By forming a seepage structure composed of photothermal materials on the surface and absorbing near-infrared spectra using photothermal effect, the problems of surface mist removal and transparency maintenance in the prior art are solved, and efficient anti-fog and ice protection in high humidity environments are achieved Effect.
Patent Information
- Application Number
- CN202380033908.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2023-03-14
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to effectively prevent or remove surface mist in the long term, especially in high relative humidity environments. Traditional methods such as superhydrophilic and superhydrophobic surfaces have shortcomings in terms of texture and contamination, and the sun-absorbing surfaces usually need to compromise on transparency or Heating effect.
The photothermal element composed of photothermal materials is produced through the Volmer-Weber growth process to form a seepage structure, which is at the seepage threshold, realizes the photothermal conversion of electromagnetic radiation, absorbs the near-infrared spectrum and remains transparent in the visible spectrum.
It realizes effective prevention or removal of mist in high relative humidity environments, maintains high transparency and visibility, and has a thin structure and is easy to integrate, durable and free from chemical or mechanical damage.
Smart Images

Figure CN119032630A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a heating device for preventing or removing deposits, in particular a heating device for demisting (eg defogging), anti-fogging (eg anti-misting), deicing or anti-icing, and a method for producing such a heating device. Background Art
[0002] The loss of transparency and visibility when a surface fogs (e.g., fogging) is very troublesome and detrimental to many daily activities (e.g., daily activities involving windows, windshields, prescription and sports glasses, optical sensors, displays, and, most recently, glasses during mask use) [1, 2]. Transparency loss due to fogging is found in many social and industrial sectors (e.g., medical, security, energy / photovoltaics, and chemical / food) [3]. Surface fogging usually occurs due to a drop in temperature or an increase in relative humidity of the surrounding environment, resulting in a large number of droplets nucleating on the surface [1, 4, 5]. These droplets scatter the incident light and thus negatively affect transparency and visibility [6-8]. Various attempts have been made and implemented to mitigate this phenomenon while maintaining transparency, also going beyond Joule heating and involving passive, energy-neutral methods. Temporary solutions such as superhydrophilic surfaces [6] or surfactants change the surface energy and produce a mostly continuous, very thin layer of condensate. As a result, transparency to the human eye can be maintained while scattering of the incident light is reduced [7-9]. However, due to gravity, drying and contaminants, the water film is not always uniform, resulting in distorted visibility
[10] . Due to the high surface energy of such surfaces, the surfaces are inherently susceptible to contamination from organic contaminants, severely limiting the durability of their effectiveness [1, 11]. Typically, more durable passive solutions rely on micro- and nano-patterned superhydrophobic surfaces [12-15], with the goal of self-removing condensed water droplets on the surface before they can grow to a size that seriously affects transparency [16, 17]. Due to the low surface energy and texture of these surfaces, condensed droplets maintain high fluidity (Cassie-Baxter wetting state
[18] ) and thus avoid pinning of water droplets on the surface (Wenzel wetting state
[19] ). However, when exposed to an environment with high relative humidity, complex engineering of the structure (which is neither easy to be robust nor easy to scale on glass) is necessary because nanoscale nucleation within the texture eliminates the Cassie-Baxter state, induces the Wenzel state and destroys the superhydrophobic properties of the structure
[20] . Therefore, the above methods are not sufficient as long-term, passive solutions to completely eliminate fog formation while maintaining high visibility, and new solutions are highly desired and sought after.
[0003] Recently, an alternative approach to preventing fogging has been to exploit the abundant natural energy of the sun, combining the thermodynamics of condensation nucleation with its selective and efficient absorption. The absorbed sunlight can be dissipated as heat (photothermal effect), which in turn reduces the likelihood of nucleation, or - if already covered with fog - quickly dry the surface to restore its transparency. Previous work has focused on making sunlight-absorbing surfaces with carbon-based materials [21, 22], plasma metal inclusions [10, 23-25], polymers [26, 27] or multilayer selective absorbers
[28] . However, these surfaces are designed for broadband absorption [10, 17, 29-33], and these surfaces usually have to compromise on transparency or heating depending on the main effect of the target. Interestingly, nearly half of the solar energy is located in the near-infrared spectrum, which is invisible to the human eye. This physical fact can be exploited to design spectrally selective coatings that have the characteristics of being transparent in the visible range and absorbing well in the infrared range of the solar spectrum to produce photothermal heating. In practice, few such attempts have been demonstrated. However, these coatings are either narrow-band absorbing [34, 35] or thick [24, 36] to achieve the required temperature increase (several micrometers, which is very cumbersome to manufacture) and are therefore difficult to integrate into existing processes for many of the above-mentioned applications. Summary of the invention
[0004] The object of the present invention is to provide an improved heating device for preventing or removing deposits, in particular for demisting, anti-fogging, deicing or anti-icing.
[0005] This object is achieved by a heating device according to claim 1. That is, a heating device for preventing or removing deposition, in particular for defogging (e.g., demisting), anti-fogging (e.g., anti-fogging), deicing or anti-icing is provided. The heating device extends along an extension direction and comprises at least one photothermal element, which is configured to exhibit a photothermal effect when irradiated with electromagnetic radiation. The photothermal element comprises or consists of a photothermal material, which comprises a percolation structure. The percolation structure is at its percolation threshold or substantially at its percolation threshold.
[0006] Therefore, the heating device according to the present invention is configured to generate heat when electromagnetic radiation impinges on the photothermal element. In other words, the photothermal element is configured to perform photothermal conversion of electromagnetic radiation, wherein the photothermal element absorbs the electromagnetic radiation and dissipates the electromagnetic radiation as heat, thereby increasing the temperature of the heating device.
[0007] As will be explained in more detail below about the method for producing such a heating device, the photothermal element is preferably produced by chemical growth and / or deposition of material on a substrate, which is preferably a dielectric element, a displacement element or a carrier element. To this end, the photothermal element is produced by island growth, wherein in the case of deposition, isolated islands of the deposited material are formed in the first step, and wherein the isolated islands will gradually grow during the further deposition process. For this purpose, it is particularly preferred to produce the photothermal element according to the so-called Volmer-Weber growth process known in the art, see, for example, https: / / link.springer.com / content / pdf / 10.1007%2F978-981-10-6884-3.pdf. In the Volmer-Weber (VW) growth process, in the initial stage of growth, small islands nucleate on the substrate, and then the islands grow and impact to form a continuous layer. If the bonding strength between the layer atoms is stronger than the bonding strength between the layer atoms and the substrate atoms, this growth mode is dominant. The layer atoms prefer to be close to the same type of atoms rather than the substrate atoms, and therefore small islands will be formed at the beginning of growth. When these islands impinge upon each other, grain boundaries are formed and the film microstructure is therefore polycrystalline (assuming no epitaxial relationship to the substrate is established).
[0008] After a certain amount of conductive material is deposited, these separated islands will contact each other and form the aforementioned conductive pattern or conductive path, ie, percolation structure.
[0009] Finally, a randomly distributed photothermal material is produced, and wherein the photothermal material forms a random conductive pattern or a random conductive path. Since the photothermal material is preferably produced on a substrate, the photothermal material is preferably randomly distributed on the substrate, so that the photothermal material forms a completely random conductive pattern or conductive path on the substrate. In other words, it can be said that the photothermal elements are randomly arranged on the substrate.
[0010] The percolation threshold is the state where the photothermal material suddenly changes from an electrical insulator to an electrical conductor when a conductive pattern or conductive path is formed. In other words, it can be said that percolation starts at the percolation threshold, and wherein percolation occurs when a conductive pattern or conductive path is formed such that electrons or current can flow. For example, the presence or absence of such a conductive pattern or conductive path can be studied by measuring the conductivity of the photothermal material or by electron microscopy or scanning electron microscopy, where the path connectivity is visually observed and quantified.
[0011] The photothermal element preferably exhibits resistance. When there is electron flow, the resistance is highest at the beginning of percolation because the resistance is associated with the most randomness of the percolation structure. At the percolation threshold, the dielectric function of the photothermal structure diverges and exhibits characteristics at both DC (direct current, i.e., low frequency) conductivity and AC (alternating current, i.e., light / high frequency) frequencies. Under DC, the characteristic is a power law decrease in resistance, from high (open circuit) to low, because the photothermal structure becomes more and more conductive as the thickness parameter of the photothermal structure increases.
[0012] In this context, such a drop from high resistance to low resistance is understood as a power law drop. Thus, the resistance of the photothermal structure at or substantially at the percolation threshold preferably drops as a power law.
[0013] Under AC, i.e. in the optical state, the percolation structure is substantially at the percolation threshold, or, if applicable, at its percolation threshold, and is further characterized by: a broadband (i.e., almost wavelength-independent, Kramers-Kronig-related) absorption spectrum; the broadband absorption is obtained for wavelengths above a certain wavelength, which depends on the photothermal material and is referred to herein as the "minimum wavelength of the range of interest". The broadband absorption occurs between the minimum wavelength of the range of interest and up to the "maximum wavelength of the range of interest" (e.g., 2500 nm for solar applications). A percolation structure substantially at the percolation threshold is understood to have a total absorption in the range of interest of at least 60% or more, preferably at least 70% or more, of the maximum total broadband absorption in the same range of interest.
[0014] For example, for a photothermal material substantially at the percolation threshold made of gold and fabricated on a titanium dioxide dielectric element, the minimum wavelength of the range of interest is approximately 800 nm. Alternatively, for a photothermal material substantially at the percolation threshold made of copper and fabricated on a titanium dioxide dielectric element, the minimum wavelength of the range of interest is approximately 800 nm, and for a photothermal material substantially at the percolation threshold made of silver and fabricated on a titanium dioxide dielectric element, the minimum wavelength of the range of interest is approximately 800 nm.
[0015] Depending on the photothermal material, the absorption behavior of percolation structures at or substantially at the percolation threshold may be the same.
[0016] Unless stated otherwise, "total absorption" or "absorption" is preferably understood herein as "average absorption", ie the "average" absorption without taking into account any weighting factors, such as sunlight, for example.
[0017] As previously described, the percolation structure at the percolation threshold is preferably determined by measuring the resistance of the photothermal material, and wherein the resistance exhibits a power-law decrease. The resistance of the photothermal material can be measured with a four-point probe measurement (e.g., a Jandel universal probe station or any other probe station). For example, for a photothermal material made of gold and fabricated on a titanium dioxide dielectric element, the resistance decreases from an open circuit (i.e., no conductive path) for a photothermal material thickness parameter of 4.25 nm (see below) to 400 Ohms for a thickness parameter of 5 nm, and further to 107 Ohms for a thickness parameter of 5.75 nm. In the case of larger thickness parameters, the resistance further "flattens"; for example, for a thickness parameter of 15 nm, the resistance reaches a value of 5 Ohms, and in the case of a thickness parameter of 30 nm, it reaches a value of 2 Ohms.
[0018] In addition to the power law decrease in resistance as described above, the percolation structure substantially at its percolation threshold is preferably determined by measuring the absorption spectrum of the photothermal material, and wherein, as described above, the total absorption within the range of interest is at least 60% or more, preferably at least 70% or more, of the maximum total broadband absorption within the same range of interest.
[0019] The absorption spectrum of the photothermal material can be measured using a LIV-VIS spectrometer (eg, V770, Jasco with an ILN-925 integrating sphere) or using FTIR (eg, using Nicolet Thermo Fisher Scientific).
[0020] For example, a percolation structure substantially at the percolation threshold having a gold photothermal material on a dielectric element made of titanium dioxide can exhibit absorption, i.e., an average absorption of at least 17% of incident electromagnetic radiation in the region from 800 nm (the minimum wavelength of the range of interest) to the maximum wavelength of the range of interest (e.g., 2500 nm) (i.e., the total absorption in the range of interest is at least 60% or more of the maximum total broadband absorption in the same range of interest). As another example, a percolation structure substantially at the percolation threshold having a copper photothermal material on a dielectric element made of titanium dioxide can exhibit an average absorption of at least 14% of incident electromagnetic radiation in the region from 800 nm (the minimum wavelength of the range of interest) to the maximum wavelength of the range of interest (e.g., 2500 nm) (i.e., the total absorption within the range of interest is at least 60% or more of the maximum total broadband absorption within the same range of interest), and a percolation structure substantially at the percolation threshold having a silver photothermal material on a dielectric element made of titanium dioxide can exhibit an average absorption of at least 18% of incident electromagnetic radiation in the region from 800 nm (the minimum wavelength of the range of interest) to the maximum wavelength of the range of interest (e.g., 2500 nm) (i.e., the total absorption within the range of interest is at least 60% or more of the maximum total broadband absorption within the same range of interest).
[0021] Depending on the photothermal material, for example for a photothermal material made of gold on a dielectric element made of titanium dioxide, the absorption behavior of the percolation structure at the percolation threshold or substantially at the percolation threshold is the same.
[0022] Additionally or alternatively, the expression "substantially at the percolation threshold" means that the percolation structure of the photothermal material preferably configures the photothermal material to exhibit an absorption (especially total absorption) of 10% or more (for example, 15% or more), more preferably 25% or more, and particularly preferably 35% or more, of incident electromagnetic radiation having a wavelength in the range of 700 nanometers to 2.5 microns.
[0023] For example, a percolation structure of a photothermal material made of gold and substantially at the percolation threshold on a dielectric element made of titanium dioxide configures the photothermal material to exhibit an average absorption of incident electromagnetic radiation in the range of 700nm to 2.5 microns exceeding 17% (i.e., the total absorption in the range of interest (here in the range of 700nm to 2.5 microns) is at least 60% or more of the maximum total broadband absorption in the same range of interest (here in the range of 700nm to 2.5 microns)). As another example, a percolation structure of a photothermal material made of copper and substantially at the percolation threshold on a dielectric element made of titanium dioxide configures the photothermal material to exhibit an average absorption of incident electromagnetic radiation in the range of 700nm to 2.5 microns exceeding 14% (i.e., the total absorption in the range of interest (here in the range of 700nm to 2.5 microns) is at least 60% or more of the maximum total broadband absorption in the same range of interest (here in the range of 700nm to 2.5 microns)). The percolation structure of a photothermal material made of aluminum and substantially at the percolation threshold on a dielectric element made of titanium dioxide configures the photothermal material to exhibit an average absorption of incident electromagnetic radiation in the range of 700nm to 2.5 microns exceeding 20% (i.e., the total absorption in the range of interest (here in the range of 700nm to 2.5 microns) is at least 60% or more of the maximum total broadband absorption in the same range of interest (here in the range of 700nm to 2.5 microns)). The absorption spectrum of the photothermal material is measured using the LIV-VIS spectrometer mentioned above.
[0024] Additionally or alternatively, the expression "substantially at the percolation threshold" means that the percolation structure of the photothermal material is within 40%, such as within 30% or within 20%, such as within 10% or within 5%, of a thickness parameter associated with the photothermal material that exhibits a maximum total broadband absorption between a minimum wavelength in the range of interest and a maximum wavelength in the range of interest (e.g. 2500 nm for solar applications). The thickness parameter is fed into a deposition device that produces the photothermal element by deposition (see further below). For this purpose, the deposition device corresponds to an Evatec BAK501 LL (thermal evaporator) or a Von Ardenne CS 320C (sputtering method). The actual thickness of the deposited photothermal material may differ slightly from the tool-specific thickness parameter.
[0025] For example, if the percolation threshold of the photothermal material is 5 nm in thickness parameter, the photothermal material substantially at the percolation threshold may be between 3.5 nm and 6.5 nm, preferably, for example, between 4 nm and 6 nm.
[0026] Specifically, if the percolation threshold of a photothermal material made of gold on a dielectric element of titanium dioxide is 4.75 nm in thickness parameter, the thickness parameter of the photothermal material substantially at the percolation threshold may be between 2.9 nm and 6.7 nm (i.e., the percolation structure is within 40% of the thickness parameter associated with the photothermal material exhibiting the maximum total broadband absorption in the range of interest), preferably between 3.3 nm and 6.2 nm (i.e., the percolation structure is within 30% of the thickness parameter associated with the photothermal material exhibiting the maximum total broadband absorption in the range of interest). As another example, if the percolation threshold of a photothermal material made of silver on a dielectric element of titanium dioxide is 7 nm in thickness parameter, the thickness parameter of the photothermal material substantially at the percolation threshold may be between 4.2 nm and 9.8 nm, preferably between 4.9 nm and 9.1 nm. As another example, if the percolation threshold of a photothermal material made of copper on a dielectric element of titanium dioxide is 5 nm in thickness parameters, the thickness parameter of the photothermal material substantially at the percolation threshold may be between 3 nm and 7 nm, preferably between 3.5 nm and 6.5 nm. As another example, if the percolation threshold of a photothermal material made of aluminum on a dielectric element of titanium dioxide is 5 nm in thickness parameters, the thickness parameter of the photothermal material substantially at the percolation threshold may be between 3 nm and 7 nm, preferably between 3.5 nm and 6.5 nm. The thickness parameter is fed into a deposition device that produces the photothermal element by deposition. To this end, the deposition device corresponds to an Evatec BAK501 LL (thermal evaporator) or a Von Ardenne CS 320C (sputtering method). The actual thickness of the deposited photothermal material may differ slightly from the tool-specific thickness parameter.
[0027] The photothermal material is preferably optically transparent. The photothermal material is particularly preferably optically transparent for electromagnetic radiation in the visible region of the electromagnetic spectrum.
[0028] Additionally or alternatively, the photothermal material is preferably configured to absorb incident electromagnetic radiation. The photothermal material is particularly preferably configured to absorb incident electromagnetic radiation in the near infrared region of the electromagnetic spectrum.
[0029] The visible region (VIS) of the electromagnetic spectrum is understood to include electromagnetic radiation having a wavelength in the range of 300 nanometers to 720 nanometers. In other words, the photothermal material preferably exhibits broadband absorption in the NIR rather than in the VIS.
[0030] The near infrared region (NIR) of the electromagnetic spectrum is understood to include electromagnetic radiation having wavelengths in the range of 720 nanometers to 2.5 micrometers.
[0031] Furthermore, the photothermal material is preferably configured to absorb 10% or more, such as 20% or more or 30% or more, preferably 35% or more, of incident electromagnetic radiation in the near infrared region. Furthermore, the photothermal material preferably has a transmittance of 40% or more, such as 50% or more or 60% or more, preferably 65% or more, in the visible region of the electromagnetic spectrum. Thus, the photothermal material is particularly preferably absorptive in the NIR while being visually transparent. In fact, the photothermal material particularly preferably exhibits strong broadband absorptivity in the NIR while being transparent in the VIS.
[0032] Furthermore, it should be noted that due to the random distribution of the photothermal material, the transmittance of the photothermal material is independent or almost independent of the incident angle of the electromagnetic radiation striking the photothermal element.
[0033] Depending on the specific field of application of the heating device, the heating device is preferably designed to have significant absorptivity and transmittance in a specific wavelength region or range of interest. For example, if the heating device is to be used with solar radiation, it is particularly preferred that the photothermal element is configured to strongly absorb electromagnetic radiation with a wavelength in the range of 720nm to 1380nm to match the solar radiation, and is further configured to be optically transparent to electromagnetic radiation with a wavelength in the range of 450nm to 650nm. In this case, the photothermal element exhibits peak transparency at the wavelength of the solar radiation.
[0034] The photothermal element may be electrically conductive or electrically insulating.
[0035] That is, the photothermal element may be electrically conductive, in which case the percolation structure of the photothermal material is at or above the percolation threshold. Above the percolation threshold means that the photothermal material is substantially at the percolation threshold previously defined, but at a higher value of the percolation threshold.
[0036] That is, for example, if the percolation threshold of the photothermal material is 5, then the “percolation structure of the photothermal material above the percolation threshold” is greater than 5, for example, 5.5.
[0037] However, it is also conceivable that the photothermal element is electrically insulating, in which case the percolation structure of the photothermal material is below the percolation threshold. Below the percolation threshold means that the photothermal material is substantially at the percolation threshold previously defined, but at a lower value of the percolation threshold. That is, for example, if the percolation threshold of the photothermal material is 5, then the "percolation structure of the photothermal material below the percolation threshold" is less than 5, for example 4.5.
[0038] As mentioned above, percolation is associated with the presence of a conductive path or conductive pattern path that allows the transmission of electrical energy. Electromagnetic radiation of a specific wavelength (for example, electromagnetic radiation in the NIR) is associated with propagating electrical oscillations on the order of hundreds of nanometers. Therefore, such electromagnetic radiation is not precisely "localized" like the electrons in the photothermal material. Therefore, there may be a situation where the photothermal element is not conductive while the photothermal element still allows the propagation of an oscillating field (preferably a high-frequency oscillating field, such as an NIR field). Therefore, referring to the above, the heating device according to the present invention is able to generate heat even when the percolation structure is not at the percolation threshold but is substantially at the percolation threshold.
[0039] The heating device may further comprise at least one electrical element configured to introduce an electric current into the photothermal element, thereby generating heat from the photothermal element.
[0040] The heating device comprising the electrical element is preferably configured to generate heat by resistive heating (also known as Joule heating). That is, the current introduced to the photothermal element is dissipated as heat within the percolation structure of the photothermal material.
[0041] The electrical elements are preferably electrodes. For example, the edges of the percolation structure may be wired.
[0042] In the absence of electrical elements, the heating device can be said to be configured to operate wirelessly. That is, the heating device is configured to generate heat solely through the photothermal material.
[0043] In the case of an electrical element, the heating device can be said to be configured for wired operation. That is, the heating device is configured to generate heat through the action of the photothermal material and through the electrical element.
[0044] For example, in situations where the heat generated by the photothermal material is insufficient (e.g., in bad weather conditions or in the absence of light, such as at night), the electrical element can provide additional heat generation. In this case, the electrical element allows the heating device to retain its deposit removal function.
[0045] For this purpose, it is particularly preferred if, as explained above, the heating device comprises at least one electrical element if the photothermal material is at or above the percolation threshold.
[0046] That is, the heating device configured for wired operation preferably comprises a photothermal material at or above the percolation threshold, i.e., the photothermal material preferably corresponds to an electrical conductor. That is, when configured for wired operation, the percolation structure substantially at the percolation threshold is preferably above 40%, more preferably above 30%, more preferably above 20%, even more preferably above 10%, and particularly preferably above 5% of the thickness parameter of the percolation threshold associated with the photothermal material.
[0047] The heating device configured for wireless operation preferably exhibits strong broadband absorption, wherein the photothermal material is preferably substantially at the percolation threshold and has a random arrangement, wherein the maximum absorption is substantially at the percolation threshold. That is, when configured for wireless operation, the percolation structure substantially at the percolation threshold is preferably above or below 40% of the thickness parameter of the percolation threshold associated with the photothermal material, more preferably above or below 30%, more preferably above or below 20%.
[0048] The photothermal element preferably has a thickness in the extension direction in the range of 1 nm to 50 nm, more preferably in the range of 1 nm to 10 nm, and particularly preferably in the range of 4 nm to 8 nm (eg 5 nm).
[0049] Additionally or alternatively, the heating device preferably has a thickness in the range of 1 nm to 100 nm, more preferably in the range of 1 nm to 50 nm, and particularly preferably in the range of 1 nm to 20 nm (e.g. 10 nm) with respect to the extension direction. That is to say, the overall thickness of the heating device with respect to the extension direction is preferably in the range of 1 nm to 100 nm, more preferably in the range of 1 nm to 50 nm, and particularly preferably in the range of 1 nm to 20 nm (e.g. 10 nm). However, greater thicknesses of the heating device are likewise conceivable and depend, for example, on the thickness of the substrate (e.g. carrier element) used.
[0050] Additionally or alternatively, the photothermal element and / or the heating device preferably has in each case a thickness for the direction of extension which is significantly smaller than the wavelength of the incident electromagnetic radiation in the visible and near infrared.
[0051] For example, the wavelength in the visible region of the electromagnetic spectrum is 450 nanometers. Therefore, the thickness of the photothermal element or heating device relative to the extension direction is less than 450 nanometers.
[0052] The heating device is preferably bendable. Additionally or alternatively, the heating device preferably comprises an inverse curvature greater than 1 micrometer when bent. Such an inverse curvature is associated with a bending radius or curvature, wherein, since the scale of the random arrangement of the heating device is much smaller than the bending curvature radius, the bending of the heating device does not affect the optical properties of the heating device.
[0053] The photothermal element is preferably a layer. Furthermore, it is preferred that the layer extends in a lateral direction extending perpendicularly to the extension direction.
[0054] The photothermal material is preferably electrically conductive. Additionally or alternatively, the photothermal material preferably comprises at least one metal or consists of at least one metal. For example, the photothermal material may comprise or consist of a single metal such as gold, silver, aluminum, copper, platinum or tungsten or titanium. However, it is also conceivable that the photothermal material comprises or consists of a metal alloy such as PtAu, CuZn, CuAg, CuSn, AICu, AgAICu or AgCu.
[0055] For this purpose, it is particularly preferred that the photothermal material corresponds to a metal layer, which preferably further consists of a single component. In view of the preferred thickness of the photothermal element outlined above, it can be said that the photothermal material particularly preferably corresponds to a thin metal layer. However, it is also preferred that the photothermal material is a semiconductor or a heavily doped semiconductor, such as InAsSb, InAs, Ge, Si, GeSn. In the case of a heating device for NIR, semiconductors are preferably used.
[0056] Additionally or alternatively, the photothermal material may comprise or consist of an optically transmissive and conductive oxide, a so-called transparent conductive oxide (TCO), such as indium tin oxide (ITO). However, other transparent conductive oxides known in the art, such as antimony-doped tin oxide (ATO), indium tin oxide (ITO), indium zinc oxide (IZO), cadmium oxide (CdO), fluorine-doped tin oxide (FTO, SnO2:F) or aluminum-doped zinc oxide (AZO, ZnO:Al) are likewise conceivable. Additionally or alternatively, the photothermal material may comprise or consist of a transition metal nitride, in particular titanium nitride (TiN).
[0057] The photothermal material is preferably provided according to the desired end-user application of the heating device. For example, gold and copper are particularly suitable for NIR absorption, while silver and aluminum perform well in the VIS.
[0058] The heating device preferably further comprises at least one dielectric element, wherein the dielectric element is arranged before or after the photothermal element with respect to the extension direction. That is, preferably, the heating device comprises at least one electrical insulator in the form of a dielectric element.
[0059] The dielectric element and the photothermal element may be in surface contact with each other at least partially or completely. That is, the dielectric element is preferably arranged at least partially on the surface of the photothermal element, and particularly preferably completely on the surface of the photothermal element. In other words, the dielectric element and the photothermal element are preferably in surface contact or direct contact with each other.
[0060] The dielectric element is preferably optically transparent. Additionally or alternatively, the dielectric element preferably comprises at least one metal oxide (e.g. titanium dioxide (TiO 2 ), silicon dioxide (SiO 2 ), Tantalum pentoxide (Ta 2 O 5 ), or a metal nitride or carbide such as silicon carbide (SiC) or titanium nitride (TiN)), or consists of at least one metal oxide, particularly preferably in the form of a continuous film.
[0061] The thickness of the dielectric element with respect to the extension direction is preferably 1 nm or more, for example between 1 nm and 1 cm. More preferably, the thickness of the dielectric element is in the range of 1 nm to 5 nm, for example in the range of 1 nm to 3 nm.
[0062] In addition, preferably, the dielectric element is at least partially functionalized. In fact, preferably, referring to above, the dielectric element is functionalized in the region in contact with the photothermal element (for example, on the surface in contact with the surface of the photothermal element). The functionalization is preferably configured to affect the formation of the percolation structure on the dielectric element. In fact, the functionalization preferably affects the growth of the percolation structure of the photothermal material, so that the percolation structure at the percolation threshold or substantially at the percolation threshold can be manufactured with a thinner or thicker thickness parameter. The dielectric element is preferably functionalized so that its wettability changes. For example, the dielectric element can be subjected to ozone or oxygen plasma treatment, so that the oxygen group is attached to the surface of the dielectric element. As another example, the dielectric element can be functionalized with a monolayer. Of course, other functionalizations known to those skilled in the art are also conceivable.
[0063] The heating device preferably comprises at least two dielectric elements, and wherein the photothermal element is particularly preferably arranged between the two dielectric elements relative to the extension direction. In other words, the photothermal element is preferably sandwiched between the two dielectric elements. The at least two dielectric elements may be identical to or different from each other. For example, the two dielectric elements may be titanium dioxide or silicon dioxide. Alternatively, one of the dielectric materials may be titanium dioxide and the other may be silicon dioxide. It should be noted that many other dielectric materials are also conceivable.
[0064] The one or more dielectric elements are preferably layers, and wherein the layer or layers preferably extend in a lateral direction extending perpendicularly to the extension direction.
[0065] That is, the heating device preferably corresponds to a layered structure comprising at least one photothermal layer and one or more dielectric layers which are superposed on each other with respect to the extension direction.
[0066] The heating device may include two or more photothermal elements, preferably two or more photothermal layers stacked on each other relative to the extension direction. In addition, the two or more photothermal elements are preferably arranged spaced apart from each other relative to the extension direction. For example, a dielectric element may be arranged between the two or more photothermal elements.
[0067] The heating device preferably further comprises at least one shifting element, wherein the shifting element is configured to shift an absorptivity and / or a transmissivity of the heating device with respect to the incident electromagnetic radiation towards shorter or longer wavelengths of the incident electromagnetic radiation.
[0068] Shifting the absorptive capacity of the heating device towards longer (shorter) wavelengths means that the device is configured to absorb electromagnetic radiation of longer (shorter) wavelengths than if the heating device lacked the shifting element.
[0069] Likewise, shifting the transmission capability of the heating device towards longer (shorter) wavelengths means that the heating device is configured to transmit electromagnetic radiation of longer (shorter) wavelengths than if the heating device lacked the shifting element.
[0070] The shifting element particularly preferably causes a shift of the maximum mean absorbance or the maximum total absorbance and / or the maximum mean transmittance in the range of interest towards longer or shorter wavelengths.
[0071] Therefore, the shifting element is used to tune the absorption and / or transmittance of the heating device to the desired wavelength region of the electromagnetic spectrum. In fact, the shifting element is configured to tune the optical response (transmission and absorption) of the percolation structure of the photothermal material. For example, if the heating device is to be used with sunlight, the absorptive capacity of the heating device (particularly its maximum average absorptivity) is preferably shifted toward the peak wavelength region of the solar radiation. In addition, if the heating device should be visibly transparent, the transmission capacity of the heating device (particularly its maximum average transmittance) is preferably shifted toward the peak wavelength of the visible spectrum. In this case, it can be said that the shifting element aligns the transparency peak of the heating device with the peak wavelength of the solar radiation.
[0072] The displacement element is preferably arranged before and / or after the photothermal element relative to the extension direction. For example, a percolation structure substantially at the percolation threshold, in which the photothermal material is gold on a dielectric element made of titanium dioxide, a displacement element made of titanium dioxide on the photothermal material and the displacement element is at least partially or completely in contact with the surface of the photothermal material, can exhibit an average absorption of at least 19% of incident electromagnetic radiation in the range of 1000nm (the minimum wavelength of the shift of the range of interest) to the maximum wavelength of the range of interest (e.g., 2500nm for solar applications). This indicates that the displacement element shifts the minimum wavelength of the range of interest, i.e., the presence of the displacement element causes the minimum wavelength of the range of interest to be shifted, and wherein the total absorption is obtained for wavelengths above the said minimum wavelength of the shift of the range of interest. The displacement element preferably also increases the maximum total absorption in the range of interest.
[0073] As another example, a percolation structure substantially at the percolation threshold, where the photothermal material is copper on a dielectric element made of titanium dioxide, a displacement element made of titanium dioxide on the photothermal material, and the displacement element is at least partially or completely in contact with the surface of the photothermal material, can exhibit an average absorption of at least 15% of incident electromagnetic radiation in the range of 820 nm (the minimum wavelength of the displacement of the range of interest) to the maximum wavelength of the range of interest (e.g., 2500 nm for solar applications). As another example, a percolation structure substantially at the percolation threshold, where the photothermal material is copper on a dielectric element made of titanium dioxide, a displacement element made of titanium dioxide on the photothermal material, and the photothermal material is at least partially or completely in contact with the surface of the photothermal material, can exhibit an average absorption of at least 17% of incident electromagnetic radiation in the range of 850 nm (the minimum wavelength of the displacement of the range of interest) to the maximum wavelength of the range of interest (e.g., 2500 nm for solar applications).
[0074] Furthermore, the heating device is preferably configured to absorb 15% or more, 25% or more, preferably 35% or more of the incident electromagnetic radiation in the near infrared region. To this end, it is preferred that the heating device comprises, for example, a photothermal element, which is arranged between two dielectric elements with respect to the extension direction, and wherein the dielectric element simultaneously corresponds to a displacement element, see also below. The "dielectric displacement element" can be, for example, titanium dioxide.
[0075] Furthermore, the displacement element is preferably optically transparent and / or dielectric.
[0076] The displacement element and the photothermal element are preferably associated in each case with a refractive index. The refractive index of the displacement element is preferably greater than the refractive index of air and / or greater than the refractive index of the photothermal element.
[0077] Therefore, the refractive index of the displacement element preferably differs from the refractive index of the photothermal element or from the refractive index of the surroundings, which leads to a change in the Fresnel coefficients and thus affects the optical properties of the heating device, ie the absorption and transmission behavior of the heating device.
[0078] The displacement element particularly preferably corresponds to the dielectric element mentioned above. That is, the displacement element and the dielectric element can be provided by a single element. However, it is also conceivable that the displacement element and the dielectric element are different elements. For example, in the latter case, it is conceivable that the heating device may include (in this order when viewed along the extension direction): a dielectric element (e.g., a titanium dioxide layer or a layer consisting of a high refractive index dielectric), a displacement element (e.g., a semiconductor layer made of Si, Ge or GaP, such as a photothermal element (e.g., a gold layer including a percolation structure at a percolation threshold)), another displacement element (e.g., a semiconductor layer and a dielectric element such as a titanium dioxide layer). In this case, it can be said that the two dielectric elements provide the top side and the bottom side of the heating device.
[0079] The heating device preferably further comprises at least one anti-reflection element, which is configured and arranged to reflect electromagnetic radiation towards the photothermal element.
[0080] The anti-reflection element preferably comprises two or more layers superposed on each other (ie stacked) with respect to the extension direction. In addition, these layers preferably have a gradually increasing refractive index with respect to the extension direction.
[0081] Furthermore, the antireflective element is preferably optically transparent and / or dielectric.
[0082] The anti-reflection element is preferably arranged before and / or after the photothermal element with respect to the extension direction. For this purpose, it is particularly preferred that the anti-reflection element provides the top side and / or the bottom side of the heating device. Therefore, if the heating device comprises one or more dielectric elements or displacement elements mentioned above, it is preferred that the anti-reflection element is arranged closer to the outside of the heating device than the dielectric element or the displacement element, respectively.
[0083] The heating device preferably further comprises at least one carrier element. The photothermal element is preferably arranged on the carrier element or at least partially embedded in the carrier element. If the heating device comprises one or more of the other components previously described (e.g. dielectric element, displacement element, anti-reflection element), it is preferred that these one or more other components are also arranged on the carrier element or at least partially embedded in the carrier element.
[0084] The carrier element is preferably bendable and / or flexible and / or deformable and / or foldable.
[0085] Furthermore, the carrier element may be optically transparent. Additionally or alternatively, the carrier element may comprise or consist of a solid (preferably an amorphous solid, such as glass) and / or one or more plastics and / or one or more polymers. For example, the carrier element may comprise or consist of an optically transparent and / or elastic plastic or polymer.
[0086] Furthermore, the carrier element is preferably a layer which is preferably further configured as a suspension, ie the carrier element is preferably a film.
[0087] The carrier element may be used for the purpose of applying or attaching the heating device to an end-user device, such as glasses that need to be protected from fogging or icing.
[0088] However, it should be noted that the application or attachment of the heating device to an end-user device does not necessarily require a carrier element. Instead, a direct application of the heating device (e.g. direct coating of the glasses with the photothermal element) is likewise conceivable. Providing a carrier element provides the possibility to retroactively attach the heating device to an already existing end-user device (e.g. glasses).
[0089] In another aspect, a method for producing a heating device for preventing or removing deposition, in particular for demisting (e.g., defogging), anti-fogging (e.g., anti-fogging), deicing or anti-icing, is provided. The heating device extends along an extension direction. The method comprises the step of providing at least one photothermal element, the at least one photothermal element being configured to exhibit a photothermal effect when irradiated with electromagnetic radiation. The photothermal element comprises or consists of a photothermal material, the photothermal material comprising a percolation structure. The percolation structure is at its percolation threshold or substantially at its percolation threshold.
[0090] The heating device preferably corresponds to the heating device described above. Therefore, any statements made about the heating device preferably also apply to the method for producing the heating device and vice versa.
[0091] The photothermal element is preferably produced by deposition, preferably by thin film deposition and / or vapor deposition. In fact, the photothermal element is particularly preferably produced by chemical vapor deposition and / or physical vapor deposition (e.g., sputtering deposition, thermal evaporation, molecular beam epitaxy, atomic layer deposition or pulsed laser deposition). Alternatively, the photothermal element is produced by chemical growth.
[0092] Additionally or alternatively, the photothermal element is preferably produced by island growth, wherein separate islands are initially formed by deposition and / or chemical growth, and wherein the separate islands gradually grow during a further deposition or growth process until a percolation structure is produced that is at or substantially at the percolation threshold.
[0093] For this purpose, it is particularly preferred that the photothermal element is produced according to the so-called Volmer-Weber growth process known in the art. In other words, the photothermal element is preferably produced by a random nucleation and growth process.
[0094] The photothermal element is preferably produced by deposition with a deposition rate in the range of 0.05 nm / s to 1 nm / s and / or during a deposition time in the range of 1 s to 150 s.
[0095] The photothermal element is particularly preferably produced by depositing at least one material, for example at least one electrically conductive material or at least one semiconductor. Preferred electrically conductive materials are electrically conductive metal compounds. As mentioned above, the metal compound can be an elemental metal or a metal alloy.
[0096] In a preferred example, sputtering deposition (using an Ardenne CS 320C) is used in a first step to form the dielectric element. For example, ~3 nm of titanium dioxide (TiO 2 ) layer: 600W Rf field, 6pbar pressure, 71s deposition time. Thereafter, a photothermal element (e.g. gold (Au)) can be produced by thermal evaporation (Evatec BAK501 LL) at a deposition rate of 0.05nm / s until an estimated optimal layer thickness of 4.75nm is reached. Finally, another dielectric element (e.g. another TiO 2 layer) to cover the infiltration Au layer.
[0097] To this end, it is particularly preferred that the photothermal element is produced by depositing the conductive material directly on a substrate (e.g., the aforementioned dielectric element, displacement element, carrier element, or end-user device). Therefore, counteracting surface fogging to maintain surface transparency is important for various applications including glasses, windows, or displays. Energy-neutral, passive methods mainly rely on designing surface wettability to prepare superhydrophilic or superhydrophobic coatings, but suffer from inhomogeneity, contaminant deposition, and lack of robustness, all of which significantly reduce their performance. Here, guided by nucleation thermodynamics, a transparent, sunlight-activated photothermal heating device is used to completely suppress fogging. In particular, the present invention provides a rationally designed photothermal heating device that can be only a few nanometers thick and has strong broadband absorption in the near-infrared region while maintaining high transparency in the visible region, taking an important step towards achievable transparent photothermal surfaces to cope with the removal of deposits such as fogging. Unlike previous work, the heating device according to the present invention strongly absorbs wavelengths invisible to the human eye while maintaining transparency in the visible range. Selective absorption of the near-infrared spectrum can be achieved by a single, easily fabricated metal layer with a thickness in the nanometer range, at or substantially at the percolation threshold [37-40], and optionally embedded in a dielectric host that can align the transparency peak of the photothermal heating device with the peak wavelength of solar radiation (occurring in the visible range). Due to its ease of design concept and its optical selectivity, the heating device can be ultrathin (~10 nm) and easily integrated onto existing structures over large areas and under additional standard coatings that are usually applied to transparent materials. This protects the heating device from outdoor influences such as chemicals, scratches or oxidation, making it durable. This thinness enables fabrication even on flexible substrates, with robust performance that can withstand damage that may be caused by multiple bending without loss of performance. Absorption and dissipation of near-infrared solar light has been exploited to prevent fogging (anti-fogging) and to achieve rapid recovery from a fogged state (defog) under non-ideal real-world outdoor conditions. The heating devices can be easily fabricated over large areas by standard methods (sputtering and thermal evaporation) and the material requirements are low, which lays the foundation for the potential of the heating devices to be used directly in applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0098] Some preferred embodiments of the present invention are described below with reference to the accompanying drawings, which are for the purpose of illustrating the current preferred embodiments of the present invention, rather than for the purpose of limiting the same. In the accompanying drawings,
[0099] 1a to 1d show schematic cross-sectional views of a heating device according to the present invention;
[0100] Figure 2 A scanning electron micrograph of a 15 nm thick gold layer is shown;
[0101] 3a to 3d show graphs depicting the absorbance ( FIG. 3a ), reflectance ( FIG. 3b ) and transmittance ( FIG. 3c ) of gold layers of varying thickness;
[0102] Figure 4 a to Figure 4 c shows a schematic diagram of the heating device ( Figure 4 a) A graph describing the maximum average near infrared absorption rate of the heating device ( Figure 4 b), and a graph describing the transmittance and absorptivity of the heating device ( Figure 4 c);
[0103] FIG5 a shows a schematic diagram of an experimental setup for simulating solar illumination of a heating device;
[0104] 5b to 5c show graphs depicting the photothermal performance of the heating device during solar illumination according to the experimental device of FIG. 5a ;
[0105] 6a to 6c show graphs depicting the anti-fog performance of a heating device, wherein FIG. 6a depicts a graph of the temperature and overpressure of the heating device over time, FIG. 6b depicts a sequence of recorded images of a control sample and a heating device according to the invention over time, and FIG. 6c depicts the fog fraction of a control sample and a heating device according to the invention;
[0106] Figure 7 a to Figure 7 e shows a graph and image depicting the defogging performance and real-world feasibility of the heating device, where Figure 7 a is a qualitative image sequence of a control sample and a heating device according to the present invention under 1 sun illumination, Figure 7 b plots the evolution of the fog fraction over time on a control sample and a heating device according to the invention, Figure 7 c depicts images of outdoor testing of spectacles lacking a heating device according to the invention and of spectacles comprising a heating device according to the invention at different locations and at various levels of solar irradiance, Figure 7 d depicts a bending test of a heating device according to the invention arranged on an overhead projector transparency, Figure 7 e depicts the arrangement according to Figure 7 d is an image of an outdoor test of a heating device according to the invention on an overhead projector transparency;
[0107] Figure 8 A graph depicting the temperature variation of nucleation rate with sample temperature is shown;
[0108] Fig. 9shows a graph depicting the optical characteristics of a heating device according to the invention comprising photothermal elements of different thicknesses;
[0109] Fig.10 Scanning electron microscope images of photothermal elements of different thicknesses are shown;
[0110] Fig.11 shows a graph depicting four-point probe measurements of photothermal elements of varying thickness;
[0111] Fig.12 shows a graph depicting the angular dependence of the transmittance of a heating device according to the invention;
[0112] Fig.13 The figure shows a depiction of bare fused silica (SiO 2 ) and the control sample (TiO 2 Graphs of advancing and receding contact angles of a heating device coated with fused silica) and according to the present invention;
[0113] Figs. 14a to 14c depict graphs and images of defogging experiments, wherein Fig. 14a depicts exemplary results of defogging experiments for a control sample and a heating device according to the present invention, Fig. 14b depicts a sequence of top-view images of the fogging area for the two exemplary experimental runs shown in Fig. 14a, and wherein Fig. 14c shows a graph depicting the defogging time required until fog covers <5% of the control sample and the heating device;
[0114] Fig.15 a to Fig.15 c shows an image of an outdoor test using a pair of vision glasses comprising a heating device according to the invention and lacking a heating device according to the invention;
[0115] Fig.16 a shows the experimental setup for outdoor experiments on photothermal effects;
[0116] Fig.16 b shows a graph depicting the temperature evolution of a control sample and a lens comprising a heating device according to the invention;
[0117] Fig.17 a to Fig.17 d shows the effect of arranging the heating device according to the present invention on a flexible substrate, wherein: Fig.17 a shows a graph depicting the transmittance and absorbance of a substrate (elevated slide) comprising a heating device before (solid line) and after (dashed line) 300 bending cycles and the transmittance of a bent sample, Fig.17 b shows Fig.17 The image of the curved sample (40°) presented in a, Fig.17c shows a photograph of a fully bent sample during a bending cycle, Fig.17 d shows a photograph showing the flexible substrate / foil being mounted on any existing glass to prevent fog formation or accelerate defogging;
[0118] Fig.18 a to Fig.18c The effect of the angular dispersion relation of the heating device according to the present invention is shown; Fig.18 a is a schematic diagram of a heating device according to the invention, the heating device comprising a gold layer at the percolation threshold, the gold layer being embedded between two titanium dioxide layers on a substrate in the form of silicon dioxide; Fig.18 b shows a scanning transmission electron microscope image (left) and an energy dispersive X-ray spectroscopy (right) of the heating device; Fig.18c shows a graph depicting the angular dispersion relation of the absorptivity for radiation incident angles of 0° to 30° to the normal to the heating device;
[0119] Fig.19 a to Fig.19 b shows a graph depicting the broadband absorptivity of the heating device according to the invention in the near infrared spectrum;
[0120] Figure 20a to Figure 20b : Fig.20a A bright field SEM image of a heating device comprising a photothermal structure at the percolation threshold is shown. The photothermal material is Au (black) and is surrounded by TiO 2 The SiO layer (dark gray) is uniformly surrounded. 2 The substrate is at the bottom, while the top is covered with carbon for easier imaging (both in light grey); Fig.20b High-resolution transmission electron microscopy is shown. The actual thickness of the Au layer (d Au =4.75nm) is estimated to be ~6nm to 7nm, TiO 2 2nm to 3nm (d TiO2 =3 nm). Scale bar: 10 nm;
[0121] Fig.21 Graphs depicting the angular dependence of the optical properties are shown. Measurements of incident radiation at 0 angle to the normal of the heating device are performed. The measured transmittance and reflectance are shown on the top and middle graphs, respectively. From these, the absorptance is derived and presented on the bottom graph;
[0122] Fig. 22 shows the visible transparency τ according to the material VIS and the solar absorption α of each layer thickness d (in nm) solar A comparison between the heating device according to the present invention and the photothermal anti-fog coating of the prior art;
[0123] Fig.23 The results of photothermal treatment under low levels of solar irradiance are shown. 0 Box plot of steady-state temperature rise under (including 0.2sun and 0.4sun) (n=5). The box plot contains the median, upper and lower quartiles and whiskers (1.5 times the interquartile range);
[0124] Figure 24a to Figure 24b shows an outdoor test of a heating device according to the invention with a pair of prescription glasses;
[0125] Figure 25a to Figure 25b shows an indoor test of a heating device according to the invention behind a triple glazed window;
[0126] Fig.26 Heating devices arranged on various polymer (including flexible) substrates are shown. Panel A) depicts the absorption α of the bare polymer (grey) and the coated substrate. Panel B) depicts an SEM micrograph of the fabricated heating device (without TiO for ease of imaging). 2 Top layer). Scale bar B): 100 nm;
[0127] Fig. 27 a to Fig. 27 b shows the thermal durability and wear resistance test. A) T s Evolution after ~1 sunlight exposure and 50 cycles. B) Absorption α before (grey) and after (dark grey) 50 temperature cycles;
[0128] Fig. 27 c to Fig. 27 d shows the thermal durability test. C) During the first 5 hours of the 63-hour sunlight exposure test, T s The evolution is higher than T amb D) Absorption α before (gray) and after (dark gray) 63 hours of sunlight exposure experiment;
[0129] Fig. 27 e to Fig. 27 f shows the abrasion resistance test. E) Transmission T of the heating device before and after the peel test, F) Transmission T of the heating device before and after the wiping test;
[0130] Fig. 27 g to Fig. 27 h shows the wear resistance test. G) Transmission T of the heating device before and after the abrasion wear resistance test, H) Transmission T of the heating device before and after the dripping sand wear resistance test. DETAILED DESCRIPTION
[0131] Various aspects of the heating device 1 according to the present invention will now be described with reference to the accompanying drawings.
[0132] According to the following Figures 1A to 1D The heating device 1 extends along the extension direction E and comprises at least one photothermal element 2, which is configured to exhibit a photothermal effect when irradiated with electromagnetic radiation. The photothermal element 2 is composed of a photothermal material, which comprises a percolation structure, and wherein the percolation structure is at its percolation threshold or substantially at its percolation threshold.
[0133] In the depicted embodiments, the heating device 1 is arranged in each case on a carrier element 7. Furthermore, in all depicted embodiments, the heating device 1 is provided as a layered structure. That is, the photothermal element 2 and the carrier element 7 are provided as a layered structure. Figures 1B to 1D Further components of the described photothermal element 2 are layers extending in a transverse direction T extending perpendicularly to the extension direction E.
[0134] like Figure 1A As indicated in , the heating device 1 may comprise at least one electrical element 3 configured to introduce an electric current into the photothermal element so that heat is generated by the photothermal element. In the depicted example, the electrical element 3 is an electrode arranged on the photothermal element 2.
[0135] As just mentioned, Figures 1B to 1D , other conceivable components of the heating device 1 are depicted. That is, the heating device 1 may also include at least one dielectric element 4. Here, two dielectric elements 4 are provided, wherein one of the two dielectric elements 4 is arranged before the photothermal element 2 with respect to the extension direction E, and the other is arranged after the photothermal element 2 with respect to the extension direction E. To this end, the dielectric element 4 and the photothermal element 2 are in full surface contact with each other.
[0136] The heating device 1 additionally comprises at least one displacement element 5, wherein the displacement element 5 is configured to shift the absorption capacity and / or transmission capacity of the heating device 1 with respect to the incident electromagnetic radiation towards shorter or longer wavelengths of the incident electromagnetic radiation. Figures 1B to 1D In the embodiment, the dielectric element 4 and the displacement element 5 are provided by the same element. That is, the dielectric element 4 corresponds to the displacement element 5 and vice versa. Figure 1D , the displacement element 5 can also be provided as an additional component. Furthermore, the dielectric element 4 does not necessarily correspond to the displacement element 5 in each case, but can only serve the purpose of electrically insulating the photothermal element 2, for example.
[0137] The heating device 1 may additionally comprise at least one anti-reflection element 6, which is configured and arranged to reflect electromagnetic radiation towards the photothermal element 2. Figure 1C and Figure 1D, in which an antireflection element 6 is arranged in each case in front of the other components of the heating device 1. In these cases, the antireflection element 6 provides the top side 8 of the heating device 1.
[0138] Despite Figures 1A to 1D Although not depicted in the drawings, the heating device 1 can be attached to or applied to a surface to prevent or remove deposits on said surface. The heating device 1 can therefore be regarded as a coating of said surface. Therefore, the expression "coating" used hereinafter should be understood as a heating device according to the invention.
[0139] Furthermore, the expression "metamaterial" is to be understood as a photothermal element comprising or consisting of a photothermal material comprising a percolation structure and wherein the percolation structure is at its percolation threshold or substantially at its percolation threshold.
[0140] Design of heating device
[0141] Figure 3a to Figure 4 c shows the design and optical characteristics of the heating device.
[0142] and Figure 2 Unlike the gold layer (having a thickness of 15 nm, flat and continuous, made of polycrystalline domains) depicted as a scanning electron micrograph in FIG, these heating devices include a photothermal element in the form of a gold layer, which includes a percolation structure and is associated with specific absorptivity, reflectivity and transmittance properties depending on the thickness of the gold layer. To this end, FIG. 3a depicts the absorptivity of different gold (Au) layer thicknesses (i.e., thickness parameter) embedded in 3 nm TiO on the top and bottom. 2 The spectrally resolved absorbance in the visible and near infrared shows a maximum in this region for a layer thickness parameter of 4.75 nm. Figure 3b depicts a 3 nm TiO layer embedded on the top and bottom 2 The spectrally resolved reflectivity increases as the film grows to form a continuous and flat mirror. Figure 3c plots the transmittance of different Au layer thicknesses (i.e., thickness parameters) embedded in two TiO layers on the top and bottom, each with a thickness parameter of 3 nm. 2 The spectrally resolved transmittance shows good transparency in the visible. Here the interband transition of gold is blocked by TiO 2 The matrix shifts to the red, with lower absorbance than the near infrared.
[0143] also, Figure 4a shows that NIR is absorbed and dissipated as heat by a heating device that is essentially transparent in the visible range (photothermal effect). The resulting increase in surface temperature prevents fogging. Figure 4 b shows the design of the heating device, focusing on optimizing the gold (Au) thickness d Au , to obtain the maximum average near-infrared absorptivity The maximum is located at the percolation threshold (ie, 4.75 nm thickness parameter). The grey curve is a spline fit to the data points. Three SEM micrographs of thin metallic Au layers indicate how at the percolation threshold (grey rectangles), disconnected clusters merge into larger connected patterns. Figure 4 c depicts the transmittance τ (black line) and absorptivity α (grey line) spectra of the heating device. The spectrum represents the AM 1.5 global solar reference spectrum. 49.9% of the solar irradiance is in the near-infrared (NIR) range, 45.5% in the visible (VIS) range, and 4.6% in the ultraviolet (UV) range. The inset shows the effect of a normal glass slide (silicon dioxide, SiO2) on the thermal conductivity of the substrate compared to the heating device (right). 2 , left) Transparency. Scale bar B): 100 nm, C) 5 mm.
[0144] Therefore, if Figure 4 As shown in A, in order to effectively collect solar energy to cope with fogging and at the same time maintain transparency, the design of the coating (i.e., the design of the heating device according to the present invention) targets high broadband absorption in the near infrared (NIR, λ = 720nm to 2000nm) solar radiation spectrum and high broadband transparency in the visible spectrum (VIS, λ = 400nm to 720nm). In fact, the NIR solar spectrum accounts for 1.5% of the incident solar irradiance I 0 50% of the sample temperature, and therefore offers great potential for collecting solar energy that is invisible to the human eye. Once the solar energy is absorbed, it dissipates itself as heat, raising the sample temperature T s Increase to ambient temperature T amb above, thus reducing the risk of fogging and maintaining its transparency in the VIS spectrum. Given the highly sensitive dependence of the condensation nucleation rate on temperature [41-44], this thermodynamic approach is powerful and, unlike many existing methods, does not rely on chemistry [45-47]. s A small increase in is sufficient to reduce the droplet nucleation rate exponentially, thereby reducing the probability of a nucleation event by several orders of magnitude (see Figure 8). The maximum temperature increase is achieved when the photothermal coating (i.e., the heating device according to the present invention) has a strong broadband absorption in the NIR spectrum. Previous work has demonstrated that good NIR absorption can be achieved with metal particles. Metal particles show strong light absorption due to their large cross-section at the plasma resonance frequency in the VIS spectrum, and this narrow-band absorption can be extended to the NIR over a wider spectrum by mixing metal nanoparticles of different sizes and shapes [10, 17, 23, 48]. In addition, it has been shown that structured particles can be used to selectively absorb the NIR spectrum. However, these particles are narrow-band absorbing and require complex, sensitive manufacturing [49-51]. In contrast, the idea of a single thin metal layer at or substantially at the percolation threshold has been proposed. In this state, disconnected clusters of individual nanoislands merge into larger connected patterns. This leads to delocalized surface modes that lead to strong broadband absorption of incident radiation in the NIR [52, 53], which is subsequently converted into heat. To realize this concept, a thin layer of gold (Au) was deposited using commercial technology (thermal evaporation) and the thickness of this layer was d Au Tuned to be at or substantially at the percolation threshold (see Figures 9 to 11 ).
[0145] Figure 4 B shows the average NIR absorbance How to use the thickness parameter d Au =4.75nm. There, the strong and broad light absorption matches the electroosmotic threshold. Au At higher temperatures, the layer becomes more metallic and loses its broadband absorption behavior. Figure 4 The top-down scanning electron microscope (SEM) micrograph in B reveals how smaller, disconnected clusters coalesce into larger, meandering connected patterns at the percolation threshold. This optimized thin Au layer is encapsulated between two high-refractive-index dielectric layers (titanium dioxide, TiO 2 , each with a thickness of ~3nm) to protect the percolation layer from oxidation. In addition, due to the TiO 2 Due to the large refractive index of these layers, the light absorption of the 3-layer heater (~10 nm thick) is shifted to longer wavelengths
[54] . The spectral response of the fabricated heaters was measured and their optical properties were determined. Figure 4 C confirms the high transmittance (τ VIS =67.1%), the transmittance is related to the solar irradiance I 0 The peaks of are well aligned. The randomness of the percolation pattern further makes the transmittance independent of the incident angle of the incident light ( Fig.12 At the same time, the heating device exhibits strong broadband absorption in the NIR (α NIR=36.9%). Apparently, at the percolation threshold, the plasmon resonance (which typically causes strong local absorption at the resonant frequency) is replaced by broadband absorption below the resonant frequency (i.e., in the NIR spectrum). Likewise, the heating device remains transparent to shorter wavelengths in the VIS spectrum because it remains optically thin. The strong transmittance near λ = 550 nm originates from the interband transitions of gold [55, 56]. There, the structural absorption in the NIR caused by percolation is stronger than the interband transitions of the film in the visible. Thus, the heating device collects nearly 30% of the incident solar energy (280 nm to 2000 nm) in only ~10 nm while remaining transparent.
[0146] Next, the photothermal performance of the heating device was evaluated. This will be discussed with reference to FIG5 , which depicts the experimental setup and the photothermal performance. In particular, FIG5a depicts a schematic diagram of the experimental setup. The samples (control and heating device coating, i.e., the heating device applied to the substrate, here the substrate is SiO 2 ) is illuminated by a solar simulator with an irradiance of 600 Wm -2 Up to 1000Wm -2 (corresponding to 0.6 to 1 sun). A color camera and its objective lens image the fog formation on the coated bottom surface of the sample. Warm steam diffuses from a copper tube to the surface of the sample at a controlled temperature.
[0147] In particular, the fused silica (SiO 2 ) substrate under simulated sunlight (see Figure 5A The surface temperature T under the experimental setup shown in s As a control sample, the SiO 2 ~3nm TiO is deposited on the substrate 2 thin layer to produce the same wetting behavior as the heating device ( Fig.13 ). Place the sample on the sample holder so that the coated side of the substrate faces downward. Irradiance I 0 Use the shutter control of the solar simulator. 1sun (corresponds to 1000Wm -2 ) 0 produces the highest measured photothermal response. However, under outdoor conditions, I 0 Usually less than 1sun. Therefore, 600Wm is also recorded -2 and 800Wm -2 The temperature response of the weaker irradiances (corresponding to 0.6sun and 0.8sun, respectively) is shown in Table 1. Figure 5B , under 1sun illumination, coated on SiO 2 The heating device on the substrate shows the strongest temperature increase above the ambient temperature (T s -T amb). Although under 1sun illumination, T s The temperature rises to above ambient temperature (T amb ≈23℃, RH≈55%)8.3℃, but SiO 2 The heating device on the substrate also heats up significantly at weaker irradiances (5.4°C and 6.4°C at 0.6sun and 0.8sun, respectively). Note that this increase is sufficient to reduce the condensation nucleation rate by several orders of magnitude (see Figure 8 ). The experimental observations agree well with the transient heat transfer model used to validate the temperature measurements. In this model, only the convective heat transfer coefficient h conv In a reasonable range
[57] (8.5Wm -2 K -1 Up to 10.5Wm -2 K -1 ) to fit the experimental data (see Supplementary Note 4). Figure 5C Summarizes SiO 2 The steady-state temperature rise of the heating device on the substrate and the control sample (t = 230s) demonstrates the significant photothermal response of the former. 2 The heating devices on the substrates were largely at least 5°C hotter than the control samples.
[0148] Then, referring to Figures 5b and 5c, the SiO 2 The performance of the heating device on the substrate against surface fogging (anti-fogging) was tested. That is, Figure 5b depicts the average temperature increase (dashed line) and standard deviation (shaded area) of the surface under solar illumination from 0.6 sun to 1 sun. The solid line represents the transient heat transfer model of the temperature, which is in good agreement with the experimental results. Figure 5c depicts the temperature rise of the surface under different solar irradiances I 0 (0.6 to 1 sun), SiO 2 Box plot of the steady-state (t=230s) temperature rise of the heating device and the control sample on the substrate. For this purpose, a heated copper tube was installed in the experimental setup, which was connected to a bubbler filled with water and a gate at the tube outlet. Figure 5A As shown in , the vapor hits the sample surface from the same side as the sample is illuminated. The vapor temperature T v It is controlled by a copper tube (surrounded by a heating cable) and is measured in close proximity to the sample. At the beginning of each experimental run, T v and T s ≈T amb Knowledge of allows calculation of the saturated vapor pressure p of the air in the immediate vicinity of the sample sat (Arden-Buck equation
[58] ), and the vapor pressure p of the transported humid air v .
[0149] FIG6 shows the anti-fogging performance. In fact, FIG6a depicts the sample temperature T during the duration of the exemplary experiment. s (coated with heating device) and overpressure p v -p sat First, the sample is irradiated by a solar simulator (1 sun is used here). After 2 minutes of sunlight exposure, the steam gate is opened for 5 seconds to expose the sample to steam. Subsequently, the gate is closed for 20 seconds to make the overpressure (p v -p sat ) to its initial state. For each experiment, the sequence was repeated 5 to 7 times. The sequences were then averaged to provide a mean and standard deviation. Fig. 6A As shown, T air and p v -p sat The peak value is reached and then equilibrates back to its initial value within ~15 s. At the same time, the condensation formation on the surface of the sample is recorded. Dark field imaging of the fog allows the identification of areas of the sample where droplets are formed. The presence of small droplets on the surface backscatters some of the incident light and provides good brightness on the camera device. The recorded images are then binarized with respect to their brightness to quantify the area covered by the fog, i.e. the fog fraction of the surface. Here, A fog is the area covered by fog, A sample is the total area of the sample.
[0150] Figure 6b depicts the results of the control sample and SiO 2 Sequence of images recorded over time of a heating device on a substrate. Shown is the considered area A of the sample sample , A sample Before opening the gate (t = 5s), the control sample and SiO 2 The heating devices on the substrate are completely free of fog (f = 0). That is, at t = 5s, both samples are completely free of fog (f = 0). After opening the steam gate, the samples begin to fog and reach their peak fog fraction. For this reason, at a comparable pressure difference p v -p sat Under the conditions of 1.56 kPa and 1.62 kPa respectively, the fog fraction f increases gradually and reaches its peak value at t = 10 s, where f = 1 for the control sample and 2 The value of the heating device on the substrate is one order of magnitude lower (f = 0.12). After 20 seconds (t = 25 s), SiO 2The heated device on the substrate was completely fog-free, while the control sample still needed more time to fully recover its initial state before its next cycle. To quantify this impressive anti-fog performance, the v -p sat Further experiments were carried out under 30° and 40° sun illumination (0.6sun, 0.8sun and 1sun).
[0151] For each experimental run, an overvoltage p was provided v -p sat and the measurements of the fog fraction f, the average values and the corresponding standard deviations.
[0152] Figure 6c plots the v -p sat At the horizontal level, SiO 2 Fog fraction f of the heater coating and control sample on the substrate. The inset table indicates that at all illumination levels, the SiO 2 The anti-fogging property of the heater coating on the substrate is improved by more than 4 times compared to the control sample. Scale bar B): 5 mm. Figure 6C As shown in the figure, the experimental results follow a linear trend. 2 The heating device on the substrate is more resistant to fogging than the control sample, which is evident in the overpressure value at which fogging begins (f>0) and the significantly smaller slope at partial fogging. The linear fit allows the determination of the corresponding overpressure when the sample is completely fog-free (f=0) and completely fogged (f=1). v -p sat These values estimate the SiO 2 The heating device on the substrate has improved anti-fogging compared to the control sample. Figure 6C The insertion table indicates that the v -p sat When f=0.67, 0.69 and 0.78 (0.6, 0.8 and 1 sun), respectively, the control sample is completely covered by fog (f=1). 2 The heating device on the substrate is only v -p sat When the f = 1, SiO2 is completely fogged (f = 1) when the f = 2.76, 2.91 and 3.82 (0.6 sun, 0.8 sun and 1 sun) respectively. This means that compared with the control sample, SiO2 is completely fogged (f = 1) when the f = 2.76, 2.91 and 3.82 (0.6 sun, 0.8 sun and 1 sun) respectively. 2 The heating device on the substrate can withstand a higher overpressure of 4.12 to 4.9, which means that the anti-fog performance is improved by more than 4 times.
[0153] After the anti-fog experiment, the SiO 2The defogging performance of the heating device on the substrate was evaluated, i.e., the restoration of visibility after the surface was completely fogged. For this purpose, the control sample and the SiO 2 The heating device on the substrate was cooled down to 2°C for 2 minutes until condensation formed under ambient conditions (Tamb≈23°C, RH≈55%). The sample was then immediately placed on the experimental device (see Figure 5A ) and illuminated it with sunlight while recording the evolution of fog on the surface.
[0154] Figure 7 Defogging performance and real-world feasibility are shown. Figure 7 A shows a qualitative image sequence of a control sample and a sample coated with a heating device under 1 sun illumination (Tamb≈23°C, RH≈55%) for t=0s to 150s. 2 The heater coating on the substrate completely defogged in less than 150 seconds and defogged to a large extent (f≈0.25) in less than 100 seconds, while the control sample mostly remained fogged for the same duration. That is, at t=150 seconds, although the control sample was still covered with fog, the SiO 2 The heater coating on the substrate has fully recovered its transparency. The small size of the condensed droplets leads to large scattering and therefore the image of the sample is very white in dark field imaging, clearly discernible in the control image at t = 0 s. The defogging front of the heater-coated sample proceeds faster than that of the control sample (see Figure 14). Experiments at different illumination levels, combined with videos of the recorded backscattered light (Tamb ≈ 23 °C, RH ≈ 55%), provide a more thorough quantification of the defogging dynamics.
[0155] like Figure 7 The evolution of the fog fraction f over time is extracted from this data, as shown in B. That is, Figure 7 B depicts the control sample and SiO 2 Evolution of the fog fraction f over time on the heating device coating on the substrate. The latter starts to defog much earlier and much faster (steeper slope) than the control sample. d Reduce by 2 to 3 times. Defogging time t d is defined and determined as the time required until f < 0.05, i.e., the time required for the sample to be covered with less than 5% fog. The control sample remained completely fogged for a longer time (f ≈ 1), and its defogging rate ( Figure 7 B) is much slower. Specifically, for the given experimental conditions and under 1 sun illumination, the average defogging time of the sample coated with the heating device is Compared with the control sample The contrast is 3 times better. The same trend is also shown in weaker light. There, at 0.8sun and 0.6sun They were reduced by 2.12 times ( right ) and 2.08 times ( right ).
[0156] With the knowledge of this improved anti-fog / defog performance, the real-world feasibility of the heating device was tested in outdoor conditions. To this end, one lens of a pair of prescription glasses was coated with a heating device and placed outdoors on a clear winter day. After 5 minutes of sunlight exposure, the glasses were put on and a suitable mask (FFP2) was worn to exhale, simulating the real-world conditions experienced every day recently. The warm breath was like a supersaturated steam stream, impinging on both the uncoated lens (at ambient temperature) and the lens coated with the heating device (due to the photothermal effect, the temperature was significantly higher than the ambient temperature).
[0157] Figure 7 C shows the results at two different locations. In particular, Figure 7 C depicts the solar irradiance at different locations and at various levels (top I 0 =212Wm -2 , Bottom I 0 =339Wm -2 ). The left lens of the glasses is coated with a heating device, which maintains its visibility even under moist human breath escaping upward from the mask, while the uncoated lens fogs up. Clearly, the strong anti-fog / defog performance enhancement is evident even in these non-ideal conditions. Fig.15 and Fig.16 Further outdoor experiments performed at different locations as well as outdoor temperature measurements of coated and uncoated lenses can be found in .
[0158] Finally, the suitability and effectiveness of the heating device in preventing the flexible material from fogging was tested. Figure 7 D shows that Figure 7 D depicts a bending test of an overhead projector transparency coated with a heating device.
[0159] To this end, a polyester sheet (overhead projector transparency) was coated with a heating device and the optical properties of the coated sheet were measured. Figure 7As shown in D, the sheet was bent 300 times before the optical properties were measured again to test its robustness to severe repeated deformations. Since the coating is only ~10nm thick, the relatively very large radius of curvature produced by the bending deformation will neither cause mechanical damage nor degrade the optical properties of the heating device coating (the random arrangement of metamaterials, i.e., photothermal elements including or consisting of photothermal materials, the photothermal materials including percolation structures, and wherein the percolation structures are at their percolation threshold or substantially at their percolation threshold, is on the order of several hundred nanometers, which is also much smaller than the bending curvature radius). Therefore, since the heating device is thin, the heating device is resistant to severe deformations and is easily applicable to flexible, foldable and portable substrates. In addition, the heating device can be arranged on any portable, flexible / foldable material and retroactively attached to existing surfaces (e.g., windows, covers or glasses).
[0160] The feasibility of this approach was further confirmed by attaching a polyester sheet to a fused quartz wafer coated with a heating device and testing the anti-fogging / defogging performance when breathing on the wafer and coating multiple times in a mountainous area. Figure 7 E(or Fig.17 ), the coated transparent sheet defogging is much faster and proves its feasibility in harsh outdoor conditions. Figure 7 E depicts outdoor testing demonstrating that a high-beam transparency with a heating device coating can be installed on any existing glass to prevent fogging or accelerate defogging. Scale bars A): 5 mm, C) and D): 10 mm, E): 20 mm.
[0161] Thus, an ultrathin heating device with high transparency in the VIS spectrum and strong absorption in the NIR is presented. 2The structural percolation effect of the metallic Au nanofilm between the nanolayers (giving the heating device a total thickness of ~10 nm) achieves spectral selectivity and broadening of the absorbance in the NIR. Due to its ultra-thin nature and its standard manufacturing process, the heating device can be easily scaled up and has the potential to be applied over a large area or integrated into existing multilayer coatings to increase anti-fogging functionality. Under 1 sun illumination, the light absorption caused by the percolation of the metallic Au film leads to a photothermal response, which increases the temperature to up to 8.3°C above the ambient temperature. This thermal response is used to exponentially reduce the nucleation rate of water vapor nucleation and improve anti-fogging (anti-fogging) by nearly 4 times. In addition, the recovery of visibility of the fully fogged coated sample is up to 3 times faster (defog) compared to the uncoated control sample. Importantly, it has been shown that the heating device performs well even under more challenging conditions (e.g., 0.6 sun illumination or 0.8 sun illumination). The real-world performance of the heating device has also been verified by applying the heating device to prescription glasses and demonstrating the impressive anti-fogging effect of the heating device under realistic outdoor conditions. Finally, the ultrathin design of the heating device enables its easy application on flexible, foldable, and portable substrates, and the heating device perfectly maintains its optical and photothermal properties even under and after intense and repeated bending.
[0162] method
[0163] Sample preparation and optical characterization
[0164] To fabricate the heating device and control samples, 500 μm thick JGS2 fused quartz wafers were used as substrates (UniversityWafer Inc.), cut into 22x22 mm squares. All specimens were cleaned by ultrasonic treatment in acetone and rinsed with isopropanol and deionized water for 2 min. Finally, they were exposed to oxygen plasma for 5 min (Oxford Instruments, Plasmalab 80Plus).
[0165] Next, the heating device and the control coating were generated by deposition:
[0166] Heating device: First, a titanium dioxide (TiO 2 ) layer with the following parameters: 600W RF field, 6pbar pressure, 71s deposition time. Shortly thereafter, gold (Au) was thermally evaporated at a deposition rate of 0.05nm / s until the estimated optimal layer thickness was reached (i.e., a thickness parameter of 4.75nm (EvatecBAK501LL)). Finally, another TiO 2For the parametric study, the TiO 2 The final step of deposition allows for four-point probe measurements.
[0167] Control sample: For the control sample, TiO 2 layer (~3nm), the TiO 2 The layers had the same parameters as used for the heating device fabrication.The transmittance and reflectance were measured at normal incidence (0.25 μm to 2.0 μm) using a LIV / VIS NIR spectrometer (Jasco, V770) and an ILN-925 integrating sphere.
[0168] The average transmittance in the visible light is determined as Among them, τ(λ) and I 0 (λ) represent the measured spectral transmittance and AM 1.5 global solar irradiance (see Figure 1C ). For VIS spectroscopy, select λ start =400nm and λ end =720nm. Similarly, the average absorbance in the NIR is calculated Where α(λ) is the measured spectral absorbance, λ start =720nm and λ end =2000nm.
[0169] Experimental setup
[0170] In order to evaluate the anti-fogging and defogging performance, a dedicated experimental setup was developed (see Figure 2 A). The sample is placed upside down on a U-shaped sample holder (polymethyl methacrylate ground plate, foam on top, opening width: 18×18 mm). A solar simulator (Newport, 66984-300XF-R1) equipped with an air mass filter (AM1.5 Global) simulates sunlight. The shutter and aperture at the simulator opening allow precise timing of the start of the experiment and the area on the irradiated sample. The sunlight is deflected towards the sample under investigation by a mirror. A CMOS color camera (FLIRBFS-U3-51S5C-C) with an objective lens (MVL7000-18-108 mm) images the sample. The solar irradiance ranges from 600 Wm -2 Up to 1000Wm -2The bubbler was adjusted and measured at the same position and height as the sample using a thermal power sensor (Thorlabs S425C and PM100USB controller). For experiments involving fog, the inlet of the bubbler was connected to a nitrogen (N2) supply (2.5 bar pressure, reduced pressure with a Swagelok pressure valve) and filled with water. The outlet of the bubbler was connected to an insulated copper tube (outer diameter: 1 cm), and its temperature was controlled by a heating cable (Horst TM 020101, 0.6m, 75W and Horst TM 060271, HTMC1 / controller), where the feedback signal comes from a resistance temperature detector (RTD, PT100). The bubbler is placed in a pot full of water, which is heated by a hot plate (VWR, Advanced Series 444-0592). The pot full of water is heated to a temperature higher than the desired steam temperature in the copper tube to ensure that the steam is always saturated. The glass slide at the outlet of the copper tube acts as a steam gate. Five different temperatures are recorded simultaneously, namely: the temperature of the ambient air, the sample, the air / steam just below the sample (where condensation occurs), and the steam at the outlet of the copper tube (all of which are measured using a PT1000 sensor). In addition, the temperature in the water pot is recorded using a PT100 sensor. All sensors are connected to a LucidControl RI8 USB logger. All temperature sensors were calibrated (Fluke 9142) before the experiment.
[0171] Using this equipment, two different types of experiments can be performed:
[0172] Anti-fog: Place the corresponding sample on the sample holder and start recording the temperature. After 10 seconds, open the gate of the solar simulator. After 2 minutes of sunlight exposure, turn on the N 2 The valve was closed and the steam gate remained closed. The system was allowed to equilibrate for another 2 minutes before starting the experiment. The sample was exposed to the steam flux for 5 s, then the gate was closed for 20 s, and this sequence was repeated 5 to 7 times while the surface was recorded by a CMOS camera.
[0173] Defogging: Place the Peltier module (Laird MS2-192-14-20-11-18) on an optical bench (heat sink) with thermal paste. Next, supply 2.8V, which causes the Peltier module to freeze under ambient conditions (T amb The cold side temperature was 2°C with a RH≈23°C, RH≈55%). The ambient condensate was then removed from the Peltier and the sample was placed on a dry surface. After 2 minutes, the sample was lifted and placed on a sample holder that had been exposed to sunlight. The time evolution of the fog on the surface was recorded by a CMOS camera.
[0174] Binarization
[0175] All frames (captured by the CMOS camera) of the partially fogged control sample and the heated device coated sample were binarized to quantify the temporal evolution of the fog fraction f. Using a dark field optical configuration, condensation droplets in the fogged areas backscatter the incident light and appear bright, while the transparent fog-free areas remain dark. The binarization threshold was set so that the fog-free (reference) surface had f = 0, while the fully fogged and white areas had f = 1. The binarization level was manually initialized to a reasonable threshold and took into account the hole-like pattern.
[0176] Linear fitting of anti-fog experiment
[0177] To determine the overpressure when the sample is completely fog-free (f=0) and completely fogged (f=1), a linear regression was performed on the experimental data. Since the fog fraction f ranges from 0 to 1, all data points with average fog fractions f<0.05 and f>0.95 were excluded for the linear fit.
[0178] Outdoor testing
[0179] The heating device was applied to the left lens of prescription glasses (Rodenstock (Schweiz AG)) with the same parameters as above. In the experiment, the glasses were first exposed to sunlight for ~5 min. Next, the operator put on a mask (FFP2) and carefully adjusted its nose pads so that the left and right spaces were almost the same. Finally, the operator put on the glasses, took a deep breath and exhaled while recording the fog formation on the glasses (Samsung Galaxy S20, Canon EOS 5D Mark4). The glasses were tested at multiple locations. Global horizontal irradiance (GHI) data were taken from MeteoSwiss, while humidity and temperature data were taken from MeteoSwiss or timeanddate.de.
[0180] Supplementary Note 1: Effect of sample temperature on nucleation thermodynamics
[0181] Based on the classical nucleation theory, the variation of the Gibbs free energy of a spherical nucleus with its radius r during homogeneous nucleation was calculated
[42] :
[0182]
[0183] Where nL(=3.35×10 28 m -3 ) is the number of water molecules per unit volume, k is the Boltzmann constant, p is the water vapor pressure of the environment, and pL is the temperature T (here, the sample temperature T s ) Saturated vapor pressure on the horizontal surface below, γLV (=72.75×1O -3 N m1 ) is the surface tension of liquid water in air. p and p L It can be calculated using the Arden-Buck equation
[58] . For p, the saturated steam is assumed to be at a temperature corresponding to the human / breath impact sample (i.e., relative humidity RH = 100% and T = 36°C), simulating the real-world conditions experienced recently when wearing glasses and masks every day. At the same time, p L With the sample temperature T s Finally, to account for the presence of insoluble flat surfaces that promote heterogeneous nucleation, Eq. (S1) can be modified as follows
[42] :
[0184]
[0185] in, yes function of
[44] , i.e., the contact angle of water on a flat surface The cosine of .
[0186] You can set To determine the critical radius r that the nucleus needs to overcome to grow into a larger droplet * , which yields
[42] :
[0187]
[0188] r=r * The corresponding critical Gibbs free energy can be obtained by substituting equation (S3) into equation (S2) and is
[42] :
[0189]
[0190] Finally, the nucleation rate (J) (i.e., the probability of a nucleation event occurring per unit surface area) is given by the following equation
[42] :
[0191]
[0192] Among them, the kinetic coefficient J 0 It can be determined as
[42] :
[0193]
[0194] Here, n′(I) represents the density of adsorbed molecules on the nucleation surface. For the condensation process, the kinetic coefficient can be approximated as 41,43 :J 0 ≈10 29 m -2 s -1 .
[0195] Figure 8Plotting the nucleation rate J as a function of sample temperature T s and shows how J changes with the sample temperature T s The slight increase of T and the significant decrease of T in equation (S5) s The inverse exponential dependence of leads to a sharp decrease in the nucleation rate. For example, T s Increasing from 20°C to 22°C results in a 5-order-of-magnitude decrease in J. In particular, T s A slight increase in leads to an exponential decrease in the nucleation rate. This demonstrates the significant impact of the heating device on anti-fogging / defogging applications due to its photothermal properties. The environmental conditions were set to relative humidity RH: 100%, T = 36°C, representing saturated human breath.
[0196] Supplementary Note 2: Characteristics of the heating device
[0197] A parametric study was performed by varying the thickness of the deposited gold layer (Au) to determine the thickness parameter for which this layer has the best overall absorption. To this end, different thicknesses of Au (for thickness parameters, see “Methods” above) were deposited on a 3 nm TiO 2 Then another 3nm TiO 2 The Au layer was covered with a layer of Au (see Methods). Next, the transmittance (T) and reflectance (R) of all samples were measured (measured at normal incidence using Jasco, V770 and ILN-925 integrating spheres) shortly after deposition, and the absorbance (α=1-τ-R) was determined (within 200nm to 2000nm wavelength).
[0198] Fig. 9 Depicted is the embedded 3nm TiO 2 Optical properties of different Au layer thicknesses for the top and bottom layers. The absorptivity of the Au layer reaches its maximum at a thickness of 4.75 nm and decreases with further increase in thickness due to enhanced reflectivity. The arrows indicate the trend with increasing Au film thickness. That is, Fig. 9 It is shown how increasing the thickness of Au decreases τ and increases R for temperatures above the plasma frequency (~580 nm). Interestingly, α increases for Au up to 4.75 nm, at which point the absorptivity reaches a flat broadband behavior in the NIR. Fig. 9 As indicated by the arrow in , increasing the Au film thickness further leads to a decrease in α (optical thickness, metallic behavior) due to the increase in R.
[0199] The percolation limit was further confirmed using a scanning electron microscope (SEM, Hitachi SLI8230). Fig.10Scanning electron microscope images of different Au thicknesses are shown in . In these SEM images, the thickness parameters are 2nm, 3nm, 4.75nm and 7nm. Below the percolation threshold (2nm and 3nm), Au nanoparticles form individual unconnected islands. The interconnection between individual clusters is reached at 4.75nm. That is, at the threshold (4.75nm), the islands are interconnected. Above the threshold (7nm), Au starts to form a continuous layer. Scale bars (A), (B), (C), (D): 100nm.
[0200] In addition, the electroosmotic flow limit was determined by four-point probe measurements (Jandel Universal Probe Station) to determine the resistance R of the Au layer for different Au thickness parameters. el . Set the current to 4.53×10 -6 A, and increased to 4.53×10 -5 A and 4.53×10 -4 A, Voltage is measured simultaneously at different points on each sample. Fig.11 The resistance of the Au layer is shown on a logarithmic scale, where each circled dot represents a data point. For a continuous layer (30 nm of Au), the Au layer is very conductive (metal), and the resistance increases towards the percolation threshold until it becomes an open circuit (dielectric). The thickness parameter d is also measured. Au = R at 2nm, 3nm, 4nm, 4.25nm and 4.5nm el , but R el increases to infinity, that is, the film is non-conductive. Therefore, with a thickness d Au The film acts as a conductor up to the percolation limit. Au =4.75nm, resistance R el The increase was several orders of magnitude, indicating dielectric behavior and that the individual Au particles were not electrically connected.
[0201] The fabricated heating device coatings (Au with a thickness parameter of 4.75 nm, TiO with a thickness parameter of 3 nm) were further quantified. 2 The angular dependence of the transmittance of the bottom and top layers is shown for incident angles up to 45°. Fig.12 It is shown that there is no dependence of τ on the angle of incidence of the incident light. Due to the grating variation of the LIV / VIS NIR spectrometer, distortion occurs between 600 nm and 900 nm.
[0202] Supplementary Note 3: Contact Angle Measurement
[0203] The uncoated substrates (fused silica, SiO 2 ), control sample (TiO 2 Coated fused silica), and the advancement of metamaterials (i.e., heater coatings) and Back Contact angle. Fig.13 The results for all samples are summarized in , with a total of 5 measurements (N=5) performed on each sample. For the control sample and the heating device coating, and This is important to exclude any effect of wettability on the antifogging / defogging behavior during the experiments. 2 Compared with SiO 2 The surface energy of SiO is high. 2 The contact angle indicates its hydrophilicity In contrast, the contact angle of the control surface Contact angle of the heating device coating Very close.
[0204] Supplementary Note 4: Transient Heat Transfer Model
[0205] The temperature evolution of a sample with metamaterial (i.e., with a heater coating on top) under solar illumination is estimated using a transient heat transfer model:
[0206]
[0207] Here, m is mass, c(=750JkgK -1 ) is the specific heat capacity, T s is the sample temperature, A is the surface area of the sample (22×22 mm), is the average absorptivity in the solar spectrum (λ = 200 nm to 2000 nm) and ε (≈1) is the thermal emissivity of the sample. 0 Indicates solar irradiance (from 600Wm -2 Up to 1000Wm -2 Changes), where the AM 1.5 Global (ASTM G173) reference spectrum is used. amb is the ambient temperature (constantly set to 25°C), h conv is the convective heat transfer coefficient. To estimate the Biot number, h conv Set to a reasonable value, approximately 10Wm -2 K -1
[57] , and later verified this hypothesis experimentally (see below). From this, the Biot number over the substrate thickness was determined to be Here, d = 0.5 mm represents the sample thickness, λ cond ≈1Wm -1 K -1 represents the thermal conductivity of the substrate (fused silica). Even for larger convective heat transfer coefficients, e.g., h conv ≈30Wm -2K -1 , Bi≈0.075<<1. 0 is uniform over the sample area (collimated light source, verified by thermal power sensor (Thorlabs S425C and PM100USB controller)) and Bi<<1, so the sample can be assumed to be isothermal.
[0208] The term on the left side of equation (S7) represents the rate of change of energy inside the sample, and the right side of the equation contains the term of absorbed solar heat, and it also takes into account reradiation to the environment and convective heat loss. Since the temperature rise of the sample above the ambient temperature is less than 10°C (i.e., dT = (T s,eq -T amb )< <T amb ), so the Taylor series expansion is used to linearize the radiation heat transfer term and remove all high-order terms to avoid T s Solving equation (S7) yields the transient sample temperature:
[0209]
[0210] in,
[0211] In order to verify the initial conv Based on the conjecture, h is experimentally determined using the lumped sum capacitance model. conv To do this, the sample is first exposed to sunlight until T s Reaching a steady state (T s =T s,eq ). Next, the solar simulator was turned off and the temperature decay of the sample was recorded for three experimental runs, from which the average value was determined. Since the solar heat term in equation (S7) disappeared in these experiments, the solution simplifies to:
[0212]
[0213] Equation (S9) allows to change h conv (and thus change C 2 ) to fit the experimental data of temperature decay measurement. It is found that h conv The best fit value is approximately equal to 9.15Wm -2 K -1 , which verifies the initial guess. Therefore, based on this value, the model is compared with Figure 2 Experimental data of temperature rise of samples under sunlight (8.5≤h conv ≤10.5Wm -2 K -1 ) for fitting.
[0214] Supplementary Note 5: Defogging behavior
[0215] The defogging behavior of the control sample and the coating is further shown in FIG. 14 .
[0216] Fig.14A An exemplary result of the time evolution of the fog fraction f is shown, where SiO is illuminated with 1 sun. 2 Heating device coating and control samples on substrates (for experimental procedures and binarization, see “Methods”). Fig.14A As can be seen in Figure 2, for the metamaterial (i.e., the sample coated with the heating device), defogging starts much earlier due to the higher surface temperature. 2 The fog fraction f on the heater coating on the substrate decreases much faster than on the control sample.
[0217] Fig. 14B The qualitative behavior is demonstrated by a sequence of top-view images of the fogged area at fog fractions f = 0.75, 0.5 and 0.25, respectively, for two exemplary experimental runs shown in A). The dashed rectangle indicates the considered sample area for which f is to be calculated. To defog 75% of the surface, the sample coated with the heating device required 107 seconds, while the control sample reached this value after 342 seconds (more than 3 times as long). That is, the SiO 2 The defogging fronts of the heater coating on the substrate and the control sample move similarly, but at significantly different speeds. Both experiments were performed at 1000Wm -2 、T amb The test was carried out under sunlight at ≈23°C and RH≈55%.
[0218] Fig. 14C The defogging time t under various sunlight conditions is summarized. d (i.e., the time required to reach f = 0.05), showing that the defogging performance of the coating is improved by 2 to 3 times compared to the control sample. Fig. 14C Depicts the defog time t d (ie the time required until the sample is less than 5% covered by fog). Scale bar B): 5 mm.
[0219] Supplementary Note 6: Outdoor testing of vision glasses coated with heating devices
[0220] The real-world feasibility of the heated device coated vision glasses was tested in various locations and under different conditions. Fig.15 , the left lens of the glasses contains a heating device coating, while the right lens is not coated.
[0221] Fig.15 A shows a clear autumn day (T amb ≈12℃、RH≈70%、I 0 =491Wm-2 ≈0.5sun) image of the first experiment on the building terrace. Fig.15 B shows a clear winter day (T amb ≈4℃、RH≈46%、I 0 =339Wm -2 ≈0.5sun), how the heated coated lenses outperformed the uncoated lenses and prevented fogging. Fig.15 C shows that the effect is also evident at different locations (T amb ≈4℃、RH≈80%、I 0 =212Wm -2 ≈0.5sun).
[0222] See also Fig.16 The photothermal performance of the vision glasses was further evaluated by outdoor experiments. To this end, the temperature of both lenses was recorded for 1 hour on a clear autumn day using a T-type thermocouple (Omega HSRTC-TT-T-36-36) connected to a thermocouple recorder (Lutron TM-947SD). In addition, the global horizontal irradiance (I 0 )(Taken from MeteoSwiss, pyranometer from Kipp&Zonen, CM21).
[0223] Fig.16 A shows a photograph of the experimental setup, Fig.16 B shows the temperature evolution of an uncoated lens (control sample, dark grey) and a lens coated with a heating device (light grey). Also shown is the global solar irradiance I 0 The coating consistently increases the temperature of the lens compared to the uncoated lens. That is, Fig.16 B shows how the temperature of the lens coated with the heating device is always higher than that of the uncoated lens, and during the experiment I 0 ≈525Wm -2 (corresponding to 0.53 sun). Scale bar A): 2 cm.
[0224] Therefore, even under realistic outdoor conditions, the T of the heated coated lens s It is also always higher than the T of the uncoated lens. s .
[0225] Supplementary Note 7: Heating device coating on flexible and portable substrates
[0226] Ultra-thin (~10nm) heating devices were tested on flexible substrates (top transparent, A4, ). The substrate was divided into 7×7 cm squares and the coating was deposited on them. Next, the sample was further divided into 3.5×3.5 cm squares, and the transmittance T and reflectance R were measured at normal incidence using an ILN-925 integrating sphere (LIVA / ISNIR spectrometer, Jasco, V770), and the absorbance α=1-τ-R was calculated.
[0227] To do this, first, all properties of a flat, unbent sample are measured and the results are Fig.17 As shown in A. Fig.17 A plots the transmittance T and absorptance α of the coated substrate (top transparency) before (solid line) and after (dashed line) 300 bending cycles. The transmittance of the bent sample is also shown. Clearly, Fig.17 As shown in A, the optical properties of the foil with the heater coating are not affected by the bending effect. Due to its ultra-thin size and porous nature, much larger radii of curvature during bending do not cause mechanical damage to the coating. In addition, since the scale of the random arrangement of the photothermal material (a few hundred nanometers) is also much smaller than the radius of curvature of the bending, the optical properties of the coating are not affected. Therefore, the heater coating can be deposited on any portable, flexible / foldable material and can be retroactively applied to various transparent surfaces (e.g., windows, displays or glasses).
[0228] Next, determine T for the sample bent at 40°. Fig.17 B depicts Fig.17 Image of the bent sample (40°) presented in A. Finally, the sample was manually folded 300 times in sequence so that the two ends of the substrates were in contact with each other each time ( Fig.17 C), and then measure the optical properties again. That is, Fig.17 The photograph depicted in C shows the sample being fully bent during the bending cycle. The sample was manually folded 300 times and its optical properties were remeasured (see Fig.17 A).
[0229] The utility of the heating device as a movable defogging foil can be further demonstrated. A piece of overhead projector transparency coated with the heating device was attached to a fused quartz wafer. Next, the coated wafer was exposed to sunlight in the Swiss Alps (irradiance I 0 ≈100Wm -2 Up to 200Wm -2 ) for 2 minutes. Then, exhale several times onto the wafer. The warm breath acts like a stream of saturated steam at body temperature, impinging on the uncoated glass (at ambient temperature) and the overhead projector foil coated with the heating device (at a temperature significantly above ambient due to the photothermal effect). The visibility of the background is then recorded. Fig.17As shown in D, after 10 seconds, the coated foil regains its full visibility, while the wafer is still covered with fog. Therefore, the flexible substrate / foil can be mounted on any existing glass to prevent fog formation or accelerate defogging (I 0 ≈100Wm -2 Up to 200Wm -2 ). Scale bars B), C): 5 mm, D): 2 cm.
[0230] Fig.18 A shows a cross-sectional rendering of the coating and illustrates a photothermal element made of gold consisting of a percolation structure substantially at the percolation threshold and embedded in a substrate (SiO 2 ) on the TiO 2 between two dielectric components. Fig.18 B shows a scanning transmission electron microscopy image (top) and energy dispersive x-ray spectroscopy mapping (bottom) of the heating device. The actual Au thickness is ~6nm to 7nm (thickness parameter d Au =4.75nm). The photothermal material made of gold (dark gray) is enclosed in SiO 2 Two ~2nm to 3nm (thickness parameter d TiO2 =3nm) of TiO 2 Scale bar B): 10 nm. Actual Au thickness is ~6 nm to 7 nm (nominal thickness d Au =4.75nm). The percolation Au layer (dark gray) is enclosed in the SiO 2 Two ~2nm to 3nm (nominal d TiO2 =3nm) of TiO 2 Between layers. Scale bar B): 10 nm. Fig.18 C shows the angular dispersion relation of the absorptivity for radiation incident angles θ up to 30° to the normal to the heating device, indicating that the absorptivity remains constant under oblique illumination.
[0231] Fig.19 A and Fig.19 B shows a graph depicting the broadband absorbance in the near infrared spectrum of a heating device comprising a photothermal element in the form of gold. Fig.19 A, broadband absorbance in the near-infrared spectrum at the percolation threshold (thickness parameter d Au =4.75 nm), making the heating device robust against slight manufacturing errors. Fig.19 B depicts the absorption spectrum of a heating device comprising a photothermal element in the form of gold, which has a (TiO 2 ), a top dielectric made of (TiO 2) made of a top dielectric, a displacement element on top. As described above, the heating device comprises a top dielectric (TiO 2 ) and the upper dielectric displacement element (TiO 2 ) exhibits a larger α, and the shifting element shifts the minimum wavelength of the range of interest toward a lower wavelength.
[0232] FIG20A shows a bright field SEM image of a heating device comprising a photothermal structure at the percolation threshold embedded between two dielectric elements. The photothermal material is Au (black) and is uniformly surrounded by the dielectric elements (TiO 2 layer, dark gray). SiO 2 The substrate is at the bottom, while the top is covered with carbon to facilitate imaging (both in light grey). Figure 20B shows a high-resolution transmission electron micrograph. The actual thickness of the photothermal element in the form of an Au layer (thickness parameter d Au =4.75nm) is estimated to be ~6nm to 7nm for TiO 2 2nm to 3nm (thickness parameter d TiO2 =3nm). The overall roughness of the structure is kept within a few nanometers, and the photothermal element (Au layer) is completely embedded in the dielectric element (TiO 2 )between.
[0233] Fig.21 The angular dependence of the optical properties of the above heating device is plotted. The incident radiation is measured at an angle of 100 nm to 2000 nm. The measured transmittance and reflectance are shown in the top and middle graphs, respectively. From these the absorbance is derived and presented in the bottom graph. The heating device is much thinner than the corresponding incident wavelength and exhibits little angular dispersion in both its transmittance and reflectance. Therefore, the wavelength between 800 nm and 2000 nm is From 0 to 30°, the absorption rate is almost constant.
[0234] Fig. 22 shows the visible transparency τ according to the material VIS and the solar absorption α of each layer thickness d (in nm) solar Comparison of the heating device according to the present invention with the prior art photothermal anti-fog coating; for α solar, values are taken based on textual values provided in the source, or if not directly available, by direct extraction from the plots and subsequent numerical integration and convolution with the Solar AM 1.5 Global (ASTM G173) reference spectrum. In the case of missing absorption or transparency data, reflectance is assumed to be zero, thus favoring the state of the art. For thickness, values are taken from the text whenever possible. In cases where the overall thickness is not reported, it is either estimated from the cross-sectional SEM images provided or estimated in conjunction with the paper implications.
[0235] Fig.23 The results of photothermal treatment under low solar irradiance levels are shown. 0 The box plots (n=5) of the steady-state temperature rise at the following levels (including 0.2sun and 0.4sun) show that the heating device according to the present invention can 0 The box plot contains the median, upper and lower quartiles, and whiskers (1.5 times the interquartile range). s The temperature rise of both the heating device and the control sample was measured below (see above for details). Fig.23 It is demonstrated that even at these low solar irradiance levels, the heating device is far superior to the control sample. At 0.2 sun, the control sample shows an average temperature rise of 0.36°C, while the coating achieves a temperature rise of 2.2°C. At 0.4 sun, the control sample temperature rises by 0.41°C, while the heating device reaches a steady-state temperature Ts of 3.7°C above the ambient temperature.
[0236] Figures 24A and 24B show outdoor testing of the heating device using a pair of prescription glasses. The photothermal performance test was conducted on a cloudy day, demonstrating that the heating device can operate effectively even in cloudy and windy conditions. The temperatures of both the uncoated lens (control sample, gray) and the lens coated with the heating device according to the present invention were recorded. The solar irradiance I is also shown. 0 The temperatures of both mirrors were recorded using a T-type thermocouple (Omega HSRTC-TT-T-36-36) connected to a thermocouple recorder (Lutron TM-947SD). In addition, the global horizontal irradiance (I 0 )(taken from MeteoSwiss, pyranometer from Kipp & Zonen, CM21). Figures 25A and 25B show indoor tests of a heating device according to the invention arranged on a pair of prescription glasses arranged behind a triple-glazed window. The temperatures of both uncoated lenses (control sample, grey) and lenses coated with the heating device according to the invention were recorded. Also shown is the solar irradiance I 0Although window glass greatly reduces transmitted solar energy, even at low levels of I 0 The heating device according to the present invention is still better than the control sample. The thermal power sensor (Thorlabs S425C and PM 100 USB controller) was used to record I 0 .
[0237] Fig.26 The performance of the heating device according to the present invention arranged on various polymer substrates is shown. 2 In addition to deposition on polystyrene (PS), polycarbonate (PC), and acrylic glass (PMMA), the heating device was also deposited on polystyrene (PS), polycarbonate (PC), and acrylic glass (PMMA). Prior to deposition, the substrates were exposed to oxygen plasma for 2 minutes (Oxford Instruments, Plasmalab80Plus). Since these substrates are inherently smooth, atomic force microscopy was used to determine the roughness of all surfaces. The root mean square (RMS) roughness of PC is 4.56nm, the root mean square roughness of PMMA is 10.83nm, and the root mean square roughness of PS is 17.78nm. Although these numbers represent the RMS roughness on a 20×20μm spot size, the RMS roughness values on a local area of the substrate (0.9×0.9μm) can be higher (i.e., the measured RMS roughness of PC is 17.20nm and the RMS roughness of PMMA is 52.80nm). Figure A) depicts the absorbance α of the bare polymer (grey) and the substrate coated with the heating device, confirming that the heating device comprises a photothermal material comprising a percolation structure at or substantially at the percolation threshold. Figure B) depicts the fabricated heating device (without TiO 2 An SEM micrograph of the top layer (top layer for ease of imaging) further confirms that the photothermal material includes a percolation structure that is at or substantially at the percolation threshold.
[0238] Fig. 27 A and Fig. 27 B shows the thermal durability and abrasion resistance test. In order to evaluate the effect of repeated and long-term heating on the optical characteristics of the heating device and thus on the photothermal performance, the heating device was repeatedly heated (~1 sun irradiance) and cooled 50 times. The heating devices used in all experiments were manufactured 6 months ago and were stored under ambient air throughout the period before the experiments. Fig. 27 A shows T at ~1 sun exposure and 50 cycles. s evolution, indicating no deterioration in performance. Fig. 27 B shows the absorbance α before (grey) and after (dark grey) 50 temperature cycles, showing no degradation.
[0239] Fig. 27 C and Fig. 27D shows a thermal durability test, where the heating device was exposed to ~1 sun irradiance for 63 hours and the absorptivity was measured before and after. C) During the first 5 hours of the 63 hour sunlight exposure test, T s Higher than T amb D) Absorption α before (grey) and after (dark grey) a 63 h sunlight exposure experiment.
[0240] Fig. 27 E and Fig. 27 F shows an abrasion test, where the transmittance T of the heated device was measured before and after E) peeling, F) rubbing test. In the peel test (adapted from ASTM D3330 standard / method A), a pressure-sensitive tape (3M TM VHB TM ) was firmly applied to the heating device and peeled off at an angle of 180° (i.e. parallel to the heating device). In the wiping test, the heating device (adapted from DIN 30643) was rubbed 50 times with a microfiber cloth under practical pressure. The heating device according to the invention thus retained its optical properties after both abrasion tests.
[0241] Fig. 27 G and Fig. 27 H shows the abrasion resistance test, in which the transmittance T of the heating device before and after the G) abrasion and H) dripping sand abrasion resistance test was measured. For the abrasion test (adapted from the standard test method ASTM F735-94), the heating device was placed in a small dish and covered with quartz sand (0.1 mm to 0.8 mm particle size). The dish was placed on a stirrer (heidolph Multi Reax) and shaken at a speed of 1000 rpm for 1 minute. The dripping sand test (adapted from ASTM F735-94) evaluates the resistance of the heating device to impact. Quartz sand (particle size 0.1 mm to 0.8 mm) was dropped onto the coating through a tube (5 cm inner diameter) through a grid (~1.5 mm grid width). The drop height was 35 cm to 40 cm. Therefore, the heating device according to the invention maintained its optical properties after both abrasion tests.
[0242] References
[0243] 1. Yoon, J. et al. Wet-Style Superhydrophobic Antifogging Coatings for Optical Sensors. Advanced Materials (Deerfield Beach, FL) 32, e2002710; 10.1002 / adma.202002710 (2020).
[0244] 2. Howarter, JA and Youngblood, JPSelf-Cleaning and Next Generation Anti-Fog Surfaces and Coatings. Macromol. Rapid Commun. 29, 455-466; 10.1002 / marc.200700733 (2008).
[0245] 3. Duran, I.R. and Laroche, G. Current trends, challenges, and perspectives of anti-fogging technology: surface and material design, fabrication strategies, and beyond. Progress in Materials Science 99, 106-186; 10.1016 / j.pmatsci.2018.09.001 (2019).
[0246] 4. Leach, RN, Stevens, F., Langford, SC and Dickinson, JT. Dropwise condensation: experiments and simulations of nucleation and growth of water drops in a cooling system. Langmuir: ACS Surfaces & Colloids 22, 8864-8872; 10.1021 / la061901 (2006).
[0247] 5. Sun, X., Hong, R., Hou, H., Fan, Z., and Shao, J. Thickness dependence of structure and optical properties of silver films deposited by magnetron sputtering. Thin Solid Films 515, 6962-6966; 10.1016 / j.tsf.2007.02.017 (2007).
[0248] 6. Lin, S. et al. Stretchable Anti-Fogging Tapes for Diverse Transparent Materials. Adv. Funct. Mater. 31, 2103551; 10.1002 / adfm.202103551 (2021).
[0249] 7. Cebeci, F.C., Wu, Z., Zhai, L., Cohen, R.E. and Rubner, M.F. Nanoporosity-driven superhydrophilicity: a means to create multifunctional antifogging coating. Langmuir: ACS Journal of Surfaces and Colloids 22, 2856-2862; 10.1021 / la053182p (2006).
[0250] 8. Tzianou, M., Thomopoulos, G., Vourdas, N., Ellinas, K., and Gogolides, E. Tailoring Wetting Properties at Extremes States to Obtain Antifogging Functionality. Adv.Funct.Mater.31, 2006687; 10.1002 / adfm.202006687 (2021).
[0251] 9. Nuraje, N., Asmatulu, R., Cohen, R. E. and Rubner, M. Durable antifog films from layer-by-layer molecularly blended hydrophilic polysaccharides. Langmuir: ACS Surfaces & Colloids 27, 782-791; 10.1021 / la103754a (2011).
[0252] 10. Walker, C. et al. Transparent Metasurfaces Counteracting Fogging by Harnessing Sunlight. Nano Letters 19, 1595-1604; 10.1021 / acs.nanolett.8b04481 (2019).
[0253] 11. Howarter, JA and Youngblood, JPSelf-Cleaning and Next Generation Anti-Fog Surfaces and Coatings. Macromol. Rapid Commun. 29, 455-466; 10.1002 / marc.200700733 (2008).
[0254] 12. Mouterde, T. et al. Antifogging abilities of model nanotextures. Nature Materials 16, 658-663; 10.1038 / nmat4868 (2017).
[0255] 13. Chen, Y. et al. Transparent superhydrophobic / superhydrophilic coatings for selfcleaning and anti-fogging. Appl. Phys. Lett. 101, 33701; 10.1063 / 1.4737167 (2012).
[0256] 14. Liu, M., Wang, S., and Jiang, L. Nature-inspired superwettability systems. Nat Rev Mater 2; 10.1038 / natrevmats.2017.36 (2017).
[0257] 15. Verho, T. et al. Mechanically durable superhydrophobic surfaces. Advanced Materials (Deerfield Beach, FL) 23, 673–678; 10.1002 / adma.201003129 (2011).
[0258] 16. Faustini, M. et al. Hydrophobic, Antireflective, Self-Cleaning, and Antifogging Sol-Gel Coatings: An Example of Multifunctional Nanostructured Materials for Photovoltaic Cells. Chem. Mater. 22, 4406-4413; 10.1021 / cm100937e (2010).
[0259] 17. Mitridis, E., Lambley, H., Trbber, S., Schutzius, TM & Poulikakos, D. Transparent Photothermal Metasurfaces Amplifying Superhydrophobicity by Absorbing Sunlight. ACS Nanotechnology 14, 11712-11721; 10.1021 / acsnano.0c04365 (2020).
[0260] 18. Cassie, ABD and Baxter, S. Wettability of porous surfaces. Trans. Faraday Soc. 40, 546; 10.1039 / TF9444000546 (1944).
[0261] 19. Wenzel, RNRESISTANCE OF SOLID SURFACES TO WETTING BY WATER. Ind. Eng. Chem. 28, 988-994; 10.1021 / ie50320a024 (1936).
[0262] 20. Papadopoulos, P., Mammen, L., Deng, X., Vollmer, D., and Butt, H.-J. How superhydrophobicity breaks down. Proceedings of the National Academy of Sciences of the United States of America 110, 3254-3258; 10.1073 / pnas.1218673110 (2013).
[0263] 21. Xue, C.-H. et al. Fabrication of superhydrophobic photothermalconversion fabric via layer-by-layer assembly of carbon nanotubes. Cellulose 28, 5107-5121; 10.1007 / s10570-021-03857-z (2021).
[0264] 22. Liu, Y. et al. Robust Photothermal Coating Strategy for Efficient Ice Removal. ACS Applied Materials & Interfaces 12, 46981-46990; 10.1021 / acsami.0c13367 (2020).
[0265] 23. Mitridis, E. et al. Metasurfaces Leveraging Solar Energy for Icephobicity. ACS Nanotechnology 12, 7009-7017; 10.1021 / acsnano.8b02719 (2018).
[0266] 24. Li, W. et al. Transparent selective photothermal coatings for antifogging applications. Cell Reports Physical Science 2, 100435; 10.1016 / j.xcrp.2021.100435 (2021).
[0267] 25. Yin,
[0268] 26. Neo, WT, Cho, CM, Shi, Z., Chua, S.-J., and Xu, J. Modulating high-energyvisible light absorption to attain neutral-state black electrochromicpolymers. J. Mater. Chem. C 4, 28-32; 10.1039 / C5TC02883C (2016).
[0269] 27. Baran, D. and Toppare, L. Donor-acceptor type random copolymers for full visible light absorption. Chemical Communications (Cambridge, UK) 47, 3933-3935; 10.1039 / c0cc04934d (2011).
[0270] 28. Wu, D. and Chen, J. Broadening Bandwidths of Few-Layer Absorbers by Superimposing Two High-Loss Resonators. Nanoscale Research Letters 16, 26; 10.1186 / s11671-020-03471-1 (2021).
[0271] 29. Gao, H. et al. Plasmonic Broadband Perfect Absorber for Visible LightSolar Cells Application. Plasmascience 15, 573-580; 10.1007 / s11468-019-01087-5 (2020).
[0272] 30. Cao, T., Wei, C., Simpson, R. E., Zhang, L. and Cryan, M. J. Broadband polarization-independent perfect absorber using a phase-change metamaterial at visible frequencies. Scientific Reports 4, 3955; 10.1038 / srep03955 (2014).
[0273] 31. Kiani, F. et al. Ultra-Broadband and Omnidirectional Perfect Absorber Based on Copper Nanowire / Carbon Nanotube Hierarchical Structure. ACS Photonics 7, 366-374; 10.1021 / acsphotonics.9b01658 (2020).
[0274] 32. Wu, S. et al. Superhydrophobic photothermal icephobic surfaces based on candle soot. Proceedings of the National Academy of Sciences; 10.1073 / pnas.2001972117 (2020).
[0275] 33. Zhang, H. et al. Solar anti-icing surface with enhanced condensate self-removing at extreme environmental conditions. Proceedings of the National Academy of Sciences of the United States of America 118; 10.1073 / pnas.2100978118 (2021).
[0276] 34. Han, M., Kim, B., Lim, H., Jang, H. and Kim, E. Transparent Photothermal Heaters from a Soluble NIR-Absorbing Diimmonium Salt. Advanced Materials (Deerfield Beach, FL) 32, e1905096; 10.1002 / adma.201905096 (2020).
[0277] 35. Liu, N., Mesch, M., Weiss, T., Hentschel, M. and Giessen, H. Infrared perfectabsorber and its application as plasmonic sensor. Nano Letters 10, 2342-2348; 10.1021 / nl9041033 (2010).
[0278] 36. Fan, X., Ding, Y., Liu, Y., Liang, J., and Chen, Y. Plasmonic Ti3C2Tx MXene Enables Highly Efficient Photothermal Conversion for Healable and Transparent Wearable Device. ACS Nanotechnology 13, 8124–8134; 10.1021 / acsnano.9b03161 (2019).
[0279] 37. Gaspar, D. et al. Influence of the layer thickness in plasmonic gold nanoparticles produced by thermal evaporation. Scientific Reports 3, 1469; 10.1038 / srep01469 (2013).
[0280] 38. Ruffino, F., Torrisi, V., Marietta, G. and Grimaldi, MG Kinetic growth mechanisms of sputter-deposited Au films on mica: from nanoclusters to nanostructured microclusters. Appl. Phys. A 100, 7-13; 10.1007 / s00339-010-5797-7 (2010).
[0281] 39. Lassesson, A., Brown, SA, van Lith, J. and Schulze, M. Electrical characterization of gold island films: A route to control of nanoparticledeposition. Appl. Phys. Lett. 93, 203111; 10.1063 / 1.3027463 (2008).
[0282] 40. Jeffers, G., Dubson, MA and Duxbury, PMI. Island-to-percolation transition during growth of metal films. Journal of Applied Physics 75, 5016-5020; 10.1063 / 1.355742 (1994).
[0283] 41. Fletcher, NH. The Chemical Physics of Ice (Cambridge University Press, 2010).
[0284] 42. Fletcher, NH The Physics of Rainclouds (Cambridge University Press, 1962).
[0285] 43. Na, B. and Webb, R. L. A fundamental understanding of factors affecting frost nucleation. International Journal of Heat and Mass Transfer 46, 3797-3808; 10.1016 / S0017-9310(03)00194-7 (2003).
[0286] 44. Attinger, D. et al. Surface engineering for phase change heat transfer: A review. MRS Energy & Sustainability 1;10.1557 / mre.2014.9 (2014).
[0287] 45. Qi, H. et al. Bioinspired Multifunctional Protein Coating for Antifogging, Self-Cleaning, and Antimicrobial Properties. ACS Applied Materials & Interfaces 11, 24504-24511; 10.1021 / acsami.9b03522 (2019).
[0288] 46. Zhao, J., Meyer, A., Ma, L., Wang,
[0289] 47. Ezzat, M. and Huang, C.-J. Zwitterionic polymer brush coatings with excellent anti-fog and anti-frost properties. RSC Adv. 6, 61695-61702; 10.1039 / C6RA12399F (2016).
[0290] 48. Zhou, L. et al. Self-assembly of highly efficient, broadband plasmonica absorbers for solar steam generation. Science Advances 2, e1501227; 10.1126 / sciadv.1501227 (2016).
[0291] 49. Wen, F. et al. Charge Transfer Plasmons: Optical Frequency Conductances and Tunable Infrared Resonances. ACS Nanotechnology 9, 6428-6435; 10.1021 / acsnano.5b02087 (2015).
[0292] 50. Sobhani, A. et al. Narrowband photodetection in the near-infrared with a plasmon-induced hot electron device. Nature Communications 4, 1643; 10.1038 / ncomms2642 (2013).
[0293] 51. Halas, N. Playing with Plasmons: Tuning the Optical ResonantProperties of Metallic Nanoshells. MRS Bull. 30, 362-367; 10.1557 / mrs2005.99 (2005).
[0294] 52. Saberi, A. A. Recent advances in percolation theory and its applications. Physics Reports 578, 1–32; 10.1016 / j.physrep.2015.03.003 (2015).
[0295] 53. Brouers, Clerc, Giraud, Laugier and Randriamantany. Dielectric and optical properties close to the percolation threshold. II. Physical Review B, Condensed Matter 47, 666-673; 10.1103 / PhysRevB.47.666 (1993).
[0296] 54. Bohren, CF and Huffman, D. R. Absorption and scattering of light by small particles (Wiley, Chichester, New York, 1993 (1998 [in print])).
[0297] 55. Kolwas, K. and Derkachova, A. Impact of the Interband Transitions in Gold and Silver on the Dynamics of Propagating and Localized Surface Plasmons. Nanomaterials (Basel, Switzerland) 10; 10.3390 / nano10071411 (2020).
[0298] 56. PB Johnson and RW Christy. Optical Constants of the Noble Metals.
[0299] 57. Moran, M. J. Fundamentals of engineering thermodynamics, 8th ed. (Wiley, Hoboken, NJ, 2014).
[0300] 58. Buck, ALNew Equations for Computing Vapor Pressure and Enhancement Factor.
[0301] Reference Mark List
[0302] 1 Heating device 7 Carrier element
[0303] 2 Photothermal element 8 top side
[0304] 3Electrical components
[0305] 4 Dielectric components
[0306] 5 Extension direction of displacement element E
[0307] 6 Anti-reflection element T in transverse direction.
Claims
1. A heating device (1) for preventing or removing deposition, the heating device (1) being particularly used for demisting, anti-fogging, deicing or anti-icing, the heating device (1) extending along an extension direction (E) and comprising: - at least one photothermal element (2) configured to exhibit a photothermal effect when irradiated with electromagnetic radiation, Characterized in that the photothermal element (2) comprises a photothermal material or consists of the photothermal material, the photothermal material comprises a seepage structure, and Therein, the percolation structure is at its percolation threshold or substantially at its percolation threshold.
2. The heating device (1) according to claim 1, wherein: The photothermal material is optically transparent, preferably optically transparent to electromagnetic radiation in the visible region of the electromagnetic spectrum, and / or Wherein the photothermal material is configured to absorb incident electromagnetic radiation, the photothermal material is preferably configured to absorb incident electromagnetic radiation in the near infrared region of the electromagnetic spectrum.
3. The heating device (1) according to any one of the preceding claims, wherein: The photothermal element is electrically conductive or electrically insulating, and / or The heating device (1) further comprises at least one electric element (3), wherein the at least one electric element (3) is configured to introduce electric current into the photothermal element (2), so that heat is generated by the photothermal element (2), and the electric element (3) is preferably an electrode.
4. The heating device (1) according to any one of the preceding claims, wherein: The photothermal element (2) has a thickness in the extension direction (E) in the range of 1 nm to 50 nm, preferably in the range of 1 nm to 10 nm, and / or The heating device (1) has a thickness in the extension direction (E) in the range of 1 nm to 100 nm, and / or Therein, the photothermal element (2) and / or the heating device (1) has a thickness with respect to the extension direction (E) which is much smaller than the wavelength of the incident electromagnetic radiation in the visible and near infrared.
5. The heating device (1) according to any one of the preceding claims, wherein: The heating device is bendable, and / or Wherein, the heating device (1) comprises an inverse curvature greater than 1 micron when bent.
6. The heating device (1) according to any one of the preceding claims, wherein: The photothermal element (2) is a layer, which preferably extends along a transverse direction (T) extending perpendicularly to the extension direction (E).
7. The heating device (1) according to any one of the preceding claims, wherein: The photothermal material is electrically conductive and / or comprises or consists of at least one metal, and / or is a metal or a metal alloy, the at least one metal being, for example, gold, silver, aluminum, copper, platinum or tungsten, or Wherein, the photothermal element is a semiconductor.
8. The heating device (1) according to any one of the preceding claims, further comprising at least one dielectric element (4), wherein: The dielectric element (4) is arranged before or after the photothermal element (2) with respect to the extension direction (E), and The dielectric element (4) and the photothermal element (2) are preferably at least partially in surface contact with each other, and / or Therein, the dielectric element (4) is preferably optically transparent and / or preferably comprises or consists of at least one metal oxide or metal nitride, such as titanium dioxide, silicon dioxide, tantalum pentoxide, titanium nitride.
9. The heating device (1) according to any one of the preceding claims, further comprising at least one displacement element (5), wherein: The displacement element (5) is configured to shift the absorption capacity and / or transmission capacity of the heating device (1) for the incident electromagnetic radiation towards shorter or longer wavelengths of the incident electromagnetic radiation, and / or It also comprises at least one anti-reflection element (6), which is configured and arranged to reflect electromagnetic radiation towards the photothermal element (2).
10. The heating device (1) according to claim 9, wherein: The displacement element (5) and / or the anti-reflection element (6) are arranged before or after the photothermal element (2) with respect to the extension direction (E), and / or The displacement element (5) and / or the anti-reflection element (6) are at least one of transparent and dielectric, and the displacement element (5) preferably includes a dielectric element (4). Or it consists of a dielectric element (4), which is preferably a dielectric element (4) according to claim 8.
11. The heating device (1) according to any one of the preceding claims, further comprising at least one carrier element (7), in, The photothermal element (2) is arranged on the carrier element (7) or is at least partially embedded in the carrier element (7), and Wherein, the carrier element (7) is preferably at least one of bendable, flexible, deformable, foldable, optically transparent, and / or includes a solid, and / or one or more plastics and / or one or more polymers or is composed of a solid, and / or one or more plastics and / or one or more polymers, the solid is preferably an amorphous solid such as glass, and the one or more plastics and / or one or more polymers are preferably transparent and / or elastic plastics or polymers.
12. A method for producing a heating device (1) for preventing or removing deposits, in particular for demisting, anti-fogging, deicing or anti-icing, the heating device (1) extending along an extension direction (E) and preferably corresponding to a heating device (1) as claimed in any one of the preceding claims, wherein The method comprises the following steps: - providing at least one photothermal element (2), the at least one photothermal element (2) being configured to exhibit a photothermal effect when irradiated with electromagnetic radiation, Characterized in that the photothermal element (2) comprises a photothermal material or is composed of a photothermal material, the photothermal material comprises a seepage structure, and Therein, the percolation structure is at its percolation threshold or substantially at its percolation threshold.
13. The method according to claim 12, wherein: The photothermal element (2) is produced by deposition, preferably by thin film deposition and / or vapor deposition, and / or by chemical growth, and the photothermal element (2) is particularly preferably produced by island growth.
14. The method according to claim 12 or 13, wherein: The photothermal element (2) is produced by deposition at a deposition rate in the range of 0.05 nanometers per second to 1 nanometer per second and / or during a deposition time in the range of 1 second to 150 seconds.
15. The method according to any one of claims 12 to 14, wherein: The photothermal element (2) is produced directly on the dielectric element (4), the displacement element (5) or the carrier element (7), and / or Therein, the photothermal element (2) is produced by direct deposition of preferably at least one electrically conductive material.