High-boron-removal polyamide reverse osmosis membrane as well as preparation method and application thereof

By performing interfacial polymerization reaction and post-treatment on the polysulfone base film, combined with the mesoporous material constructed by three-dimensional cubic phase pores, the problem of insufficient desalination and deboronization rates of existing reverse osmosis membranes under high throughput is solved, and the problem of insufficient desalination and deboration rates of existing reverse osmosis membranes is achieved. The efficient seawater desalination effect reduces operation and maintenance costs.

CN119034514APending Publication Date: 2024-11-29WANHUA CHEM GRP CO LTD

Patent Information

Application Number
CN202411457376.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

While ensuring high throughput, it is difficult to increase the desalination rate and deboronization rate at the same time, resulting in an intensification of energy and environmental crises during seawater desalination. It is urgent to develop low-energy consumption, high-throughput, high-desalination and high-boronization. membrane.

Method used

Interface polymerization reaction is carried out by dipping and spraying the polysulfone-based film on the polysulfone-based film, combining the mesoporous material constructed by three-dimensional cubic phase pores to strengthen the polyamide separation layer, improve the deboronization performance of the film, and perform post-treatment and moisturizing treatment to enhance the overall performance of the film.

Benefits of technology

It significantly improves the deboronization rate and desalination rate of the reverse osmosis membrane, while enhancing the water flux, greatly improving the comprehensive performance of the membrane, suitable for seawater desalination and reducing operation and maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005090862410000081
    Figure BDA0005090862410000081
  • Figure BDA0005090862410000091
    Figure BDA0005090862410000091
Patent Text Reader

Abstract

The invention discloses a high-boron-removal polyamide reverse osmosis membrane as well as a preparation method and application thereof. The preparation method comprises the following steps: 1) contacting a polysulfone-based membrane with a diamine aqueous phase solution in a dip-coating manner, and respectively removing water drops on the front and back surfaces after contact; (2) a multi-element acyl chloride oil phase solution is sprayed on the front face and the back face of the membrane at the same time, interfacial polymerization reaction is carried out, the multi-element acyl chloride oil phase solution sprayed on the back face of the membrane contains a mesoporous material of a three-dimensional cubic phase pore structure, and a polyamide membrane is prepared; and 3) immersing the polyamide membrane into a sodium hypochlorite water tank for post-treatment, and drying after moisturizing treatment to obtain the polyamide reverse osmosis membrane. By strengthening the polyamide separation layer, the reverse osmosis membrane is endowed with excellent boron removal performance, and meanwhile, the reverse osmosis membrane has high flux and high desalination performance through structural modification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polyamide reverse osmosis membrane with improved performance, in particular to a high-boron removal polyamide reverse osmosis membrane and a preparation method and application thereof. Background Art

[0002] With the rapid development of the world economy, the demand for fresh water resources is increasing. Even in some coastal areas, facing the vast ocean, it is difficult to solve the drinking water problem. Therefore, high-boron removal seawater desalination technology has received widespread attention and is expected to alleviate the water crisis.

[0003] The core of seawater desalination technology is high-boron removal seawater desalination membrane. Although the seawater desalination membrane preparation technology has made significant progress in the past two years, there are still many problems with the membrane itself. For example, while ensuring the ideal water production flux, the desalination rate and boron removal rate of the membrane have not been well improved. Therefore, facing the increasingly tense energy and environmental crisis, further development and application of low-energy consumption, high-flux, high-desalination and high-boron removal reverse osmosis membranes have become the most important research topic and development direction in the field of seawater desalination.

[0004] In order to improve the flux, desalination rate and deboronization rate of the reverse osmosis membrane, the currently disclosed patents mainly add different types of additives to the aqueous solution or the organic solution, and improve the performance by optimizing the interfacial polycondensation and improving the polyamide layer structure. For example, in patent CN114345149A, polyisobutyleneamine is dissolved in the organic solution to adjust the micro-nano structure of the membrane, adjust the pore size, fill the defects of the reverse osmosis membrane, and further enhance the deboronization performance of the reverse osmosis membrane.

[0005] Although the prior art has formed some technical solutions for improving the boron removal performance of reverse osmosis membranes, these technical solutions still need to be further improved in terms of pursuing higher boron removal performance while maintaining high flux and high desalination.

[0006] Therefore, there is an urgent need to develop a reverse osmosis membrane with high flux, high desalination and excellent boron removal performance in this field. Summary of the invention

[0007] In order to solve the above technical problems, the present invention proposes a high-boron removal polyamide reverse osmosis membrane and its preparation method and application. The present invention imparts excellent boron removal performance to the reverse osmosis membrane by strengthening the polyamide separation layer, and at the same time performs structural modification to enable it to have high flux and high desalination performance. The reverse osmosis membrane prepared by the present invention can be applied to seawater desalination, further improving the treatment effect and reducing operation and maintenance costs.

[0008] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a high-boron removal polyamide reverse osmosis membrane comprises the following steps:

[0010] 1) contacting the polysulfone-based membrane with a diamine aqueous solution by dip coating, and removing water droplets from the front and back surfaces respectively after contact;

[0011] 2) spraying a polyacyl chloride oil phase solution on the front and back of the membrane simultaneously to carry out an interfacial polymerization reaction, wherein the polyacyl chloride oil phase solution sprayed on the back of the membrane contains a mesoporous material with a three-dimensional cubic pore structure, thereby obtaining a polyamide membrane;

[0012] 3) The polyamide membrane is immersed in a sodium hypochlorite water tank for post-treatment, and then dried after moisturizing to obtain a polyamide reverse osmosis membrane.

[0013] The polysulfone-based membrane described in the present invention is a polysulfone support membrane formed on a non-woven fabric. The finished product can be directly purchased through commercial channels, or it can be prepared by dissolving a polysulfone resin to prepare a casting solution, then filtering and degassing, coating on a non-woven fabric, and forming a membrane by phase transformation in an aqueous phase. The general method or any known method is prepared, which is a known technology to those skilled in the art.

[0014] In some preferred examples of the present invention, in the diamine aqueous solution, the mass concentration of diamine is 2.5-7.5wt%;

[0015] Preferably, the diamine is selected from one or more of m-phenylenediamine, p-phenylenediamine and piperazine.

[0016] In some preferred examples of the present invention, the mass concentration of the polyacyl chloride in the polyacyl chloride oil phase solution sprayed on the front and back sides of the film is 0.1-0.3%wt% respectively;

[0017] Preferably, the polyacyl chloride is selected from one or more of trimesoyl chloride and isophthaloyl chloride.

[0018] In some preferred examples of the present invention, the mass concentration of the mesoporous material in the polyacyl chloride oil phase solution sprayed on the back of the membrane is 0.002-0.02wt%;

[0019] Preferably, the mesoporous material is MCM-48 with a three-dimensional cubic pore structure and a particle size range of 50-200 nm.

[0020] Preferably, the mesoporous material can be evenly distributed in the polyacyl chloride oil phase solution sprayed on the back of the membrane, for example, by ultrasonic dispersion.

[0021] In some preferred examples of the present invention, the reaction time of the interfacial polymerization reaction is 2-60 s, preferably 10-30 s.

[0022] In some preferred examples of the present invention, the mass concentration of the sodium hypochlorite solution in the sodium hypochlorite water tank is 50-500 ppm.

[0023] In some preferred examples of the present invention, the post-treatment time of the sodium hypochlorite water tank is 30-120s.

[0024] In some preferred examples of the present invention, the moisturizing treatment is to immerse the polyamide membrane in a moisturizing agent with a mass concentration of 2-20wt% for 10-120s;

[0025] Preferably, the moisturizing agent is an aqueous solution of glycerol and / or citric acid;

[0026] Preferably, the drying temperature is 40-90° C. and the drying time is 30-180 seconds.

[0027] The present invention also provides a high-boron removal polyamide reverse osmosis membrane prepared by the method described above.

[0028] The present invention also provides an application of the high-boron removal polyamide reverse osmosis membrane prepared by the method described above in the field of water treatment, especially in the field of seawater desalination treatment.

[0029] The high-boron removal polyamide reverse osmosis membrane provided by the method of the present invention can be applied to seawater desalination technology, particularly to seawater desalination water treatment components or devices. The water treatment component or device can be any component or device installed with the high-boron removal polyamide reverse osmosis membrane of the present invention that can be applied to the water treatment process. The "applied in a water treatment component or device" includes the application to the component or device product installed with the high-boron removal polyamide reverse osmosis membrane of the present invention, and also includes the application to the preparation of such component or device product. The component can be, for example, a spiral membrane component and a disc-type flat membrane component.

[0030] The present invention strengthens the polyamide separation layer by simultaneously performing interfacial polymerization on both sides of the polysulfone-based membrane, greatly improving the deboronization effect and desalination rate; wherein, the mesoporous material of the three-dimensional cubic phase pore structure itself has a water channel, and a capillary effect occurs when water molecules pass through the hydrophilic pores of the particles, which can further enhance the hydrophilicity of the membrane surface and improve the water flux of the reverse osmosis membrane. Therefore, the reverse osmosis membrane provided by the present invention not only has a higher deboronization performance and a higher desalination rate, but also has an efficiently improved water flux, greatly enhancing the comprehensive performance of the reverse osmosis membrane. DETAILED DESCRIPTION

[0031] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0032] Unless otherwise specified, the raw materials used in the following examples or comparative examples are all commercially available industrial grade conventional raw materials. The main raw material information is as follows:

[0033] Polysulfone base film: P3500 LCD MB7, SOLVAY

[0034] Metaphenylenediamine: purity 99.9%, Shanghai Annuo Aromatic Amine Chemicals Co., Ltd.

[0035] Trimesoyl chloride: purity > 97.5%, Qingdao Sanlibennuo New Materials Co., Ltd.

[0036] n-Heptane: purity 99%, Aladdin Reagent (Shanghai) Co., Ltd.

[0037] Three-dimensional mesoporous material MCM-48: purity 99%, Aladdin Reagent (Shanghai) Co., Ltd. Two-dimensional mesoporous material MCM-41: purity 99%, Aladdin Reagent (Shanghai) Co., Ltd. Sodium hypochlorite: purity ≥ 6%, Wanhua Chlor-Alkali Co., Ltd.

[0038] Glycerin: purity 99.5%, Shandong Luliya New Materials Co., Ltd.

[0039] Sodium chloride: purity 99.5%, Beijing Inokai Technology Co., Ltd.

[0040] Boric acid: analytical grade, Komiou Co., Ltd.

[0041] The performance testing methods involved in the following embodiments of the present invention are as follows:

[0042] The boron removal rate (Rb) is defined as: the difference between the boron concentration in the feed solution and the boron concentration in the permeate, divided by the boron concentration in the feed solution, under certain operating conditions;

[0043] The salt rejection rate (R) is defined as: under certain operating conditions, the difference between the salt concentration in the feed solution and the salt concentration in the permeate, divided by the salt concentration in the feed solution;

[0044] Permeation flux (F) is defined as the volume of water that passes through a unit membrane area per unit time under certain operating conditions, and its unit is L / (m 2 h).

[0045] The following Examples 1-4 and Comparative Examples 1-3 are used to prepare polyamide reverse osmosis membranes:

[0046] [Example 1]

[0047] First, the polysulfone-based membrane is contacted with a 3.5wt% m-phenylenediamine aqueous solution by dipping, and water droplets on the front and back surfaces are removed respectively after contact; a polyacyl chloride oil phase solution is sprayed on the front and back of the membrane at the same time for interfacial polymerization reaction, wherein the front is sprayed with a 0.14wt% trimesoyl chloride n-heptane solution, and the back of the membrane is sprayed with a 0.1wt% trimesoyl chloride n-heptane solution containing 0.005wt% of a three-dimensional mesoporous material MCM-48, and an interfacial polymerization reaction is carried out for 20s. The reverse osmosis membrane after the reaction is immersed in a water tank with a pH of 8 and containing 500ppm sodium hypochlorite for post-treatment for 1min, and then immersed in a 4wt% glycerol solution for moisturizing treatment for 30s, dried at 50°C for 2min, and rolled up to obtain a polyamide reverse osmosis membrane.

[0048] [Example 2]

[0049] First, the polysulfone-based membrane is contacted with a 2.5wt% m-phenylenediamine aqueous solution by dipping, and water droplets on the front and back surfaces are removed respectively after contact; a polyacyl chloride oil phase solution is sprayed on the front and back of the membrane at the same time for interfacial polymerization reaction, wherein the front is sprayed with a 0.2wt% trimesoyl chloride n-heptane solution, and the back of the membrane is sprayed with a 0.1wt% trimesoyl chloride n-heptane solution containing 0.02wt% of a three-dimensional mesoporous material MCM-48, and an interfacial polymerization reaction is carried out for 20s. The reverse osmosis membrane after the reaction is immersed in a water tank with a pH of 8 and containing 50ppm sodium hypochlorite for post-treatment for 1min, and then immersed in a 10wt% glycerol solution for moisturizing treatment for 60s, dried at 50°C for 2min, and rolled up to obtain a polyamide reverse osmosis membrane.

[0050] [Example 3]

[0051] First, the polysulfone-based membrane is contacted with a 7.5wt% m-phenylenediamine aqueous solution by dipping, and water droplets on the front and back surfaces are removed respectively after contact; a polyacyl chloride oil phase solution is sprayed on the front and back of the membrane at the same time for interfacial polymerization reaction, wherein the front is sprayed with a 0.3wt% trimesoyl chloride n-heptane solution, and the back of the membrane is sprayed with a 0.1wt% trimesoyl chloride n-heptane solution containing 0.002wt% of a three-dimensional mesoporous material MCM-48, and an interfacial polymerization reaction is carried out for 20s. The reverse osmosis membrane after the reaction is immersed in a water tank with a pH of 8 and containing 300ppm sodium hypochlorite for post-treatment for 1min, and then immersed in a 2wt% glycerol solution for moisturizing treatment for 40s, dried at 50°C for 2min, and rolled up to obtain a polyamide reverse osmosis membrane.

[0052] [Example 4]

[0053] First, the polysulfone-based membrane is contacted with a 5wt% aqueous solution of m-phenylenediamine by dipping, and water droplets on the front and back surfaces are removed respectively after contact; a polyacyl chloride oil phase solution is sprayed on the front and back of the membrane at the same time to perform an interfacial polymerization reaction, wherein the front is sprayed with a 0.1wt% n-heptane solution of trimesoyl chloride, and the back of the membrane is sprayed with a 0.2wt% n-heptane solution of trimesoyl chloride and the solution contains 0.01wt% of a three-dimensional mesoporous material MCM-48, and an interfacial polymerization reaction is performed for 20s. The reverse osmosis membrane after the reaction is immersed in a water tank with a pH of 8 and containing 500ppm sodium hypochlorite for post-treatment for 1min, and then immersed in a 6wt% glycerol solution for moisturizing treatment for 120s, dried at 50°C for 2min, and rolled up to obtain a polyamide reverse osmosis membrane.

[0054] [Comparative Example 1]

[0055] First, the polysulfone-based membrane was exposed to a 3.5wt% aqueous solution of m-phenylenediamine by dipping, and water droplets on the front and back surfaces were removed after contact; 0.14wt% trimesoyl chloride n-heptane solution was sprayed on the front of the membrane for interfacial polymerization reaction, and the reaction lasted for 20s. The reverse osmosis membrane after the reaction was immersed in a water tank with a pH of 8 and containing 500ppm sodium hypochlorite for post-treatment for 1min, and then immersed in a 4wt% glycerol solution for moisturizing treatment for 30s, dried at 50°C for 2min, and rolled up to obtain a polyamide reverse osmosis membrane.

[0056] [Comparative Example 2]

[0057] First, the polysulfone-based membrane is contacted with a 3.5wt% m-phenylenediamine aqueous solution by dipping, and water droplets on the front and back surfaces are removed respectively after contact; a polyacyl chloride oil phase solution is sprayed on the front and back of the membrane at the same time to perform an interfacial polymerization reaction, wherein the front is sprayed with a 0.14wt% trimesoyl chloride n-heptane solution, and the back of the membrane is sprayed with a 0.1wt% trimesoyl chloride n-heptane solution, and the interfacial polymerization reaction is performed for 20s. The reverse osmosis membrane after the reaction is immersed in a water tank with a pH of 8 and containing 500ppm sodium hypochlorite for post-treatment for 1min, and then immersed in a 4wt% glycerol solution for moisturizing treatment for 30s, dried at 50°C for 2min, and rolled up to obtain a polyamide reverse osmosis membrane.

[0058] [Comparative Example 3]

[0059] First, the polysulfone-based membrane is contacted with a 3.5wt% aqueous solution of m-phenylenediamine by dipping, and water droplets on the front and back surfaces are removed respectively after contact; a polyacyl chloride oil phase solution is sprayed on the front and back of the membrane at the same time for interfacial polymerization reaction, wherein the front is sprayed with a 0.14wt% n-heptane solution of trimesoyl chloride, and the back of the membrane is sprayed with a 0.1wt% n-heptane solution of trimesoyl chloride and the solution contains 0.005wt% of the two-dimensional mesoporous material MCM-41, and the interfacial polymerization reaction is carried out for 20s. The reverse osmosis membrane after the reaction is immersed in a water tank with a pH of 8 and containing 500ppm sodium hypochlorite for post-treatment for 1min, and then immersed in a 4wt% glycerol solution for moisturizing treatment for 30s, dried at 50°C for 2min, and rolled up to obtain a polyamide reverse osmosis membrane.

[0060] Reverse osmosis membrane performance test:

[0061] The inlet liquid was a 32000 ppm sodium chloride aqueous solution, the boron content was 5 ppm, the operating pressure was 5.52 MPa, the operating temperature was 25° C., and the pH of the aqueous solution was 8. The reverse osmosis membranes prepared in the examples and comparative examples were tested for salt rejection rate R, flux F, and boron removal rate Rb, and the results are recorded in Table 1.

[0062] Table 1. Performance test results

[0063]

[0064]

[0065] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high-boron removal polyamide reverse osmosis membrane, characterized in that: The following steps are involved: 1) contacting the polysulfone-based membrane with a diamine aqueous solution by dip coating, and removing water droplets from the front and back surfaces respectively after contact; 2) spraying a polyacyl chloride oil phase solution on the front and back of the membrane simultaneously to carry out an interfacial polymerization reaction, wherein the polyacyl chloride oil phase solution sprayed on the back of the membrane contains a mesoporous material with a three-dimensional cubic pore structure, thereby obtaining a polyamide membrane; 3) The polyamide membrane is immersed in a sodium hypochlorite water tank for post-treatment, and then dried after moisturizing to obtain a polyamide reverse osmosis membrane.

2. The method for preparing a high-boron removal polyamide reverse osmosis membrane according to claim 1, wherein: In the diamine aqueous solution, the mass concentration of diamine is 2.5-7.5wt%; Preferably, the diamine is selected from one or more of m-phenylenediamine, p-phenylenediamine and piperazine.

3. The method for preparing a high-boron removal polyamide reverse osmosis membrane according to claim 1 or 2, characterized in that: The mass concentration of the polyacyl chloride in the polyacyl chloride oil phase solution sprayed on the front and back of the film is 0.1-0.3%wt% respectively; Preferably, the polyacyl chloride is selected from one or both of trimesoyl chloride and isophthaloyl chloride.

4. The method for preparing a high-boron removal polyamide reverse osmosis membrane according to any one of claims 1 to 3, characterized in that: The mass concentration of the mesoporous material in the polyacyl chloride oil phase solution sprayed on the back of the membrane is 0.002-0.02wt%; Preferably, the mesoporous material is MCM-48 with a three-dimensional cubic pore structure and a particle size range of 50-200 nm.

5. The method for preparing a high-boron removal polyamide reverse osmosis membrane according to any one of claims 1 to 4, characterized in that: The reaction time of the interfacial polymerization reaction is 2-60 s, preferably 10-30 s.

6. The method for preparing a high-boron removal polyamide reverse osmosis membrane according to any one of claims 1 to 5, characterized in that: In the sodium hypochlorite water tank, the mass concentration of the sodium hypochlorite solution is 50-500ppm.

7. The method for preparing a high-boron removal polyamide reverse osmosis membrane according to any one of claims 1 to 6, characterized in that: The post-treatment time of the sodium hypochlorite water tank is 30-120s.

8. The method for preparing a high-boron removal polyamide reverse osmosis membrane according to any one of claims 1 to 7, characterized in that: The moisturizing treatment is to immerse the polyamide membrane in a moisturizing agent with a mass concentration of 2-20wt% for 10-120s; Preferably, the moisturizing agent is an aqueous solution of glycerol and / or citric acid; Preferably, the drying temperature is 40-90° C. and the drying time is 30-180 seconds.

9. A high-boron removal polyamide reverse osmosis membrane prepared by the method according to any one of claims 1 to 8.

10. Use of a high-boron removal polyamide reverse osmosis membrane prepared by the method according to any one of claims 1 to 8 in the field of water treatment, especially in the field of seawater desalination.

Citation Information

Patent Citations

  • High-boron-removal polyamide reverse osmosis membrane and preparation method thereof

    CN114345149A

  • Membrane, Water Treatment System, And Method Of Making

    CN104010717A

  • Mesoporous silica sphere / semi-aromatic polyamide nano-composite reverse osmosis membrane and preparation method thereof

    CN104841295A

  • High-flux and anti-pollution reverse osmosis membrane as well as preparation method and application thereof

    CN116036878A

  • Silylated mesoporous silica membranes on polymeric hollow fiber supports

    US20150114906A1

Cited By

  • High-boron-removal polyamide reverse osmosis membrane and preparation method thereof

    CN120115008A

  • Polyamide composite membrane and preparation method thereof

    CN121288588A