Supported nano zero-valent iron as well as preparation method and application thereof
The preparation method of sodium alginate/biochar combined with loaded nano zero-valent iron was formed, which solved the problem of poor dispersion and stability of nano zero-valent iron in water, achieved efficient removal of tetracycline pollution, and had good Recycling potential.
Patent Information
- Application Number
- CN202411389186.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN119034689A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials, and in particular to a sodium alginate / biochar jointly loaded nano zero-valent iron and a preparation method and application thereof. Background Art
[0002] China is the world's largest producer and exporter of aquatic products. In 2022, the total output of aquatic products in the country reached 68.6591 million tons, of which 81.9% of aquatic products came from artificial breeding. Antibiotics have the effects of preventing and treating diseases of aquatic fish and other products, promoting growth, etc., and therefore are widely used in aquaculture. However, the metabolic rate of antibiotics in aquatic animals is very low, of which about 80% of antibiotics cannot be metabolized and enter the water body, causing antibiotic pollution. At the same time, most aquaculture farms in my country lack efficient sewage treatment facilities, and only 20% are treated by simple oxidation ponds or sedimentation tanks. Most aquaculture wastewater enters the environment directly without effective treatment, and the antibiotic residues in the wastewater migrate into the water and soil environment, causing pollution to the water and soil.
[0003] In aquaculture, tetracycline (TC) is currently the most widely used antibiotic due to its broad antimicrobial spectrum, high efficiency, low cost, and multiple advantages in promoting the growth of farmed fish, preventing or treating fish diseases. Studies have found that only 20-30% of tetracycline can be absorbed and utilized by aquatic products, and the remaining tetracycline remains in the aquaculture water or accumulates in the bottom mud. The concentration of tetracycline in the environment ranges from ng / L to μg / L. Tetracycline is difficult to biodegrade in the aquatic environment and has a long half-life. This results in its low environmental content, but due to its long-term accumulation in the environment, and through biological enrichment and concentration in the food chain, until it is transmitted and amplified, it will eventually cause harm to human health.
[0004] The treatment methods for tetracycline pollution at home and abroad mainly include physical and chemical treatment and biochemical treatment. Biochemical treatment has high requirements on environmental factors such as pH value, pollutant concentration, ion type and content, temperature, etc., and has disadvantages such as long treatment time and low removal efficiency. Physical and chemical treatment mainly includes coagulation and sedimentation, adsorption, advanced oxidation, reverse osmosis and micro-electrolysis. Among them, the adsorption method is widely used in actual wastewater treatment due to its simple process, wide source of adsorbents, low price, and recyclable materials.
[0005] Nano zero-valent iron (nZVI), as an emerging environmental material, has a high specific surface area and reactivity and is widely used in environmental remediation. However, exposed nZVI particles are easily oxidized or even self-ignited, and are easy to agglomerate in water, resulting in poor dispersibility and stability, and poor practical application effects. Currently, the commonly used carriers for fixing nZVI can be divided into inorganic (activated carbon, montmorillonite, biochar, etc.) and organic (chitosan, sodium alginate, etc.) materials, which effectively improve the stability of nano zero-valent iron. The void structure of the inorganic material itself can effectively overcome the shortcomings of nZVI when used alone and improve the ability to remove pollutants, but it is difficult to separate from water, and the material has a low reuse rate. When forming a gel, organic materials can embed nZVI in the internal structure, thereby avoiding Fe 0 However, the pore size and mechanical strength of the embedded spheres need to be improved. Therefore, it is of great significance to modify nano-zero-valent iron to make it have a high-efficiency adsorption effect on tetracycline. Summary of the invention
[0006] The purpose of the present invention is to provide a sodium alginate / biochar combined loaded nano zero-valent iron for efficiently removing tetracycline and a preparation method thereof, so as to overcome the shortcomings of the existing prepared nano zero-valent iron carriers and improve the treatment effect of pollutants.
[0007] In order to achieve the above object, the present invention provides a method for preparing sodium alginate / biochar-coated nano-zero-valent iron, comprising the following steps:
[0008] (1) dissolving sodium alginate in deionized water, heating to dissolve and expelling bubbles in the sol to obtain a sodium alginate solution with a mass concentration of 2%;
[0009] (2) mixing the nano-zero-valent iron, biochar and the sodium alginate solution obtained in step (1), and stirring them evenly to obtain a sodium alginate / biochar-supported nano-zero-valent iron blend SA / BC-nZVI;
[0010] (3) preparing a CaCl2 aqueous solution with a mass concentration of 4.0%, adding the obtained blend SA / BC-nZVI to the CaCl2 aqueous solution for cross-linking reaction to obtain spherical SA / BC-nZVI;
[0011] (4) The obtained spherical SA / BC-nZVI is washed and freeze-dried to obtain finished SA / BC-nZVI pellets.
[0012] Preferably, the mass concentrations of nano zero-valent iron and biochar in the sodium alginate solution in the above preparation method are 1% respectively.
[0013] Preferably, the adding in step (3) of the above preparation method is dropwise adding.
[0014] Preferably, the cleaning in the above preparation method is ultrapure water cleaning, and the cleaning is performed at least 5 times.
[0015] The present invention also provides a supported nanometer zero-valent iron prepared by the above-mentioned preparation method. The supported nanometer zero-valent iron can be applied to wastewater pollution treatment, including tetracycline pollution treatment, and can be particularly used for the treatment of wastewater contaminated by tetracycline in aquaculture.
[0016] The present invention has the following advantages:
[0017] The invention discloses a method for preparing modified nano zero-valent iron. Meanwhile, the prepared SA / BC-nZVI beads can solve the technical problem of low reaction activity of embedded beads in the prior art and the operation is simple.
[0018] The sodium alginate / biochar combined with loaded nano zero-valent iron beads prepared by the present invention can repair tetracycline-contaminated water bodies, with a removal rate of more than 90%, and has the characteristics of good effluent quality, no secondary pollution, simple separation, etc. The treatment system and the treated water body can be completely separated by a simple fishing or grid device, and the separated beads can be recycled, which is conducive to improving the utilization rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The figure shows the physical state comparison of the SA / BC-nZVI beads prepared in Example 1 of the present invention before and after freeze-drying.
[0020] Figure 2 The TC removal rate results of SA / BC-nZVI beads obtained in different embodiments of the present invention at different reaction times.
[0021] Figure 3 The TC removal rate results of different SA / BC-nZVI ball dosages in the present invention.
[0022] Figure 4 This is the TC removal efficiency result of the SA / BC-nZVI beads obtained in the present invention after regeneration. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Note: The experimental methods in the following examples are conventional methods unless otherwise specified, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples are all commercially available unless otherwise specified.
[0025] Example 1
[0026] This embodiment provides a method for preparing sodium alginate / biochar-coated nano-zero-valent iron, and the specific steps are as follows:
[0027] (2) dissolving 2 g of sodium alginate (SA) in 100 mL of oxygen-free deionized water, heating to dissolve at 55° C., and standing for 60 min to expel bubbles in the sol to obtain a sodium alginate solution with a mass concentration of 2%;
[0028] (3) mixing 1 g of nano zero-valent iron (nZVI) and 1 g of biochar (BC) with the obtained sodium alginate solution and stirring them evenly to obtain a sodium alginate / biochar-loaded nano zero-valent iron blend SA / BC-nZVI;
[0029] (4) Weigh 20 g of CaCl2 and dissolve it in 500 mL of ultrapure water to obtain a CaCl2 solution with a mass concentration of 4.0%. Take 100 mL of the obtained blend SA / BC-nZVI and add it dropwise into the prepared CaCl2 solution using a syringe to perform a cross-linking reaction. After reacting for 60 min, spherical sodium alginate / biochar-coated nano-zero-valent iron (SA / BC-nZVI beads) are obtained. The physical state of the SA / BC-nZVI beads before freeze-drying is as follows: Figure 1 As shown in a;
[0030] (5) The spherical sodium alginate / biochar-co-loaded nano-zero-valent iron obtained in step (3) was washed with ultrapure water for 5 times, and placed in a vacuum freeze drying oven for 24 hours to obtain a sodium alginate / biochar-co-loaded nano-zero-valent iron finished product, wherein the physical state of the freeze-dried SA / BC-nZVI beads is as follows: Figure 1 As shown in b.
[0031] Example 2
[0032] This embodiment provides a method for preparing sodium alginate / biochar jointly loaded nano zero-valent iron, which is different from Example 1 only in that the ratio of nano zero-valent iron to biochar is set to 1g:0.5g, that is, the mass concentration of nano zero-valent iron in the reaction system is 1%, and the mass concentration of biochar is 0.5%, to obtain a SA / BC-nZVI pellet.
[0033] Example 3
[0034] This embodiment provides a method for preparing sodium alginate / biochar-co-loaded nano zero-valent iron, which is different from Example 1 only in that the ratio of nano zero-valent iron to biochar is set to 1g:2g to obtain a SA / BC-nZVI pellet.
[0035] Comparative Example 1
[0036] This comparative example provides a method for preparing sodium alginate-loaded nano zero-valent iron, which is different from Example 1 only in that no biochar loading is added, and the nano zero-valent iron is set to 1g, thereby obtaining a SA / nZVI pellet.
[0037] Experimental Example 1
[0038] This experimental example compares the removal rates of different products obtained in Examples 1 to 3 and Comparative Example 1, as follows:
[0039] The obtained SA / BC-nZVI beads and SA / nZVI beads were respectively put into 30mL of 30mg / L tetracycline (TC) solution, the pH was adjusted to 6, and the reaction was carried out on a constant temperature oscillator at a speed of 150r / min and a temperature of 25°C. Certain solutions were taken as samples every 1, 4, 8, 16, 24, 48, 72, and 96 hours, and after filtering through a 0.45μm filter membrane, the concentration of TC was determined by spectrophotometry, and the removal rate η was calculated. The calculation formula is shown in the following formula 1.
[0040]
[0041] Wherein, C0 (mg / L) and C (mg / L) in Formula 1 are the initial TC concentration and the concentration of the remaining TC in the solution at different reaction times, respectively.
[0042] The samples with different reaction times were measured, and the TC removal rates of SA / BC-nZVI beads at different reaction times were calculated. Figure 2 As shown, it can be seen that when nZVI:BC is 1:1, the obtained SA / BC-nZVI pellets have the best removal effect on TC.
[0043] Experimental Example 2
[0044] This experiment aims to determine the removal effect of different SA / BC-nZVI ball dosages on TC, as follows:
[0045] SA / BC-nZVI beads (nZVI:BC=1:1) were added into 30mL30mg / L TC solution at 0.5g / L, 1g / L, 2g / L, and 3g / L, respectively. The pH was adjusted to 6 and the reaction was carried out on a constant temperature oscillator at a speed of 150r / min and a temperature of 25℃. Samples were taken at regular intervals, filtered through a 0.45μm filter membrane, and the TC concentration was determined by spectrophotometry to calculate its removal rate.
[0046] The TC removal rates of different SA / BC-nZVI ball dosages were calculated as follows: Figure 3 As shown in the figure, when the dosage of SA / BC-nZVI beads is 2g / L, the removal rate of TC by SA / BC-nZVI beads can reach 97.58%. Dosages above 2g / L will not significantly increase the removal rate of TC. Therefore, from an economic point of view, the dosage of 2g / L is the best dosage in the TC removal process.
[0047] Experimental Example 3
[0048] This experimental example aims to determine the removal effect of the obtained material after regeneration: SA / BC-nZVI beads (nZVI: BC = 1:1) were added to 30mL 30mg / LTC solution at 2g / L, and reacted on a constant temperature oscillator with a speed of 150r / min and a temperature of 25°C. After the reaction reached the equilibrium time, samples were taken and filtered through a 0.45μm filter membrane. The concentration of TC was determined by spectrophotometry and its removal rate was calculated. The used SA / BC-nZVI beads were then washed three times with ultrapure water, freeze-dried and used in the regeneration experiment. The number of regenerations was set to 5 times, and the removal effect of the material after each regeneration was determined. The regeneration experiment results are as follows Figure 4 As shown, it can be seen that the composite material has a good recycling rate. After 5 regenerations, the removal rate of TC by the composite can still reach 80%.
[0049] In summary, the present invention provides a sodium alginate / biochar jointly loaded nano zero-valent iron and a preparation method thereof. The obtained product SA / BC-nZVI pellets have a high removal effect on tetracycline and have good recycling potential. They have a good repair effect on water contaminated by tetracycline and have application value in wastewater treatment, especially in the treatment of tetracycline-contaminated wastewater in aquaculture.
[0050] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.
Claims
1. A method for preparing sodium alginate / biochar-coated nano-zero-valent iron, characterized in that: The following steps are included: (1) dissolving sodium alginate in deionized water, heating to dissolve and expelling bubbles in the sol to obtain a sodium alginate solution with a mass concentration of 2%; (2) mixing the nano-zero-valent iron, biochar and the sodium alginate solution obtained in step (1), and stirring them evenly to obtain a sodium alginate / biochar-supported nano-zero-valent iron blend SA / BC-nZVI; (3) preparing a CaCl2 aqueous solution with a mass concentration of 4.0%, adding the obtained blend SA / BC-nZVI to the CaCl2 aqueous solution for cross-linking reaction to obtain spherical SA / BC-nZVI; (4) The obtained spherical SA / BC-nZVI is washed and freeze-dried to obtain finished SA / BC-nZVI pellets.
2. The preparation method according to claim 1, characterized in that: The mass concentrations of the nano zero-valent iron and the biochar in the sodium alginate solution are respectively 1%.
3. The preparation method according to claim 1, characterized in that: The adding in step (3) is performed dropwise.
4. The preparation method according to claim 1, characterized in that: The cleaning is performed with ultrapure water.
5. Supported nano zero-valent iron prepared by the preparation method according to any one of claims 1 to 5.
6. Use of the supported nano zero-valent iron as claimed in claim 6 in wastewater pollution treatment.
7. The use according to claim 7, characterized in that: The application described includes tetracycline contamination treatment.
Citation Information
Patent Citations
Preparation method of sodium alginate / inorganic mineral linked load type nanometer zero-valent iron
CN105921763A
Preparation method and application of blue-green algae modified biochar loaded nano zero-valent iron series material
CN113244883A
Activated carbon-zero-valent iron composite gel particle, preparation method thereof and application of activated carbon-zero-valent iron composite gel particle in removal of heavy metal ions
CN114405492A