise a catalyst, a polymer ionomer, and a conductive polymer. One embodiment of the invention is one, any or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the cathode catalyst comprises platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, nickel, molybdenum, iron, copper, chromium, their alloys, their oxides, their carbides, their phosphides, or combinations thereof. One embodiment of the invention is one, any or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the anode catalyst comprises iridium, platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, copper, nickel, molybdenum, iron, chromium, their alloys, their oxides, their carbides, their phosphides, or combinations thereof. One embodiment of the invention is one, any or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the polymer ionomer comprises a proton conducting fluorinated or non-fluorinated polymer ionomer, or a hydroxide conducting polymer ionomer. One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the ion conducting membrane comprises a proton exchange membrane or an anion exchange membrane. One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the first embodiment in this paragraph, wherein the proton exchange membrane comprises a polyelectrolyte multilayer-coated proton exchange membrane, the polyelectrolyte multilayer-coated proton exchange membrane comprising a cation exchange membrane and a polyelectrolyte multilayer coating on the surface of the cation exchange membrane, wherein the polyelectrolyte multilayer coating comprises alternating layers of polycationic polymer layers and polyanionic polymers, and wherein the polycationic polymer layers are in contact with the cation exchange membrane.
[0075] A second embodiment of the invention is a membrane electrode assembly comprising an ion conducting membrane; a first porous transport layer adjacent to a first side of the ion conducting membrane; and a second porous transport layer adjacent to a second side of the ion conducting membrane; an anode between the first side of the ion conducting membrane and the first porous transport layer, the anode comprising an anode catalyst coating on the first side of the ion conducting membrane adjacent to the first porous transport layer, or on the first side of the first porous transport layer adjacent to the first side of the ion conducting membrane, or both; and a cathode between the second side of the ion conducting membrane and the second porous transport layer, the cathode comprising a cathode catalyst coating on the second side of the ion conducting membrane adjacent to the second porous transport layer, or on the first side of the second porous transport layer adjacent to the second side of the ion conducting membrane, or both; wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer. An embodiment of the invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the conductive polymer comprises a conductive organic polymer. One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the conductive organic polymer comprises poly(3,4-ethylenedioxythiophene) (PEDOT), a blend of PEDOT and polystyrene sulfonate, polyacetylene, polyaniline, polypyrrole, polythiophene, polyparaphenylene, polyparaphenylene vinylene, polyfuran or a mixture thereof. One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the anode catalyst coating or the cathode catalyst coating or both comprise a catalyst, a polymer ionomer and a conductive polymer. One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the cathode catalyst comprises platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, nickel, molybdenum, iron, copper, chromium, alloys thereof, oxides thereof, carbides thereof, phosphides thereof, or combinations thereof. One embodiment of the invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the anode catalyst comprises iridium, platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, copper, nickel, molybdenum, iron, chromium, their alloys, their oxides, their carbides, their phosphides, or combinations thereof. One embodiment of the invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the polymer ionomer comprises a proton conducting fluorinated or non-fluorinated polymer ionomer, or a hydroxide conducting polymer ionomer.One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the ion conducting membrane comprises a proton exchange membrane or an anion exchange membrane. One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, wherein the proton exchange membrane comprises a polyelectrolyte multilayer-coated proton exchange membrane, the polyelectrolyte multilayer-coated proton exchange membrane comprising a cation exchange membrane and a polyelectrolyte multilayer coating on the surface of the cation exchange membrane, wherein the polyelectrolyte multilayer coating comprises alternating layers of polycationic polymer layers and polyanionic polymers, and wherein the polycationic polymer layers are in contact with the cation exchange membrane. One embodiment of the present invention is one, any or all of the previous embodiments in this paragraph to the second embodiment in this paragraph, further comprising a pair of bipolar plates, one plate adjacent to the outside of the first porous transport layer, and one plate adjacent to the outside of the second porous transport layer.
[0076] A third embodiment of the present invention is an electrolysis system comprising at least one cell forming a cell stack, the at least one cell comprising a membrane electrode assembly, wherein the membrane electrode assembly comprises: an ion conductive membrane; a first side of a first porous transport layer adjacent to a first side of the ion conductive membrane; a first side of a second porous transport layer adjacent to a second side of the ion conductive membrane; an anode between the first side of the ion conductive membrane and the first side of the first porous transport layer, the anode comprising an anode catalyst coating on a surface of a first side of the ion conductive membrane adjacent to the first porous transport layer, on the first side of the first porous transport layer adjacent to the first side of the ion conductive membrane, or on both; A cathode between the second side of the ion-conducting membrane and the first side of the second porous transport layer, the cathode comprising a cathode catalyst coating on the second side of the ion-conducting membrane adjacent to the second porous transport layer, or on the first side of the second porous transport layer adjacent to the second side of the ion-conducting membrane, or on both; wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer; a pair of bipolar plates, the first bipolar plate being adjacent to the second side of the first porous transport layer, and the second side of the second bipolar plate being adjacent to the outer side of the second porous transport layer; and a pair of current collectors, the first current collector being adjacent to the first end of the battery stack, and the second current collector being adjacent to the second end of the battery stack.
[0077] Although there is no further detailed description, it is believed that those skilled in the art can utilize the present invention to the greatest extent by using the foregoing description and can easily determine the essential characteristics of the present invention without departing from the spirit and scope of the present invention to make various changes and modifications of the present invention and adapt it to various usages and conditions. Therefore, the aforementioned preferred specific embodiments should be understood as merely illustrative and not to limit the rest of the present disclosure in any way, and are intended to cover various modifications and equivalent arrangements included within the scope of the appended claims.
[0078] In the foregoing, all temperatures are set forth in degrees Celsius and all parts and percentages are by weight unless otherwise indicated.
Claims
1. A catalyst-coated ion-conducting membrane, include: Ion conducting membranes; and an anode catalyst coating on the first surface of the ion conducting membrane, or a cathode catalyst coating on the second surface of the ion conducting membrane, or both; wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer.
2. The catalyst coated ion conducting membrane of claim 1, wherein the conductive polymer comprises a conductive organic polymer.
3. The catalyst-coated ion-conducting membrane of claim 2, wherein the conductive organic polymer comprises poly(3,4-ethylenedioxythiophene) (PEDOT), a blend of PEDOT and polystyrene sulfonate, polyacetylene, polyaniline, polypyrrole, polythiophene, polyparaphenylene, polyparaphenylene vinylene, polyfuran, or a mixture thereof.
4. The catalyst coated ion conducting membrane of claim 1, wherein the anode catalyst coating or the cathode catalyst coating or both comprise a catalyst, a polymer ionomer and the conductive polymer.
5. The catalyst-coated ion-conducting membrane of claim 1, wherein the cathode catalyst comprises platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, nickel, molybdenum, iron, copper, chromium, alloys thereof, oxides thereof, carbides thereof, phosphides thereof, or combinations thereof.
6. The catalyst-coated ion-conducting membrane of claim 1, wherein the anode catalyst comprises iridium, platinum, ruthenium, osmium, rhodium, palladium, tin, tungsten, vanadium, cobalt, silver, gold, copper, nickel, molybdenum, iron, chromium, alloys thereof, oxides thereof, carbides thereof, phosphides thereof, or combinations thereof.
7. The catalyst coated ion conducting membrane of claim 4, wherein the polymer ionomer comprises a proton conducting fluorinated or non-fluorinated polymer ionomer, or a hydroxide conducting polymer ionomer.
8. The catalyst coated ion conducting membrane of claim 1, wherein the ion conducting membrane comprises a proton exchange membrane or an anion exchange membrane.
9. A catalyst-coated ion-conducting membrane according to claim 8, wherein the proton exchange membrane comprises a polyelectrolyte multilayer-coated proton exchange membrane, the polyelectrolyte multilayer-coated proton exchange membrane comprising a cation exchange membrane and a polyelectrolyte multilayer coating on the surface of the cation exchange membrane, wherein the polyelectrolyte multilayer coating comprises alternating layers of polycationic polymer layers and polyanionic polymers, and wherein the polycationic polymer layers are in contact with the cation exchange membrane.
10. An electrolysis system, include: at least one battery forming a battery stack, the at least one battery comprising: A membrane electrode assembly, wherein the membrane electrode assembly comprises: Ion conducting membranes; a first side of a first porous transport layer adjacent to the first side of the ion conducting membrane; a first side of a second porous transport layer adjacent to a second side of the ion conducting membrane; an anode between the first side of the ion conducting membrane and the first side of the first porous transport layer, the anode comprising an anode catalyst coating on a surface of a first side of the ion conducting membrane adjacent to the first porous transport layer, on the first side of the first porous transport layer adjacent to the first side of the ion conducting membrane, or on both; and a cathode between the second side of the ion conducting membrane and the first side of the second porous transport layer, the cathode comprising a cathode catalyst coating on the second side of the ion conducting membrane adjacent to the second porous transport layer, on the first side of the second porous transport layer adjacent to the second side of the ion conducting membrane, or both; wherein the anode catalyst coating or the cathode catalyst coating or both comprise a conductive polymer; a pair of bipolar plates, a first bipolar plate adjacent to the second side of the first porous transport layer and a second bipolar plate adjacent to the second side of the second porous transport layer; and A pair of current collectors, a first current collector adjacent a first end of the battery stack and a second current collector adjacent a second end of the battery stack.
Citation Information
Cited By
Coating type catalyst composite PEM electrolytic cell gas diffusion layer and preparation method thereof
CN122235752A