Laminate, battery case for nonaqueous electrolyte secondary battery, and battery for nonaqueous electrolyte secondary battery
By adopting a laminated structure in the battery case, combining the flame retardant layer and the fiber-reinforced resin layer, the problem of difficult to take into account both the flame retardant and mechanical properties in the fiber-reinforced resin is solved, and the high flame retardant and impact resistance of the battery case is achieved .
Patent Information
- Application Number
- CN202380034794.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-02-16
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult to obtain sufficient flame retardant and mechanical properties by adding flame retardant to the conventional fiber reinforced resin, and mechanical properties may be reduced after the flame retardant is improved.
The laminated structure is adopted, including a flame retardant layer and a fiber reinforced resin layer. The flame retardant layer contains 20% to 80% thermoplastic resin and 20% to 80% flame retardant, and the fiber reinforced resin layer contains 30% to 90% thermoplasticity. The resin and 10% to 70% reinforcing fibers are preferably used in the fiber-reinforced resin layer. The content of the reinforcing fiber is more than 10% larger than the flame retardant layer, and the flame retardant content is controlled in the fiber-reinforced resin layer. 0%~20%.
It achieves dual excellence of flame retardancy and mechanical properties (impact resistance), ensuring high flame retardancy and good mechanical properties.
Smart Images

Figure BDA0005089935490000261 
Figure BDA0005089935490000271 
Figure BDA0005089935490000301
Abstract
Description
Technical Field
[0001] The present invention relates to a laminate, a battery case for a non-aqueous electrolyte secondary battery, and a battery for the non-aqueous electrolyte secondary battery. Background Art
[0002] In order to reduce CO2 emissions during vehicle driving and increase the driving distance of electric vehicles, vehicles are required to be lighter than ever before. From the perspective of improving weight reduction, it is possible to reduce the metal used in battery packs and battery modules or to convert the used materials into resin.
[0003] On the other hand, electric vehicles are required to be safer than ever before. For example, various storage batteries, such as lithium batteries, may catch fire due to internal short circuits, overcharging, penetration of foreign objects, external overheating, abnormal heating, etc.
[0004] As a vehicle battery case formed of a carbon fiber reinforced polypropylene resin having both flame retardancy and electromagnetic wave shielding properties and excellent mechanical properties, for example, Patent Document 1 discloses a vehicle battery case, characterized in that it is formed by molding a carbon fiber reinforced polypropylene resin composition prepared by blending 8 to 70 parts by weight of carbon fibers (B) and 0.6 to 37.5 parts by weight of a flame retardant (C) relative to 100 parts by weight of a polypropylene resin (A), and the weight average fiber length of the carbon fibers in the molded product is greater than 0.5 mm and less than 3 mm.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2014-62189 Summary of the invention
[0008] Problems to be solved by the invention
[0009] According to the research of the inventor of the present application, if a flame retardant is added to a fiber-reinforced material (fiber-reinforced resin), the improvement of flame retardancy is suppressed compared to the case where a flame retardant is added to a resin that is not fiber-reinforced, and it is difficult to obtain sufficient flame retardancy. In addition, with regard to the battery case described in Patent Document 1, although the flame retardancy of the battery case for a vehicle is improved, the flame retardancy is not sufficient, and further improvement of the flame retardancy is required.
[0010] An object to be solved by one embodiment of the present invention is to provide a laminate having excellent flame retardancy despite containing reinforcing fibers, a battery case for a nonaqueous electrolyte secondary battery, and a battery for a nonaqueous electrolyte secondary battery having the same.
[0011] Means for solving problems
[0012] Means for solving the above-mentioned problems include the following.
[0013] <1> A laminate comprising a flame retardant layer and a fiber reinforced resin layer,
[0014] The flame retardant layer contains 20% to 80% by mass of a thermoplastic resin relative to the total mass of the flame retardant layer, and 20% to 80% by mass of a flame retardant relative to the total mass of the flame retardant layer, wherein the flame retardant is at least one selected from the group consisting of a phosphorus flame retardant, a bromine flame retardant, and an inorganic hydrate flame retardant, and the content of the reinforcing fiber is 0% to 20% by mass relative to the total mass of the flame retardant layer.
[0015] The fiber-reinforced resin layer contains 30 to 90% by mass of a thermoplastic resin based on the total mass of the fiber-reinforced resin layer and 10 to 70% by mass of reinforcing fibers based on the total mass of the fiber-reinforced resin layer.
[0016] <2> like <1> The laminated body, wherein the content of the reinforcing fibers contained in the fiber-reinforced resin layer is greater than the content of the reinforcing fibers contained in the flame-retardant layer by 10% by mass or more.
[0017] <3> like <1> or <2> The laminate, wherein the content of the flame retardant in the fiber-reinforced resin layer is greater than or equal to 0% by mass and less than 20% by mass relative to the total mass of the fiber-reinforced resin layer, and the flame retardant is at least one selected from the group consisting of phosphorus-based flame retardants, bromine-based flame retardants and inorganic hydrate-based flame retardants.
[0018] <4> like <1> ~ <3> The laminate according to any one of the preceding claims, wherein the flame-retardant layer contains 40% by mass to 80% by mass of the flame retardant relative to the total mass of the flame-retardant layer.
[0019] The fiber-reinforced resin layer contains 40% to 60% by mass of the reinforcing fiber relative to the total mass of the fiber-reinforced resin layer, and the content of the flame retardant is 0% to 10% by mass relative to the total mass of the fiber-reinforced resin layer, and the flame retardant is at least one selected from the group consisting of phosphorus-based flame retardants, bromine-based flame retardants and inorganic hydrate-based flame retardants.
[0020] <5> like <1> ~ <4> The laminated body described in any one of the preceding claims, wherein the fiber-reinforced resin layer contains at least one resin selected from the group consisting of polypropylene resins and polyamide resins as the thermoplastic resin.
[0021] <6> like <1> ~ <5> The laminated body described in any one of the above aspects, wherein the reinforcing fibers include at least one type of fiber selected from the group consisting of carbon fibers and glass fibers.
[0022] <7> like <1> ~ <6> The laminated body described in any one of the above-mentioned fiber-reinforced resin layer and the above-mentioned flame-retardant layer contains an electromagnetic wave shielding filler.
[0023] <8> like <1> ~ <7> The laminated body described in any one of the above aspects, wherein the fiber-reinforced resin layer has a thickness of 0.5 to 30 mm.
[0024] <9> Battery case for non-aqueous electrolyte secondary battery, which is used <1> ~ <8> The invention is formed by the laminated body described in any one of the above.
[0025] <10> like <9> In the battery case for a non-aqueous electrolyte secondary battery, the flame retardant layer in the laminate is arranged on the inner side of the battery case.
[0026] <11> like <9> In the battery case for a non-aqueous electrolyte secondary battery, the flame retardant layer in the laminate is arranged on the inner side and the outer side of the battery case.
[0027] <12> like <9> ~ <11> The battery case for a nonaqueous electrolyte secondary battery described in any one of the above aspects further includes an electromagnetic wave shielding layer.
[0028] <13> A battery for a non-aqueous electrolyte secondary battery, comprising <9> ~ <12> The battery case for a non-aqueous electrolyte secondary battery described in any one of the above.
[0029] Effects of the Invention
[0030] According to one embodiment of the present invention, there are provided a laminate having excellent flame retardancy despite containing reinforcing fibers, a battery case for a nonaqueous electrolyte secondary battery, and a battery for a nonaqueous electrolyte secondary battery including the same. DETAILED DESCRIPTION
[0031] Hereinafter, the contents of the present invention will be described in detail. The contents of the constituent elements described below may be described based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.
[0032] In this specification, the term "polymer" is a concept including homopolymers and copolymers.
[0033] In the present specification, "to" indicating a numerical range is used to mean that the numerical values described before and after it are included as the lower limit and the upper limit.
[0034] In the present specification, "to" indicating a numerical range means that the units described before and after it represent the same unit unless otherwise specified.
[0035] In the present specification, a combination of two or more preferred aspects is a more preferred aspect.
[0036] In the present specification, when a plurality of substances belonging to each component are present in each layer, the amount of each component in each layer refers to the total amount of the plurality of substances present in each layer unless otherwise specified.
[0037] Hereinafter, the present invention will be described in detail.
[0038] (Laminated body)
[0039] The laminated body according to the present invention comprises a flame-retardant layer and a fiber-reinforced resin layer, the flame-retardant layer contains 20% to 80% by mass of a thermoplastic resin relative to the total mass of the flame-retardant layer, and 20% to 80% by mass of a flame retardant relative to the total mass of the flame-retardant layer, wherein the flame retardant is at least one selected from the group consisting of a phosphorus-based flame retardant, a bromine-based flame retardant, and an inorganic hydrate-based flame retardant, and the content of the reinforcing fiber is 0% to 20% by mass relative to the total mass of the flame-retardant layer, the fiber-reinforced resin layer contains 30% to 90% by mass of a thermoplastic resin relative to the total mass of the fiber-reinforced resin layer, and 10% to 70% by mass of the reinforcing fiber relative to the total mass of the fiber-reinforced resin layer.
[0040] Since the laminate according to the present invention has the above-mentioned structure, it is excellent in flame retardancy and also excellent in impact strength despite the inclusion of reinforcing fibers. The reason for this is not clear, but it is presumed as follows.
[0041] When a flame retardant is added to a resin containing reinforcing fibers (i.e., fiber-reinforced resin), it is difficult to obtain a sufficient flame retardant effect because heat is conducted along the reinforcing fibers (candle effect) when the thermoplastic resin is melted, compared with a resin not containing reinforcing fibers. In addition, when a large amount of flame retardant is added to a fiber-reinforced resin in order to improve flame retardancy, there is a concern that the mechanical properties (impact resistance) of the resulting molded body may be reduced.
[0042] It is inferred that in the laminate according to the present invention, the flame retardant effect can be further improved by adjusting the content of the above-mentioned reinforcing fiber in the flame retardant layer to 0 to 20% by mass, and high mechanical properties are ensured by having a fiber-reinforced resin layer containing a thermoplastic resin and reinforcing fibers, thereby the laminate has excellent flame retardancy despite containing reinforcing fibers. In addition, it is inferred that since the laminate according to the present invention has a flame retardant layer and a fiber-reinforced resin layer having the above-mentioned structure, both flame retardancy and mechanical properties are excellent.
[0043] Hereinafter, each structure of the laminate will be described in detail.
[0044] <Flame retardant layer>
[0045] The laminated body according to the present invention has a flame retardant layer. The flame retardant layer is a layer containing a thermoplastic resin and a flame retardant. The flame retardant layer contains at least one flame retardant selected from the group consisting of a phosphorus flame retardant, a bromine flame retardant and an inorganic hydrate flame retardant. As the flame retardant, from the viewpoint of further improving the flame retardancy of the laminated body, preferably a phosphorus flame retardant and a bromine flame retardant, more preferably a phosphorus flame retardant.
[0046] <<Phosphorus flame retardants>>
[0047] The phosphorus-based flame retardant is not particularly limited as long as it contains a phosphorus atom in its structural formula. When the phosphorus-based flame retardant is a salt, it only needs to contain a phosphorus atom in the structural formula of at least one of the anion component and the cationic component.
[0048] As the phosphorus flame retardant, for example, phosphate compounds, phosphazene compounds, polyphosphate compounds, phosphate compounds, phosphinates, phosphonic acid compounds, phosphine oxide compounds, phosphite compounds, phosphite compounds, phosphite monoester compounds, phosphine compounds, phosphine compounds, phenanthroline compounds, red phosphorus, etc. Among them, polyphosphate compounds, phosphinates and red phosphorus are preferred, and polyphosphate compounds are particularly preferred.
[0049] Examples of the polyphosphate compound include ammonium polyphosphate, melamine polyphosphate, melamine-melam-melem polyphosphate, and ammonium polyphosphate.
[0050] The phosphorus-based flame retardant may be used alone or in combination of two or more.
[0051] The decomposition temperature of the phosphorus-based flame retardant is preferably within a range of 100°C to 500°C, more preferably within a range of 200°C to 470°C, and still more preferably within a range of 250°C to 450°C.
[0052] In the above-mentioned method for measuring the decomposition temperature, the mass of the sample is measured while the temperature is raised at a certain temperature (e.g., +10°C per minute) to 700°C in a thermogravimetric measuring apparatus (TGA), and the mass (Td5) at which the sample mass decreases by 5% by weight from the mass at the start of the measurement is read. The 5% weight reduction temperature (Td5) is determined as the decomposition temperature.
[0053] The reason why the flame retardant layer contains a phosphorus-based flame retardant as a flame retardant is not clear, but the inventors of the present application speculate that this is because the charred layer formed by thermal decomposition of the phosphorus-based flame retardant shields the heat directed to the fiber reinforcement layer, thereby inhibiting the candle effect of the reinforcing fibers.
[0054] <<Brominated flame retardants>>
[0055] As the brominated flame retardant, an organic compound containing bromine is preferred, for example, ethylenebis(pentabromobiphenyl), hexabromobenzene, tetrabromobisphenol S, hexabromocyclododecane (HBCD), tetrabromobisphenol A (TBBA), TBBA epoxide oligomers or polymers, TBBA-bis(2,3-dibromopropyl ether), dibromoethyl-dibromocyclohexane, dibromoneopentyl glycol, tribromophenol, tribromophenol allyl ether, pentabromophenol, pentabromotoluene, hexabromodiphenyl ether, dibromoneopentyl glycol tetracarbonate, N-methylhexabromophenylamine, etc.
[0056] Among them, ethylenebis(pentabromobiphenyl) is preferred.
[0057] The brominated flame retardants may be used alone or in combination of two or more.
[0058] <<Inorganic Hydrate Flame Retardant>>
[0059] As the inorganic hydrate flame retardant, magnesium hydroxide, aluminum hydroxide, aluminum oxide (hydrate), zinc borate, hydrotalcite, dawsonite, calcium aluminate, kaolinite clay, etc. can be cited. Among them, as the inorganic hydrate flame retardant, magnesium hydroxide and aluminum hydroxide are preferred from the aspect of being able to take into account both flame retardancy and cost.
[0060] The inorganic hydrate-based flame retardant may be used alone or in combination of two or more.
[0061] From the viewpoint of improving flame retardancy, the flame-retardant layer may contain a flame retardant other than the above-mentioned phosphorus-based flame retardant, bromine-based flame retardant, and inorganic hydrate-based flame retardant (hereinafter also referred to as “other flame retardant”).
[0062] Other flame retardants include metal oxides such as zinc oxide, calcium oxide, barium oxide, aluminum oxide, tin oxide, and magnesium oxide; antimony compounds such as antimony trioxide, antimony tetroxide, antimony pentoxide, and sodium antimonate; zinc compounds such as zinc stannate and zinc phosphate; silicone-based flame retardants; and sulfur-based flame retardants.
[0063] The flame retardant layer contains 20 to 80 mass % of at least one flame retardant selected from the group consisting of phosphorus-based flame retardants, bromine-based flame retardants and inorganic hydrate-based flame retardants, preferably 40 to 80 mass % based on the total mass of the flame retardant layer.
[0064] In addition, in the flame retardant layer, the content of the reinforcing fiber described later is 0% to 20% by mass relative to the total mass of the flame retardant layer, preferably 0% to 5% by mass, more preferably 0% to 3% by mass, and particularly preferably 0% by mass (i.e., excluding reinforcing fibers). If the content of the reinforcing fiber in the flame retardant layer is within the above range, there is a tendency for the flame retardancy of the laminate to be improved.
[0065] On the other hand, when the flame retardant layer does not contain reinforcing fibers, the difference in molding shrinkage between the flame retardant layer and the fiber reinforced resin layer becomes larger. Therefore, when the laminate is molded by, for example, two-color molding, warping of the molded body may be easily generated. In this case, although it can also be dealt with by adjusting the molding conditions, it is preferred that the fiber reinforced resin layer contains more reinforcing fibers on the basis of containing a certain degree of reinforcing fibers in the flame retardant layer. In this case, the content of reinforcing fibers in the flame retardant layer is preferably 5% to 20% by mass relative to the total mass of the flame retardant layer.
[0066] <<Thermoplastic resin>>
[0067] The flame-retardant layer contains 20% to 80% by mass of the thermoplastic resin, preferably 20% to 60% by mass of the thermoplastic resin, based on the total mass of the flame-retardant layer.
[0068] The thermoplastic resin contained in the flame-retardant layer is the same as the thermoplastic resin contained in the fiber-reinforced resin layer described later, and the preferred aspects are also the same.
[0069] The flame retardant layer may further contain resins other than the above-mentioned thermoplastic resins. Examples of the resins other than the thermoplastic resins include thermosetting resins, such as epoxy resins, thermosetting unsaturated polyester resins, and phenolic resins.
[0070] The content of the resin other than the thermoplastic resin in the flame-retardant layer is preferably 0 to 10% by mass, more preferably 0 to 5% by mass, and even more preferably 0 to 3% by mass, based on the total mass of the flame-retardant layer.
[0071] The thickness of the flame retardant layer is preferably 0.1 to 30 mm, more preferably 0.3 to 20 mm, and even more preferably 0.5 to 10 mm. The thickness of the flame retardant layer can be appropriately adjusted depending on the application and the flame retardancy required.
[0072] In the present invention, the flame retardant layer contains 20% to 80% by mass of a thermoplastic resin. Therefore, it is believed that the content of the flame retardant can be increased compared to the case where the thermosetting resin is included in the same content as the thermoplastic resin, and the flame retardancy of the obtained laminate can be further improved. It should be noted that when the flame retardant layer contains a thermosetting resin, if the content of the flame retardant in the flame retardant layer increases, the thermosetting resin is prone to reduce toughness due to crosslinking, and the mechanical properties are easily reduced.
[0073] <Fiber-reinforced resin layer>
[0074] The laminated body according to the present invention comprises a fiber-reinforced resin layer. The fiber-reinforced resin layer is a layer containing a thermoplastic resin and reinforcing fibers.
[0075] <<Thermoplastic resin>>
[0076] Examples of thermoplastic resins include polycarbonate, styrene resins, polyamide resins, polyester resins, polyphenylene sulfide (PPS resin), modified polyphenylene ether (modified P PE resin), polyacetal (POM resin), liquid crystal polyester, polyarylate, acrylic resins such as polymethyl methacrylate resin (PMMA), vinyl chloride, polyimide (PI), polyamideimide (PAI), polyetherimide (PEI), polysulfone, polyethersulfone, polyketone, polyetherketone, polyetheretherketone (PEEK), polyethylene, polypropylene and other polyolefin resins, modified polyolefin resins, phenolic resins, phenoxy resins, and the like.
[0077] Among them, from the viewpoint of light weight and excellent flame retardancy, the thermoplastic resin included in the flame retardant layer is preferably at least one resin selected from the group consisting of acrylic resin, polyolefin resin, polyamide resin and polyester resin, more preferably at least one resin selected from the group consisting of polyamide resin, polyethylene and polypropylene resin, and particularly preferably polyamide resin and / or polypropylene resin. These thermoplastic resins can be derived from fossil fuels or from biomass raw materials.
[0078] From the viewpoint of excellent flame retardancy and impact resistance, the thermoplastic resin contained in the fiber-reinforced resin layer is preferably at least one resin selected from the group consisting of acrylic resins, polyolefin resins, polyamide resins and polyester resins, more preferably at least one resin selected from the group consisting of polyamide resins, polyethylene and polypropylene resins, and particularly preferably polyamide resins and / or polypropylene resins.
[0079] -Polypropylene resin-
[0080] The polypropylene resin may be an unmodified polypropylene resin or a polypropylene resin containing a carboxylic acid structure or a carboxylate structure by modification or the like. When both an unmodified resin and a polypropylene resin containing a carboxylic acid structure or a carboxylate structure are used, the preferred mass ratio thereof is 99 / 1 to 80 / 20, more preferably 98 / 2 to 85 / 15, and even more preferably 97 / 3 to 90 / 10 in terms of the unmodified form / modified form ratio.
[0081] The polypropylene resin includes, for example, homopolypropylene, random polypropylene, block polypropylene, and a propylene-based polymer called modified polypropylene.
[0082] The polypropylene resin is a polymer containing a structural unit derived from propylene, and is preferably a copolymer containing a structural unit derived from propylene and a structural unit derived from at least one olefin other than propylene selected from the group consisting of α-olefins, conjugated dienes, and non-conjugated dienes.
[0083] Examples of α-olefins include α-olefins having 2 to 20 carbon atoms other than propylene, such as ethylene, 1-butene, 3-methyl-1-butene, 4-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 1-nonene, 1-octene, 1-heptene, 1-hexene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. Among them, 1-butene, ethylene, 4-methyl-1-pentene, and 1-hexene are preferred, and 1-butene and 4-methyl-1-pentene are more preferred.
[0084] Examples of the conjugated diene and the non-conjugated diene include butadiene, ethylidene norbornene, dicyclopentadiene, and 1,5-hexadiene.
[0085] Two or more α-olefins, conjugated dienes and non-conjugated dienes may be used in combination. Among them, the propylene resin is preferably a copolymer of propylene and α-olefin. Examples of the copolymer include ethylene·propylene copolymer, propylene·1-butene copolymer, ethylene·propylene·1-butene copolymer, and the like.
[0086] The propylene, α-olefin, conjugated diene and non-conjugated diene contained in the polypropylene resin may be derived from fossil fuels or biomass raw materials.
[0087] From the viewpoint of improving the mechanical properties of the obtained laminate, the ratio of the structural units derived from propylene in the polypropylene resin is preferably 50 to 100 mol %, more preferably 60 to 100 mol %, particularly preferably 70 to 100 mol % relative to all structural units of the polypropylene resin.
[0088] The polypropylene resin may have a structure containing, for example, an element of Groups 15 to 17 of the periodic table. Examples of the structure containing an element of Groups 15 to 17 of the periodic table include functional groups such as carboxylic anhydride groups, carboxylic acid groups, amino groups, amide groups, and halogen groups.
[0089] Such a structure can be introduced by known methods such as free radical grafting reaction. Examples of group 17 elements include halogen atoms such as chlorine atoms. Examples of group 16 elements include oxygen atoms and sulfur atoms, preferably oxygen atoms. Examples of group 15 elements include nitrogen atoms. Among them, oxygen atoms are preferred. That is, the structure containing elements of groups 15 to 17 of the periodic table can be preferably a carboxylic acid (salt). The carboxylic acid (salt) is preferably a carboxylic acid group or a carboxylic anhydride group, more preferably a group having a maleic anhydride structure.
[0090] When the polypropylene resin has a structure containing an element of Groups 15 to 17 of the periodic table, the content of the element is preferably 0.0003 to 5% by mass, more preferably 0.0005 to 4.5% by mass, further preferably 0.0008 to 4.3% by mass, particularly preferably 0.001 to 4% by mass, based on the total mass of the polypropylene resin.
[0091] The above content can be calculated from the input ratio of each component in the graft reaction, for example, or can be determined using an elemental analyzer (for example, varioELIII model: manufactured by Elementar).
[0092] The polypropylene resin preferably contains an unmodified polypropylene resin and an acid-modified polypropylene resin.
[0093] The melt flow rate (MFR) of the polypropylene resin measured at 230° C. and a load of 2.16 kg is usually 3 to 100 g / 10 minutes, preferably 15 to 100 g / 10 minutes.
[0094] MFR can be determined by the measuring method described in Examples below.
[0095] The fiber-reinforced resin layer contains 30 to 90 mass % of the thermoplastic resin, preferably 30 to 80 mass % and more preferably 35 to 60 mass % of the thermoplastic resin, based on the total mass of the fiber-reinforced resin layer.
[0096] The fiber-reinforced resin layer may further contain resins other than the above-mentioned thermoplastic resins. Examples of the resins other than the thermoplastic resins include thermosetting resins, such as epoxy resins, thermosetting unsaturated polyester resins, and phenolic resins.
[0097] The content of resins other than the thermoplastic resin in the fiber-reinforced resin layer is preferably 0 to 10% by mass, more preferably 0 to 5% by mass, and even more preferably 0 to 3% by mass, based on the total mass of the fiber-reinforced resin layer.
[0098] In particular, when the resin other than the thermoplastic resin is a thermosetting resin, it is more preferable to substantially not contain any of the above-mentioned thermoplastic resins from the viewpoint of suppressing the reduction of mechanical properties caused by the reduction of toughness due to crosslinking. It should be noted that the term "substantially not containing" means that components that are inevitably mixed are allowed.
[0099] <<Reinforcement Fiber>>
[0100] Examples of the reinforcing fibers include carbon fibers, glass fibers, aramid fibers, alumina fibers, silicon carbide fibers, and boron fibers. From the perspective of improving the impact strength of the laminate, the reinforcing fibers preferably include at least one fiber selected from the group consisting of carbon fibers and glass fibers.
[0101] <<Carbon Fiber>>
[0102] As the carbon fiber, various known carbon fibers can be used. As the carbon fiber, for example, polyacrylonitrile-based, rayon-based, asphalt-based, polyvinyl alcohol-based, regenerated cellulose-based, asphalt-based carbon fibers produced from mesophase asphalt, etc. can be cited. The carbon fiber can be a general-purpose fiber or a high-strength fiber. In addition, the carbon fiber can be a long fiber, a short fiber, and a regenerated fiber.
[0103] <<Fiberglass>>
[0104] The glass fiber is not particularly limited, and examples thereof include fibers composed of glass compositions such as glass A, glass C, glass D, glass E, and glass S. Among these, fibers composed of a glass composition of glass E (alkali-free glass) are particularly preferred.
[0105] The reinforcing fibers may be short fibers or long fibers. The short fibers may be short fibers in the form of chopped fibers (cut fibers) or short fibers in the form of pulp having fibrils. In addition, the reinforcing fibers may be single fibers or fibers formed by twisting a plurality of single fibers.
[0106] The average fiber length of the reinforcing fibers is preferably 0.01 mm or more, more preferably 0.1 mm or more, further preferably 1 mm or more, preferably 100 mm or less, more preferably 50 mm or less, further preferably 30 mm or less. When the average fiber length is within the above range, the reinforcing effect of the mechanical properties by the reinforcing fibers tends to be fully exhibited, and the dispersibility of the reinforcing fibers in the fiber-reinforced resin layer is improved, so the appearance tends to be improved.
[0107] The ratio of the number of fibers having a fiber length of less than 0.1 mm to the total number of reinforcing fibers is preferably 18% or less.
[0108] The average fiber diameter of the reinforcing fibers is preferably 1 μm or more, more preferably 5 μm or more, preferably 30 μm or less, more preferably 20 μm or less. In this manner, the reinforcing fibers are less likely to be damaged during molding, and the impact strength of the resulting molded body tends to be higher. In addition, the appearance of the molded body becomes better, and a sufficient reinforcing effect can be obtained in terms of mechanical properties such as rigidity and heat resistance of the molded body.
[0109] The average fiber length and average fiber diameter can be obtained, for example, by photographing the reinforcing fibers using an optical microscope, measuring the lengths or diameters of 100 reinforcing fibers randomly selected from the obtained photograph, and calculating the arithmetic average of the lengths or diameters.
[0110] Among the above, the form of glass fiber can preferably include, for example, a single fiber, a "glass roving" obtained by continuously winding a plurality of twisted fibers, a "chopped strand" obtained by uniformly cutting the average fiber length to 1 to 10 mm, and a "milled fiber" obtained by crushing the average fiber length to about 10 to 500 μm.
[0111] The reinforcing fibers may be fibers that have not been surface treated (hereinafter referred to as "fibers (C0)") or fibers that have been surface treated (hereinafter referred to as "surface-treated fibers (C1)").
[0112] For example, the "surface-treated fiber (C1)" may be a fiber obtained by surface treatment using various sizing agents (hereinafter, "sizing agent-treated fiber (C1A)"). The "sizing agent-treated fiber (C1A)" in most cases comprises the fiber (C0) and a sizing agent coating the fiber (C0).
[0113] Examples of the sizing agent include acrylic sizing agents, urethane sizing agents, acid copolymer sizing agents, etc. Among these, the sizing agent is preferably an acid copolymer sizing agent.
[0114] Here, when the above-mentioned "sizing agent treated fiber (C1A)" is a glass fiber roving obtained by surface treatment with a sizing agent (hereinafter referred to as "sizing agent treated glass fiber roving"), the sizing agent contained in the "sizing agent treated glass fiber roving" is preferably an acid copolymer sizing agent from the viewpoint of sufficiently impregnating the sizing agent treated fiber with the resin component. In addition, an acrylic sizing agent is also one of the preferred sizing agents.
[0115] On the other hand, when the "sizing agent treated fiber (C1A)" is a fiber other than the "sizing agent treated glass fiber roving", for example, a chopped strand bundle obtained by surface treatment with a sizing agent (hereinafter referred to as "sizing agent treated chopped strand bundle"), the sizing agent contained in the "sizing agent treated chopped strand bundle" is not limited to an acid copolymer-based sizing agent, and may also be an acrylic sizing agent, a urethane sizing agent, or the like other than an acid copolymer-based sizing agent.
[0116] Even such a "sizing agent treated chopped strands" containing a sizing agent other than the acid copolymer-based sizing agent is preferred because it can be sufficiently impregnated with the resin component, similarly to the "sizing agent treated chopped strands" containing the acid copolymer-based sizing agent.
[0117] The reinforcing fiber may contain one or more components selected from silane coupling agents, titanate coupling agents, aluminum coupling agents, zirconium coupling agents, borane coupling agents, curing catalysts, lubricants, fillers, thixotropic agents, tackifiers, waxes, heat stabilizers, light stabilizers, fluorescent whitening agents, foaming agents, pH adjusters, leveling agents, gelation inhibitors, dispersion stabilizers, antioxidants, free radical scavengers, heat resistance imparting agents, inorganic fillers, organic fillers, plasticizers, reinforcing agents, antibacterial agents, mildew inhibitors, rust inhibitors, thermoplastic resins, thermosetting resins, pigments, dyes, conductivity imparting agents, antistatic agents, moisture permeability enhancers, hydrophobic agents, oleophobic agents, hollow foams, compounds containing crystal water, flame retardants, water absorbents, moisture absorbents, deodorants, foam stabilizers, defoamers, mildew inhibitors, preservatives, algae inhibitors, pigment dispersants, antiblocking agents, and anti-hydrolysis agents.
[0118] Examples of the surface treatment method of the reinforcing fibers using a sizing agent include a method of applying the sizing agent to the surface of the reinforcing fibers using an applicator or the like, a method of immersing the reinforcing fibers in the sizing agent, a method of spraying the sizing agent onto the reinforcing fibers, and a method of contacting the reinforcing fibers with a roll to which the sizing agent is applied. The surface treatment method may be either a batch method or a continuous method.
[0119] When the reinforcing fiber is surface treated with a sizing agent, the mass ratio of the sizing agent in the reinforcing fiber, i.e., the ignition loss, is preferably 0.1 to 1.5% by mass relative to the total mass of the reinforcing fiber. The mass ratio of the sizing agent (ignition loss) is measured for the fiber obtained by applying the sizing agent to the reinforcing fiber using, for example, an applicator, and completely volatilizing the volatile substances by drying. When the ignition loss of the sizing agent applied to the surface of the carbon fiber or glass fiber is 0.1% by mass or more, the interface between the above-mentioned resin and the reinforcing fiber can be stabilized and heat resistance can be exhibited, so it is preferred. On the other hand, when the ignition loss of the sizing agent applied to the surface of the reinforcing fiber is 1.5% by mass or less, it can be confirmed that the physical properties such as heat resistance are improved, so it is preferred.
[0120] The ignition loss of the sizing agent in the reinforcing fiber is a value measured in accordance with JIS R 3420 (2006) 7.3.2.
[0121] After the surface-treated reinforcing fibers are bundled and wound in a predetermined number, they can be cut and / or crushed as necessary to be processed into chopped strands, milled fibers, yarns, rovings, and the like.
[0122] The fiber-reinforced resin layer may further contain fibers other than the reinforcing fibers (hereinafter also referred to as “other fibers”) as long as the effects of the present invention can be achieved.
[0123] As other fibers, for example, natural fibers such as cotton fibers, silk fibers, wood fibers, and cellulose fibers can be cited; synthetic fibers formed from synthetic resins such as wholly aromatic polyamides (aramids), wholly aromatic polyesters, wholly aromatic polyester amides, wholly aromatic polyethers, wholly aromatic polycarbonates, wholly aromatic polyazomethines, polyphenylene sulfide, poly(p-phenylene benzobisoxazole), poly(p-phenylene benzobisthiazole), polybenzimidazole, polyetheretherketone, polyamideimide, polyimide, polytetrafluoroethylene, polyvinyl alcohol, polyolefins, polyarylates, and fluorine-based polymers.
[0124] The fiber-reinforced resin layer may contain any additives as necessary in addition to the reinforcing fibers and the thermoplastic resin.
[0125] As arbitrary additives, for example, nucleating agents, anti-caking agents, pigments, fillers, fillers, dyes, lubricants, plasticizers, release agents, antioxidants, ultraviolet absorbers, antibacterial agents, surfactants, antistatic agents, weathering stabilizers, heat stabilizers, anti-slip agents, crystallization aids, anti-corona agents, anti-aging agents, hydrochloric acid absorbers, impact modifiers, crosslinking agents, co-crosslinking agents, crosslinking aids, adhesives, softeners, processing aids, etc. can be cited.
[0126] These additives may be used alone or in combination of two or more.
[0127] The content of the reinforcing fibers contained in the fiber-reinforced resin layer is preferably greater than the content of the reinforcing fibers contained in the flame-retardant layer by 10% by mass or more, and more preferably greater than the content of the reinforcing fibers contained in the flame-retardant layer by 20% by mass or more.
[0128] The fiber-reinforced resin layer contains 10% to 70% by mass of reinforcing fibers relative to the total mass of the fiber-reinforced resin layer, preferably contains 20% to 60% by mass of reinforcing fibers relative to the total mass of the fiber-reinforced resin layer, and more preferably contains 40% to 60% by mass of reinforcing fibers relative to the total mass of the fiber-reinforced resin layer.
[0129] In addition, from the viewpoint of sufficiently improving the impact resistance of the laminate, the content of the flame retardant in the fiber-reinforced resin layer is preferably 0% by mass or more and less than 20% by mass, more preferably 0% by mass to 10% by mass, further preferably 0% by mass to 5% by mass, and particularly preferably 0% by mass to 3% by mass, relative to the total mass of the fiber-reinforced resin layer.
[0130] The density of the fiber-reinforced resin layer is preferably 0.9 to 1.8 g / cm 3 , more preferably 1.0 to 1.7 g / cm 3 .
[0131] The density of the fiber-reinforced resin layer can be determined by the measuring method described in Examples below.
[0132] The thickness of the fiber-reinforced resin layer is preferably 0.5 to 30 mm, more preferably 1.0 to 20 mm, further preferably 2.0 to 10 mm, and particularly preferably 3.0 to 10 mm. If the thickness of the fiber-reinforced resin layer is above the lower limit, the warping of the laminate can be suppressed, and there is a tendency for the impact strength to be further improved. In addition, if the thickness of the fiber-reinforced resin layer is below the upper limit, there is a tendency for excellent formability. The thickness of the fiber-reinforced resin layer can be appropriately adjusted according to the application and the mechanical strength required.
[0133] <<Method for forming a fiber-reinforced resin layer>>
[0134] The method for forming the fiber-reinforced resin layer is not particularly limited, and a conventionally known method can be used. For example, a resin can be mixed with the above-mentioned carbon fiber or glass fiber, and extrusion molding, injection molding, vacuum molding, pressure molding, press molding, etc. can be used to form a fiber-reinforced film, a fiber-reinforced sheet, a fiber-reinforced plate, etc. to make a fiber-reinforced resin layer. In addition, a masterbatch-like pellet formed by the above-mentioned reinforcing fiber and thermoplastic resin can be mixed with a thermoplastic resin pellet to form a fiber-reinforced resin layer by injection molding. Alternatively, a mixed felt formed by the above-mentioned reinforcing fiber and thermoplastic resin fiber can be used, and press molding can be performed above the flow starting temperature of the thermoplastic resin fiber to form a fiber-reinforced resin layer.
[0135] <<Electromagnetic wave shielding filler>>
[0136] From the perspective of preventing electromagnetic wave noise generated by lithium-ion batteries and the like from leaking to the outside, the fiber-reinforced resin layer or the flame-retardant layer may contain an electromagnetic wave shielding filler. From the perspective of simultaneously achieving the mechanical properties and electromagnetic wave shielding properties of the laminate, the electromagnetic wave shielding filler is preferably contained in the flame-retardant layer. It should be noted that in this specification, when the flame-retardant layer contains an electromagnetic wave shielding filler, the flame-retardant layer is sometimes referred to as a "flame-retardant and electromagnetic wave shielding layer."
[0137] From the viewpoint of making flame retardancy, electromagnetic wave shielding and mechanical properties good, relative to the total mass of the fiber reinforced resin layer and the flame retardant layer (the total mass of the fiber reinforced resin layer and the flame retardant layer), the content of electromagnetic wave shielding filler in the fiber reinforced resin layer and the flame retardant layer is preferably 0.1% by mass to 20% by mass, more preferably 0.5% by mass to 15% by mass, and further preferably 1% by mass to 10% by mass. In addition, similarly, relative to the total mass of the flame retardant layer, preferably 0.1% by mass to 20% by mass, more preferably 0.5% by mass to 15% by mass, and further preferably 1% by mass to 10% by mass.
[0138] The electromagnetic wave shielding filler is not particularly limited as long as it can shield electromagnetic waves, and can be a filler that reflects electromagnetic waves or a filler that absorbs electromagnetic waves. As the electromagnetic wave shielding filler, a known and commonly used electromagnetic wave shielding filler can be used. As the electromagnetic wave shielding filler, for example, carbon-based electromagnetic wave shielding fillers and metal-based electromagnetic wave shielding fillers can be cited.
[0139] Examples of the carbon-based electromagnetic shielding filler include carbon nanotubes, carbon black, graphite, graphene, and graphite.
[0140] Examples of the metallic electromagnetic wave shielding filler include metals such as gold, silver, platinum, aluminum, copper, iron, nickel, palladium, chromium and stainless steel, and metal powders, metal flakes and metal fibers obtained from oxides of these metals.
[0141] As the metal-based electromagnetic shielding filler, a filler obtained by coating soft magnetic powder flakes with a conductive metal can also be preferably used.
[0142] As the soft magnetic powder flakes, silicon steel, Sendust magnetic alloy, Permalloy, Co-based or Fe-based amorphous alloy powder flakes, or ferrite-based oxide powder flakes are preferred.
[0143] The conductive metal has the same meaning as the conductive metal in the electromagnetic shielding filler contained in the electromagnetic shielding layer described later, and the preferred aspects are also the same.
[0144] As a coating method for conductive metals, known methods can be used, but non-electroplating is particularly preferred. According to this method, a certain amount of uniform coating can be obtained on the surface of the powder sheet. Non-electroplating can be carried out according to conventional methods. For example, the soft magnetic powder sheet is washed, the surface is activated, added to an aqueous solution containing a complexing agent and a reducing agent, and a salt of a conductive metal is added thereto. As a complexing agent, for example, salts of ammonia water, ethylenediaminetetraacetic acid, nitrilotriacetic acid, triethylenetetraaminehexaacetic acid, etc. can be cited. As a reducing agent, formalin, hydrazine and its derivatives, tartaric acid, glucose, etc. can be used. They can be appropriately selected according to the conductive metal used. As a salt of a conductive metal, for example, nitrates, sulfates, etc. can be used.
[0145] The preferred coating amount of the conductive metal varies depending on the type of soft magnetic powder flakes, the size and shape of the powder flakes, and the type of conductive metal. For example, the specific gravity of ferrite-based oxides is lighter than that of alloy-based powder flakes. Therefore, even for powder flakes of the same shape with approximately the same coating thickness, when ferrite-based powder flakes are used, the metal mass ratio (%) in the coated powder flakes is higher than that in the case of alloy-based powder flakes. For example, when ferrite-based soft magnetic alloy powder flakes with an average particle size of 5 to 200 μm and an aspect ratio of 10 to 50 are used and coated with silver, copper or nickel, the coating amount is appropriately about 5 to 75 mass % relative to the unit mass of the coated powder flakes, preferably 10 to 50 mass %, and more preferably 10 to 20 mass %.
[0146] <<Electromagnetic wave shielding layer>>
[0147] The laminate may further include an electromagnetic wave shielding layer. When the laminate includes the electromagnetic wave shielding layer, the electromagnetic wave shielding layer is preferably provided between the flame retardant layer and the fiber reinforced resin layer.
[0148] The electromagnetic wave shielding layer is not particularly limited as long as it is a layer that shields electromagnetic waves, and a known and commonly used electromagnetic wave shielding layer can be used. As the electromagnetic wave shielding layer, for example, it is preferably a layer containing a binder resin and the above-mentioned electromagnetic wave shielding filler. As the binder resin contained in the electromagnetic wave shielding layer, there is no particular limitation, and thermoplastic resins and thermosetting resins can be cited. As thermoplastic resins and thermosetting resins, they are synonymous with the thermoplastic resins and thermosetting resins in the above-mentioned fiber-reinforced resin layer, and the preferred mode is also the same.
[0149] The conductive metal constituting the electromagnetic wave shielding filler includes, for example, metals such as gold, silver, platinum, aluminum, copper, iron, nickel, palladium, chromium and stainless steel, and metal powders, metal flakes and metal fibers obtained from oxides of these metals. Among them, the conductive metal is preferably composed of at least one metal selected from silver, nickel, copper and stainless steel, and more preferably composed of at least one metal selected from copper and stainless steel.
[0150] The shape of the electromagnetic shielding filler is preferably fibrous.
[0151] The diameter of the electromagnetic wave shielding filler is preferably 1 μm to 20 μm, more preferably 4 μm to 8 μm.
[0152] The length of the electromagnetic wave shielding filler is preferably 0.5 mm to 5.0 mm, more preferably 1 mm to 2 mm.
[0153] The content of the electromagnetic shielding filler is preferably 0.1 mass % or more and less than 5.0 mass %, more preferably 0.1 mass % to 3 mass %, and further preferably 0.3 mass % to 1 mass % based on the total solid content of the electromagnetic shielding layer.
[0154] The thickness of the electromagnetic wave shielding layer is preferably 0.5 to 30 mm, more preferably 0.5 to 20 mm, and even more preferably 0.5 to 10 mm.
[0155] The laminated body of the present invention may be provided with a plurality of the above-mentioned layers. As the layer composition of the laminated body of the present invention, for example, "flame retardant layer / fiber reinforced resin layer", "flame retardant layer / fiber reinforced resin layer / flame retardant layer", "flame retardant layer / electromagnetic wave shielding layer / fiber reinforced resin layer", "flame retardant layer / fiber reinforced resin layer / electromagnetic wave shielding layer", "electromagnetic wave shielding layer / flame retardant layer / fiber reinforced resin layer", "flame retardant layer / fiber reinforced resin layer / flame retardant layer / electromagnetic wave shielding layer", "flame retardant layer / electromagnetic wave shielding layer / fiber reinforced resin layer / flame retardant layer", and "electromagnetic wave shielding layer / flame retardant layer / fiber reinforced resin layer / flame retardant layer" etc. may be cited.
[0156] The laminate according to the present invention may include layers other than the flame retardant layer, fiber-reinforced resin layer, and electromagnetic wave shielding layer (hereinafter also referred to as “other layers”). Examples of the other layers include a protective layer and an insulating layer.
[0157] The laminate according to the present invention is excellent in flame retardancy and impact resistance and can be applied to parts requiring flame retardancy and impact resistance.
[0158] It can be applied to parts or shells in various applications requiring impact resistance and flame retardancy, such as automobiles, ships, railway vehicles, aircraft, household electrical equipment, OA equipment, AV equipment, office equipment, building and residential equipment, working machinery, industrial machinery, etc. In addition, it can be applied to the shell of millimeter wave radar and the battery shell for non-aqueous electrolyte secondary batteries described later.
[0159] <Battery case for non-aqueous electrolyte secondary battery>
[0160] The battery case for a non-aqueous electrolyte secondary battery of the present invention (hereinafter, also referred to as "battery case") is a battery case for a non-aqueous electrolyte secondary battery formed using the above-mentioned laminate. Since the battery case is formed using the above-mentioned laminate, it has excellent flame retardancy and impact resistance. In addition, when the above-mentioned laminate including a flame retardant and electromagnetic wave shielding layer is used to form the battery case, in addition to flame retardancy and impact resistance, electromagnetic wave shielding is also excellent.
[0161] The battery case of the present invention is not particularly limited as long as it is a case for storing a battery for a non-aqueous electrolyte secondary battery. For example, a case formed as a case for storing a lithium ion storage battery can be cited. When the battery case of the present invention is applied to a battery pack for an electric vehicle, it is lightweight compared to a metal case, and therefore, the driving distance of the electric vehicle can be extended.
[0162] In the battery case, the flame retardant layer is preferably disposed on the inner side of the battery case, and the flame retardant layer is more preferably disposed on the inner surface of the battery case.
[0163] The battery case usually has a non-aqueous electrolyte, an electrode group, etc. inside it. The so-called "inside of the battery case" refers to the side of the battery case that contains the non-aqueous electrolyte, the electrode group, etc. In addition, the so-called "inner surface of the battery case" refers to the surface inside the battery case.
[0164] Such a configuration can be implemented using, for example, a laminate having a layer structure of "flame retardant layer / fiber reinforced resin layer" or a laminate having a layer structure of "flame retardant layer / fiber reinforced resin layer / flame retardant layer" as a laminate.
[0165] The battery case may further include an electromagnetic wave shielding layer. When the battery case further includes an electromagnetic wave shielding layer, the laminate preferably includes the electromagnetic wave shielding layer. The electromagnetic wave shielding layer in the battery case is synonymous with the electromagnetic wave shielding layer in the laminate, and the preferred embodiment is the same.
[0166] In the battery case, the flame retardant layer and the fiber reinforced resin layer may be laminated in contact with each other, or the electromagnetic wave shielding layer may be laminated between the flame retardant layer and the fiber reinforced resin layer.
[0167] From the perspective of preventing the leakage of electromagnetic wave noise generated by lithium-ion batteries, etc. to the outside, the above-mentioned electromagnetic wave shielding layer is preferably stacked between the flame retardant layer and the fiber reinforced resin layer. More preferably, the electromagnetic wave shielding layer is stacked between the flame retardant layer and the fiber reinforced resin layer, and the flame retardant layer and the fiber reinforced resin layer are stacked in a contact manner.
[0168] The battery case may further include a layer other than the electromagnetic wave shielding layer on the surface opposite to the flame-retardant layer (that is, on the fiber-reinforced resin layer).
[0169] As other layers, for example, there can be mentioned a protective layer, etc. As the protective layer, for example, there can be mentioned a layer formed of the above-mentioned thermoplastic resin.
[0170] In the case of the battery, the fiber-reinforced resin layer or the flame-retardant layer in the laminate may contain an electromagnetic wave shielding filler.
[0171] The electromagnetic wave shielding filler in the battery case has the same meaning as the electromagnetic wave shielding filler in the above-mentioned laminate, and the preferred embodiments are also the same.
[0172] The shape of the battery case is not particularly limited as long as it can accommodate the secondary battery, and may be, for example, square (flat rectangular parallelepiped), cylindrical, or bag-shaped.
[0173] The battery case may be provided with an external terminal, a liquid injection hole, a gas discharge valve, a current interrupting device (CID), and the like.
[0174] <<Method for manufacturing battery casing>>
[0175] There is no particular limitation on the molding method of the battery shell, and known molding methods can be applied. For example, it can be obtained by molding using blow molding, injection molding, compression molding, extrusion molding, extrusion blow molding, injection blow molding, vacuum molding, etc. Among the above molding methods, the battery shell is preferably molded using injection molding.
[0176] <Non-aqueous electrolyte secondary battery>
[0177] The battery for a nonaqueous electrolyte secondary battery according to the present invention includes the battery case for a nonaqueous electrolyte secondary battery described above.
[0178] The non-aqueous electrolyte secondary battery can be provided with the battery case as described above, and can be provided with a conventionally known non-aqueous electrolyte secondary battery. The conventionally known non-aqueous electrolyte secondary battery may include, for example, an electrode body having a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, the electrode body being disposed in a battery case together with a non-aqueous electrolyte.
[0179] As the nonaqueous electrolyte secondary battery, preferably, a lithium ion secondary battery containing a nonaqueous electrolyte is used.
[0180] <<Positive Electrode>>
[0181] The positive electrode preferably includes a positive electrode current collector and a positive electrode composite material layer formed on the main surface of the positive electrode current collector. The positive electrode current collector may be, for example, aluminum (Al) foil or the like. The Al foil may be pure Al foil or Al alloy foil. The positive electrode current collector may have a thickness of, for example, 10 to 30 μm.
[0182] <<Positive electrode composite material layer>>
[0183] The positive electrode composite material layer preferably includes a positive electrode active material, a conductive material and a binder. The positive electrode composite material layer may include, for example, 80 to 98% by mass of the positive electrode active material, 1 to 15% by mass or less of the conductive material and 1 to 5% by mass or less of the binder. The positive electrode composite material layer may have a thickness of, for example, 100 to 200 μm.
[0184] <<Positive electrode active material, conductive material and binder>>
[0185] The positive electrode active material, the conductive material and the binder are not particularly limited.
[0186] The positive electrode active material can be, for example, LiCoO2, LiNiO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NCM: nickel cobalt manganese oxide), LiMn O2, LiMn2O4, LiFePO4, etc.
[0187] The conductive material may be, for example, acetylene black (AB), furnace black, vapor deposited carbon fiber (VGCF), graphite, or the like.
[0188] The binder may be, for example, PVDF (polyvinylidene fluoride), PTFE (polytetrafluoroethylene), or the like.
[0189] <<Negative Electrode>>
[0190] The negative electrode preferably includes a negative electrode current collector and a negative electrode composite material layer formed on a main surface of the negative electrode current collector. The negative electrode current collector may be, for example, copper (Cu) foil, etc. The negative electrode current collector may have a thickness of, for example, about 5 to 20 μm.
[0191] <<Negative Electrode Composite Material Layer>>
[0192] The negative electrode composite material layer preferably contains a negative electrode active material and a binder. The negative electrode composite material layer may contain, for example, 95 to 99% by mass of the negative electrode active material and 1 to 5% by mass of the binder. The negative electrode composite material layer may have a thickness of, for example, about 50 to 150 μm.
[0193] <<Negative electrode active material and binder>>
[0194] The negative electrode active material and the binder are not particularly limited. The negative electrode active material may be, for example, graphite, graphitizable carbon, non-graphitizable carbon, silicon, silicon oxide, tin, tin oxide, etc. In addition, they may also be coated with amorphous carbon. The binder may be, for example, carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), etc.
[0195] <<Non-aqueous electrolyte>>
[0196] The non-aqueous electrolyte includes a lithium salt, an additive and a solvent. The lithium salt may be, for example, LiPF6, LiFSI, etc. The additive may be, for example, Li[B(C2O4)], LiPO2F2, vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), ethylene sulfite (ES), propane sultone (PS), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), LiBF2(C2O4), LiPF2(C2O4)2, etc. The solvent may be, for example, a mixture of cyclic carbonate and chain carbonate.
[0197] The mixing ratio of the cyclic carbonate and the linear carbonate is measured by volume ratio, for example, cyclic carbonate: linear carbonate = 1:9 to 5:5. As the cyclic carbonate, for example, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used. The linear carbonate can be, for example, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), etc.
[0198] <<Diaphragm>>
[0199] As the separator, for example, microporous films such as polyethylene (PE) and polypropylene (PP) can be preferably mentioned. The separator can be a single-layer structure of PE, or a three-layer structure in which a PP film, a PE film and a PP film are stacked in sequence. The thickness of the separator can be, for example, about 9 to 30 μm. In the case where the separator has the above-mentioned three-layer structure, the thickness of the PE layer can be, for example, about 3 to 10 μm, and the thickness of the PP layer can be, for example, about 3 to 10 μm. The pore size and porosity of the separator can be appropriately adjusted in such a way that the air permeability becomes the desired value.
[0200] In addition, the diaphragm may be a diaphragm formed by stacking a plurality of microporous membranes, or may be a diaphragm formed by forming a heat-resistant layer containing an inorganic filler and a binder on its surface. The inorganic filler contained in the heat-resistant layer may be, for example, aluminum oxide, boehmite, titanium dioxide, zirconium oxide, magnesium oxide, etc. The binder contained in the heat-resistant layer may be, for example, PVdF, aramid, SBR, PTFE, etc. The amount of the binder contained in the heat-resistant layer may be 2 to 30% by mass, and the thickness of the heat-resistant layer may be, for example, about 3 to 10 μm.
[0201] Example
[0202] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples.
[0203] The measuring methods of various physical properties are as follows.
[0204] (raw materials)
[0205] Homopolypropylene: Trade name J137G (manufactured by Prime Polymer Co., Ltd., MFR at 230°C and 2.16 kg load according to ASTM D1238: 30 g / 10 minutes)
[0206] Glass fiber masterbatch: Trade name Mostron L-5071PL9 (manufactured by Prime Polymer Co., Ltd., glass fiber content: 50% by mass, polypropylene: 50% by mass)
[0207] Carbon fiber masterbatch: a masterbatch prepared in the following Production Example 2 containing 40% by mass of carbon fiber, 54% by mass of polypropylene, and 6% by mass of polyamide
[0208] Phosphorus flame retardant masterbatch: brand name MB32B (manufacturer: JLS Company), phosphorus flame retardant (Melamine polyphosphate: concentration 39% by mass, Polyphosphoric acid salt, compound: concentration 36% by mass): 75% by mass, polypropylene (PP): 25% by mass
[0209] Brominated flame retardant masterbatch: Trade name Daifunen EH931 (manufacturer: Dainichi Seika Industries, Ltd.), brominated flame retardant (ethylene bispentabromobiphenyl: concentration 54% by mass, antimony trioxide: concentration 21% by mass, polyethylene (PE): 25% by mass)
[0210] Carbon nanotube masterbatch: a masterbatch prepared in the following Production Example 1 containing 15% by mass of carbon nanotubes, 83% by mass of polypropylene, and a total amount of 2% by mass of a dispersant, a stabilizer, and a processing stabilizer
[0211] <Production Example 1>
[0212] (Manufacturing of Carbon Nanotube Masterbatch)
[0213] A carbon nanotube masterbatch was produced using the following materials and the following method.
[0214] -Raw materials-
[0215] Multilayer carbon nanotube: "NC7000" manufactured by Nanocyl Corporation (average diameter: 9.5 mm, average length: 1.5 μm, form: powder, layer structure: multilayer)
[0216] · Polypropylene: "Prime Polypro (registered trademark) J707G" manufactured by Prime Polymer Co., Ltd.
[0217] Dispersant: "L-MODU S400" manufactured by Idemitsu Kosan Co., Ltd. (low stereoregular polyolefin, Mw = 45,000, (Mw / Mn) = 2, softening point: 93°C
[0218] Hindered phenol antioxidant ("Irganox 1010" manufactured by BASF Japan Co., Ltd., chemical formula: pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate)
[0219] Phosphorus-based processing stabilizer ("Irgafos 168" manufactured by BASF Japan Co., Ltd., chemical formula: tris(2,4-di-tert-butylbenzene)phosphite)
[0220] -Manufacturing method-
[0221] 91% by mass of multilayer carbon nanotubes and 9% by mass of a dispersant were placed in an FM mixer ("FM10C / I" manufactured by Nippon Coke & Engineering Co., Ltd., capacity: 9 L). They were stirred at a stirring temperature of 140°C, a stirring time of 60 minutes, and a screw speed of 1000 rpm. Thus, a mixed powder was obtained.
[0222] Next, 16.5% by mass of the mixed powder and 83.5% by mass of polypropylene were dry-blended to obtain a dry-blended product. Specifically, the mixed powder and polypropylene were added to a twin-screw extruder ("TEM-35B" manufactured by Toshiba Machine Co., Ltd., screw diameter: 35 mm, L / D: 32, exhaust type), and a wire bundle with a diameter of 3 mm was obtained from the outlet of the twin-screw extruder. The wire bundle was placed in a water tank, cooled, and cut with a wire bundle cutter. Thus, pellets as a dry-blended product were obtained.
[0223] 99.6 parts by mass of the obtained pellets, 0.2% by mass of a hindered phenol antioxidant, and 0.2% by mass of a phosphorus processing stabilizer were placed in a kneading extruder ("KZW-15TW" manufactured by Technovel Co., Ltd., screw diameter: 15 mmΦ), and kneaded and granulated at a kneading temperature of 230°C and a screw speed of 100 rpm. Thus, a carbon nanotube masterbatch was obtained.
[0224] <Production Example 2>
[0225] (Manufacturing of Carbon Fiber Masterbatch)
[0226] A carbon fiber masterbatch was produced by the following method using the following materials.
[0227] -Raw materials-
[0228] Carbon fiber: "TENAX (registered trademark) HTS40 12K" manufactured by Toho Tenax Co., Ltd. Density: 1.79 g / cm 3 )
[0229] Polypropylene: Homopolymer polypropylene with an MFR of 220 g / 10 min at 230°C and 2.16 kg load according to ASTM D1238, manufactured by Prime Polymer Co., Ltd.
[0230] Polyamide: Polyamide 12 "UBESTA (registered trademark) 3012U" manufactured by Ube Industries, Ltd. (melting point: 180°C, MFR: 17 g / 10 minutes (value measured at 190°C and 1000 g load in accordance with ISO 1133))
[0231] · Acid-modified polyolefin resin: Mitsui Chemicals, Inc. "ADMER QE800"
[0232] -Manufacturing method-
[0233] The components of the matrix resin, namely 76.4 parts by mass of the above-mentioned polypropylene, 10.0 parts by mass of polyamide, and 13.6 parts by mass of acid-modified polyolefin, were put into the feed hopper of a screw extruder whose temperature was adjusted to 250°C. In addition, the above-mentioned carbon fiber roving was opened by a fiber opening process, and the resin and carbon fiber from the extruder were supplied to the impregnation die to obtain a wire bundle with a diameter of 1 mm in such a manner that the content of carbon fiber became 40% by mass. After cooling and solidification, a wire bundle cutter was used to obtain a carbon fiber masterbatch.
[0234] (Examples 1 to 8)
[0235] Using an injection molding machine (manufactured by JSW, 180t injection molding machine) with two barrels of a main unit and a sub-unit, the above raw materials were two-color molded in the mixing ratio described in Table 1 to form a flat test piece. Specifically, the raw materials for the flame retardant layer were put into the main unit, and the raw materials for the fiber reinforced resin layer were put into the sub-unit. The molding conditions are a barrel temperature of 240°C, an injection speed of 15mm / s, a back pressure of 8MPa (main unit side), 3MPa (sub-unit side), and a mold temperature of 60°C. The sub-unit side is injected, and then the movable side of the mold is retreated to create a space in the mold for molding the second layer. The main unit side is injected to obtain a two-layer flat laminate having a flame retardant layer and a fiber reinforced resin layer. The size of the flat laminate is 13cm×10cm. The thickness of each layer is as shown in Table 1.
[0236] (Comparative Examples 1 and 2)
[0237] The above raw materials were dry-blended at the ratios listed in Table 2 to obtain a raw material mixture. The raw material mixture was fed only into the main unit of an injection molding machine (180t injection molding machine manufactured by JSW Co., Ltd.), without using a sub-unit, and injection molding was performed only from the main unit, with the barrel temperature set at 240°C, the injection speed at 15 mm / s, the back pressure at 3 MPa, and the mold temperature at 60°C to obtain a 13 cm×10 cm single-layer molded product.
[0238] [Table 1]
[0239]
[0240] In Tables 1 and 2, "PP" represents polypropylene resin, "PA" represents polyamide, "GF" represents glass fiber, "CF" represents carbon fiber, and "PE" represents polyethylene.
[0241] [Table 2]
[0242]
[0243] The physical properties of the flat-plate laminates and single-layer molded products obtained in Examples 1 to 8 and Comparative Examples 1 and 2 were measured and evaluated by the following methods.
[0244] <<Evaluation>>
[0245] 〔Physical property measurement method〕
[0246] (1) Mechanical properties: Charpy impact strength
[0247] The flat laminates and single-layer molded bodies obtained in Examples 1 to 8 and Comparative Examples 1 and 2 were cut to produce long test pieces (size: 80 mm × 10 mm × 2.5 mm). The impact strength of the produced test pieces was measured using a Charpy impact tester with a constant temperature bath, DG-UB type (manufactured by Toyo Seiki Seisaku-sho, Ltd.). The obtained results are shown in Tables 1 and 2.
[0248] The measurement conditions of the impact test were as follows: a test temperature of 23° C., and a hammer energy of 4 J (for a notched test piece) and 15 J (for a non-notched test piece).
[0249] The measurement of the Charpy impact strength is in accordance with JIS K7111-1 and JIS K7111-2. The larger the value of the Charpy impact strength is, the better the impact resistance is.
[0250] (2) Flame retardancy (UL94 5V)
[0251] The above flat test piece was subjected to a combustion test in accordance with the UL94 5V standard. The center of the flame retardant layer of the test piece was exposed to flames to check whether a hole was formed. If no hole was formed, it was considered acceptable (OK), and if a hole was formed, it was considered unacceptable (NG).
[0252] As shown in Tables 1 and 2, the laminates of Comparative Examples 1 and 2 had poor flame retardancy and failed the test, whereas the laminates of Examples 1 to 8 according to the present invention had excellent flame retardancy and were sufficiently excellent in impact resistance.
[0253] (Examples 9 and 10)
[0254] Except that the raw materials and the blending ratio were as described in Table 3, the same operation as in Example 1 was carried out to obtain a two-layer flat-plate laminate having a flame-retardant and electromagnetic wave shielding layer and a fiber-reinforced resin layer.
[0255] The flat-plate laminates and the single-layer molded products obtained in Examples 9 and 10 were measured for the following tensile strength, tensile elastic modulus, flexural strength, flexural elastic modulus, electromagnetic wave shielding properties, and the above-mentioned Charpy impact strength. The results are shown in Table 3, respectively.
[0256] (3) Mechanical properties: tensile strength and tensile elastic modulus
[0257] The flat plate laminate and the single-layer molded body obtained in Examples 9 and 10 were cut to produce dumbbell test pieces (JIS K 7161-2 type 1BA). The tensile strength and tensile modulus of the produced test pieces were measured using a tensile tester AG-20kNXDPlus (manufactured by Shimadzu Corporation). The results are shown in Table 3.
[0258] The tensile test was conducted at a test temperature of 23° C., a tensile speed of 2 mm / min, and a distance between markings of 25 mm.
[0259] The tensile strength and tensile modulus were measured in accordance with JIS K7161. The larger the tensile strength value, the greater the force required to break the test piece in the tensile mode. The larger the tensile modulus value, the greater the hardness of the test piece in the tensile mode.
[0260] (4) Mechanical properties: flexural strength and flexural modulus
[0261] The flat laminate and the single-layer molded body obtained in Examples 9 and 10 were cut to produce long test pieces (size: 80 mm×10 mm×2.5 mm). The bending strength and bending modulus of the produced test pieces were measured using a bending tester AG-1kNX plus (manufactured by Shimadzu Corporation). The results are shown in Table 3.
[0262] The measurement conditions of the bending test were as follows: a test temperature of 23° C., a bending speed of 2 mm / min, and a span distance of 64 mm.
[0263] The bending strength and bending modulus were measured in accordance with JIS K7171. The larger the bending strength value, the greater the force required to break the test piece in the bending mode. The larger the tensile modulus value, the greater the hardness of the test piece in the bending mode.
[0264] (6) Evaluation of electromagnetic shielding properties
[0265] The electromagnetic shielding performance (dB) of the flat-plate laminate and molded product (13 cm×10 cm) obtained in Examples 9 and 10 was quantitatively evaluated by the KEC method.
[0266] The KEC method is a method developed by the Kansai Electronics Industry Promotion Center (KEC) for measuring electromagnetic shielding performance in the near field. The electromagnetic shielding performance quantified by the KEC method is expressed as the difference between the received intensity when the sample is clamped and the received intensity when the sample is not clamped.
[0267] As a measuring device, an electric field shielding effect evaluation device of KEC Kansai Electronics Industry Promotion Center was used. The measured values when the measuring frequencies were set to 100 kHz, 10 MHz, and 1 GHz are shown in Table 3, respectively.
[0268] As shown in Table 3, the flat laminates of Examples 9 and 10 can impart electromagnetic wave shielding properties without reducing flame retardancy. It should be noted that, for the sake of caution, flat laminates that do not have components that shield electromagnetic waves generally have low electromagnetic wave shielding properties, which are 0 db at each frequency of 100 kHz, 10 MHz, and 1 GHz.
[0269] [Table 3]
[0270]
[0271] (5) Flame retardancy (burner test)
[0272] Using a Bunsen burner, a flame of 1000°C was used to heat the center of the flat plate on the flame retardant layer side of the flat plate laminate obtained in Examples 1 to 6, 9 and 10 for 5 minutes. Then, the state was observed visually and evaluated according to the following evaluation criteria. The results are shown in Table 4. It should be noted that the burner test is a test with much higher intensity than the UL94 5V flame retardancy test. Even if it is an NG evaluation, it does not directly indicate that the flame retardancy is low. If the test result of UL94 5V is OK, the flame retardancy is excellent. Furthermore, if the test result of the burner test is OK, the flame retardancy is particularly excellent.
[0273] <Evaluation Criteria>
[0274] OK: There are no openings in the flat plate stack.
[0275] NG: A hole is opened in the flat plate stack.
[0276] [Table 4]
[0277]
Claims
1. A laminate comprising a flame retardant layer and a fiber reinforced resin layer, The flame retardant layer contains 20% to 80% by mass of a thermoplastic resin relative to the total mass of the flame retardant layer, and 20% to 80% by mass of a flame retardant relative to the total mass of the flame retardant layer, wherein the flame retardant is at least one selected from the group consisting of a phosphorus flame retardant, a bromine flame retardant, and an inorganic hydrate flame retardant, and the content of the reinforcing fiber is 0% to 20% by mass relative to the total mass of the flame retardant layer. The fiber-reinforced resin layer contains 30% to 90% by mass of a thermoplastic resin based on the total mass of the fiber-reinforced resin layer and 10% to 70% by mass of reinforcing fibers based on the total mass of the fiber-reinforced resin layer.
2. The laminate according to claim 1, wherein The content of the reinforcing fiber included in the fiber-reinforced resin layer is greater than the content of the reinforcing fiber included in the flame-retardant layer by 10% by mass or more.
3. The laminate according to claim 1, wherein The content of the flame retardant in the fiber-reinforced resin layer is 0 mass % or more and less than 20 mass % relative to the total mass of the fiber-reinforced resin layer, and the flame retardant is at least one selected from the group consisting of phosphorus-based flame retardants, bromine-based flame retardants, and inorganic hydrate-based flame retardants.
4. The laminate according to claim 1, wherein The flame retardant layer contains 40% to 80% by mass of the flame retardant relative to the total mass of the flame retardant layer. The fiber-reinforced resin layer contains 40% to 60% by mass of the reinforcing fiber relative to the total mass of the fiber-reinforced resin layer, and the content of the flame retardant is 0% to 10% by mass relative to the total mass of the fiber-reinforced resin layer, and the flame retardant is at least one selected from the group consisting of phosphorus-based flame retardants, bromine-based flame retardants and inorganic hydrate-based flame retardants.
5. The laminate according to claim 1, wherein The fiber-reinforced resin layer includes at least one resin selected from the group consisting of polypropylene resins and polyamide resins as the thermoplastic resin.
6. The laminate according to claim 1, wherein The reinforcing fibers include at least one type of fiber selected from the group consisting of carbon fibers and glass fibers.
7. The laminate according to claim 1, wherein At least one of the fiber-reinforced resin layer and the flame-retardant layer contains an electromagnetic wave shielding filler.
8. The laminate according to claim 1, wherein The thickness of the fiber-reinforced resin layer is 0.5 to 30 mm. 9 . A battery case for a non-aqueous electrolyte secondary battery, the battery case being formed using the laminate according to claim 1 .
10. The battery case for a non-aqueous electrolyte secondary battery according to claim 9, wherein: The flame retardant layer in the laminate is arranged inside the battery case.
11. The battery case for a non-aqueous electrolyte secondary battery according to claim 9, wherein: The flame retardant layer in the laminate is disposed inside and outside the battery case. 12 . The battery case for a nonaqueous electrolyte secondary battery according to claim 9 , further comprising an electromagnetic wave shielding layer. 13 . A battery for a non-aqueous electrolyte secondary battery, comprising the battery case for a non-aqueous electrolyte secondary battery according to claim 9 .