Ruthenium and vanadium double-doped cerium-manganese catalyst for denitration and VOCs removal as well as preparation method and application of ruthenium and vanadium double-doped cerium-manganese catalyst
Through the ruthenium and vanadium double-doped cerium manganese catalyst, the synergistic effect of MOFs structure and oxides is used to solve the high cost and complex process problems of synergistic removal of VOCs and NOx in the prior art, and achieve efficient and stable low-temperature removal The results reduce operating costs and increase market prospects.
Patent Information
- Application Number
- CN202411386862.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Existing catalysts have high cost, cumbersome process and market limitations in synergistic removal of VOCs and NOx, and it is difficult to achieve low temperature stability and efficient removal effects.
The cerium-manganese catalyst with double-doped ruthenium and vanadium is prepared by co-precipitation method, and the cerium-manganese catalyst with MOFs structure is combined with the synergistic effects of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide to improve the redox capacity and stability of the catalyst. .
The coordinated removal of VOCs and NOx is achieved, which reduces operating costs, improves the low-temperature nitrogen removal effect and water resistance of the catalyst, extends the service life, and significantly improves the stability and market prospects of the catalyst.
Smart Images

Figure CN119034734A_ABST
Abstract
Description
Technical Field
[0001] The invention provides a ruthenium-vanadium dual-doped cerium-manganese catalyst for denitration and removal of VOCs, and a preparation method and application thereof, belonging to the field of environmentally friendly catalytic materials and air pollution control. Background Art
[0002] In recent years, while my country's economy and society have developed rapidly, environmental problems have become increasingly prominent. Volatile organic compounds (VOCs) and nitrogen oxides (NO x ) are two common air pollutants. Controlling and reducing their emissions has become one of the key processes in solving air pollution problems. VOCs is a general term for various organic compounds with a boiling point of 50-260°C at room temperature. VOCs emissions in the environment are second only to atmospheric particulate matter and are considered the second largest category of air pollutants. These compounds not only damage the ozone layer and intensify the greenhouse effect, but also cause secondary pollution. NO in the atmosphere x The sources of NO are mainly divided into natural sources and human-generated sources. Compared with natural processes, NO generated by human factors x It is the main source of air pollution, most of which comes from the emissions from the combustion of fossil fuels. x The two pollutants often exist at the same time, so the study of VOCs and NO x The comprehensive and coordinated control of the two pollutants is of great significance to improving environmental pollution problems.
[0003] Thermal catalytic technology is currently commonly used for synergistic removal of NO x and VOCs, both the selective catalytic reduction reaction (SCR) and catalytic oxidation (CO) require the catalyst to have high redox properties. Among the existing patents for catalytic removal of VOCs, patent CN202310938297 discloses a catalyst with copper oxide and vanadium pentoxide as active components. The catalyst adopts a three-step synthesis process of solvent hydrothermal-impregnation-carbonization. First, the ZSM5 molecular sieve is added to the N, N diethylbenzamide solution for hydrothermal reaction, followed by centrifugation and washing operations, and the obtained white solid is carbonized to obtain a hollow ZSM5 molecular sieve; ammonium metavanadate and copper nitrate solution are added to the hollow molecular sieve, and the catalyst is obtained after stirring, impregnation, and carbonization. Patent CN202310983347 provides a precious metal-embedded mesoporous CeO2 hollow sphere composite material and a preparation method thereof. The preparation method of the reaction solution is to add organic acid, alcohol organic solvent, cerium salt and precious metal salt into pure water solution, stir well, stand at about 200°C, wash, and dry the precipitate; the dried product is calcined at 200-300°C to finally obtain the catalyst. xA catalyst for the coordinated removal of VOCs and a preparation method thereof, wherein vanadium is doped into the lattice of a CeO2 matrix as an active component. The catalysts prepared in the above patents either use precious metals or have a complicated preparation process, and have great market limitations. Summary of the invention
[0004] The present invention is aimed at the current VOCs and NO x The current status and existing problems of synergistic removal process and catalyst research provide a ruthenium and vanadium dual-doped cerium-manganese catalyst for denitrification and VOCs removal, which can achieve VOCs oxidation while reducing NO x It has a synergistic removal effect, removing NO x and VOCs are catalytically decomposed into N2, CO2, H2O and other components. In addition, the catalyst of the present invention can truly achieve NO x The reduction and harmlessness of VOCs have important economic and social value.
[0005] A method for preparing a ruthenium- and vanadium-doped cerium-manganese catalyst for denitration and removal of VOCs, the preparation method of the catalyst is as follows:
[0006] (1) Preparation of Mn-MOF
[0007] A manganese salt and a high molecular polymer are dissolved in a solvent to form a solution A, a 1,3,5-benzoic acid solution is slowly added to the solution A and allowed to stand for 10 to 16 hours, a precipitate is collected and washed and dried, and the obtained sample is marked as Mn-MOF;
[0008] (2) Mn μ CeO x Catalyst preparation
[0009] The Mn-MOF powder is added to the cerium salt solution and mixed, and then centrifuged, washed, dried and calcined in sequence to obtain Mn μ CeO x catalyst, wherein μ represents the molar ratio of Mn / Ce;
[0010] (3) Ru, V dual doping
[0011] Mn μ CeO x The catalyst is added to the solvent and mixed to obtain a suspension, and then the vanadium salt and the ruthenium salt are added to the suspension and mixed again. After mixing, it is dried and calcined twice to obtain the final product RuV / Mn μ CeO x .
[0012] In the above preparation method: the high molecular polymer described in step (1) is polyvinyl pyrrolidone, and the mass ratio of manganese salt, high molecular polymer and 1,3,5-benzoic acid is 0.1-1:1-4:0.5-1.5.
[0013] In the above preparation method: in step (1), the drying is performed in a vacuum drying oven, the drying temperature is 70 to 90° C., and the drying time is 10 to 14 hours.
[0014] In the above preparation method: in step (2), the calcination temperature is 300-600° C. and the calcination time is 2-4 hours.
[0015] In the above preparation method: in step (3), the first drying temperature is 40-70° C., the calcination time is 2-4 hours, the calcination temperature is 250-400° C., and the calcination atmosphere is 5-15% H2 / Ar atmosphere.
[0016] In the above preparation method: in step (3), the second drying temperature is 40-70° C., the calcination time is 2-4 hours, the calcination temperature is 600-800° C., and the calcination atmosphere is 5-15% H2 / Ar atmosphere.
[0017] In the above preparation method: the manganese salt described in step (1) is Mn(OAc)2·4H2O, and the cerium salt is Ce(NO3)3·6H2O; the vanadium salt described in step (3) is NH4VO3, and the ruthenium salt is Rucl3·3H2O.
[0018] In the above preparation method: RuV / Mn μ CeO x The mass ratio of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide is 1-5:1-5:0.1-5:0.1-5.
[0019] In some preferred technical solutions: the mass ratio of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide is 1-5:1-3:0.1-1.5:0.1-1.
[0020] A ruthenium-vanadium dual-doped cerium-manganese catalyst for denitration and removal of VOCs is prepared by the above method.
[0021] In the technical solution of the present invention, the catalyst prepared by the above method is used as a catalyst to synergistically remove VOCs and NO x Application in this area.
[0022] Beneficial effects:
[0023] (1) Metal organic frameworks (MOFs) have potential application prospects in various fields due to their unique structure and function. The cerium manganese catalyst with a MOFs structure prepared by the coprecipitation method of the present invention has more active centers and excellent redox ability.
[0024] (2) Effect of Ce oxide content on MnCeO x The microscopic morphology, crystal structure, and adsorption and activation of o-DCB molecules have a wide range of effects. The modification of manganese (Mn) oxide can provide more oxygen vacancies and enhance the low-temperature denitrification effect of the catalyst. Ruthenium (Ru) composite oxide can remain stable under VOCs catalytic oxidation conditions containing water vapor, improve the water resistance of the catalyst, and thus extend the service life of the catalyst. Vanadium (V) oxide can improve the redox ability of the catalyst and the amount of surface active oxygen adsorption.
[0025] (3) Compared with single metal catalysts, the synergistic effect of mixed metals gives the catalyst excellent stability and oxidation performance, and has broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the removal rate of NO by the catalyst in Examples 1 to 3 and Comparative Examples 1 to 3.
[0027] Figure 2 It is the removal rate of o-dichlorobenzene by the catalyst in Examples 1 to 3 and Comparative Examples 1 to 3.
[0028] Specific embodiment
[0029] The present invention will be further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto:
[0030] Example 1
[0031] (1) Preparation of Mn-MOF catalyst
[0032] 0.48 g Mn(OAc)2·4H2O and 2 g polyvinylpyrrolidone (PVP) were dissolved in a mixture of 100 mL ethanol and deionized water (V 乙醇 :V 水 =2:1) to form solution A. 0.9 g of 1,3,5-benzoic acid was dissolved in 30 ml of a mixed solution of ethanol and deionized water (V 乙醇 :V 水 =2:1) to form solution B. Solution B was slowly dripped into solution A and allowed to stand for 12 hours. The white precipitate was then collected after washing with methanol three times, centrifuged and dried in a vacuum oven at 80°C for 12 hours. The obtained sample was labeled as Mn-MOF.
[0033] (2) Mn μ CeO x Catalyst preparation
[0034] First, 0.326 g of Ce(NO3)3·6H2O was dissolved in 15 ml of ethanol solution, and 1.28 g of Mn-MOF prepared in step (1) was dispersed in the solution and ultrasonicated for 30 min. Then, it was stirred at room temperature for 1 h, and finally washed with methanol 3 times and dried. Finally, the sample was calcined at 450 ° C for 3 h to obtain a cerium-manganese-based catalyst.
[0035] (3) Ru, V dual doping
[0036] First, the catalyst prepared in step (2) was added to 20 ml of deionized water and then ultrasonically treated for 30 min. 7.02 mg NH4VO3 and 26.1 mg RuCl3 were added to the suspension and ultrasonically treated for 30 min again. Then, the suspension was placed in a 50° C. water bath and kept stirring continuously until the solvent evaporated. The sample was dried overnight in a vacuum oven at 60° C., and then the sample was transferred to a tube furnace and reacted at 300° C. for 3 h in a 10% H2 / Ar atmosphere. After that, the prepared sample was repeatedly washed and centrifuged with deionized water to wash away residual ions, and then dried overnight in a vacuum oven at 60° C. The sample was then transferred to a tube furnace and reacted at 700° C. for 3 h in a 10% H2 / Ar atmosphere, and finally a ruthenium and vanadium dual-doped cerium-manganese-based catalyst (the mass ratio of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide was 3.12:1.56:0.16:0.35).
[0037] (4) Catalyst activity test
[0038] The prepared catalyst was weighed and loaded into a catalyst performance evaluation reaction device, and the weighed mass was 1.936g. The inner diameter of the quartz tube in the evaluation reaction device was 30mm, and simulated gas was introduced for activity evaluation. The simulated gas composition was: NO (400ppm), NH3 (400ppm), o-dichlorobenzene (40ppm), O2 (11%), N2 as carrier gas, the total gas flow rate was 1000mL / min, and the catalytic reaction test temperature range was 200-400℃. The test results showed that at 200℃, the NO removal efficiency after 15min was 85.7%, and the o-dichlorobenzene removal efficiency was 80.6%. After two hours of reaction, the catalyst weighed and gained 0.132g, and the weight gain ratio was 6.8%.
[0039] Example 2
[0040] (1) The preparation of Mn-MOF catalyst was the same as in Example 1.
[0041] (2) Mn μ CeO x Catalyst preparation
[0042] First, 0.0978 g of Ce(NO3)3·6H2O was dissolved in 15 ml of ethanol solution, and 1.28 g of Mn-MOF prepared in step (1) was dispersed in the solution and ultrasonicated for 30 min. Then, it was stirred at room temperature for 1 h, and finally washed with methanol 3 times and dried. Finally, the sample was calcined at 450 ° C for 3 h to obtain a cerium-manganese-based catalyst.
[0043] (3) Ru, V dual doping
[0044] First, the catalyst prepared in step (2) was added to 20 ml of deionized water and then ultrasonically treated for 30 min. 11.7 mg NH4VO3 and 15.6 mg RuCl3 were added to the suspension and ultrasonically treated for 30 min again. Then, the suspension was placed in a 50° C. water bath and kept stirring continuously until the solvent evaporated. The sample was dried overnight in a vacuum oven at 60° C. and then reduced at 300° C. in a 10% H2 / Ar atmosphere for 3 hours. Afterwards, the prepared sample was repeatedly washed and centrifuged with deionized water to wash away residual ions and then dried overnight in a vacuum oven at 60° C. Finally, the sample was reduced at 700° C. in a 10% H2 / Ar atmosphere for 3 hours to obtain a ruthenium and vanadium dual-doped cerium-manganese-based catalyst (the mass ratio of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide was 3.37:1.03:0.53:0.61).
[0045] (4) Catalyst activity test
[0046] The prepared catalyst was weighed and loaded into a catalyst performance evaluation reaction device, and the weighed mass was 1.072g. The inner diameter of the quartz tube in the evaluation reaction device was 30mm, and simulated gas was introduced for activity evaluation. The simulated gas composition was: NO (400ppm), NH3 (400ppm), o-dichlorobenzene (40ppm), O2 (11%), N2 as carrier gas, the total gas flow rate was 1000mL / min, and the catalytic reaction test temperature range was 200-400℃. The test results showed that at 200℃, the NO removal efficiency after 15min was 90.5%, and the o-dichlorobenzene removal efficiency was 83.5%. After two hours of reaction, the catalyst was weighed and gained 0.161g, and the weight gain ratio was 15.0%.
[0047] Example 3
[0048] (1) Preparation of Mn-MOF catalyst
[0049] 0.84 g Mn(OAc)2·4H2O and 2 g polyvinylpyrrolidone (PVP) were dissolved in a mixture of 100 mL ethanol and deionized water (V 乙醇 :V 水=2:1) to form solution A. 0.9 g of 1,3,5-benzoic acid was dissolved in 30 ml of a mixed solution of ethanol and deionized water (V 乙醇 :V 水 =2:1) to form solution B. Solution B was slowly dripped into solution A and allowed to stand for 12 hours. The white precipitate was then collected after washing with methanol three times, centrifuged and dried in a vacuum oven at 80°C for 12 hours. The obtained sample was labeled as Mn-MOF.
[0050] (2) Mn μ CeO x Catalyst preparation
[0051] First, 0.627 g of Ce(NO3)3·6H2O was dissolved in 15 ml of ethanol solution, and 1.62 g of Mn-MOF prepared in step (1) was dispersed in the solution and ultrasonicated for 30 min. Then, it was stirred at room temperature for 1 h, and finally washed with methanol 3 times and dried. Finally, the sample was calcined at 450 ° C for 3 h to obtain a cerium-manganese-based catalyst.
[0052] (3) Ru, V dual doping
[0053] First, the catalyst prepared in step (2) was added to 20 ml of deionized water and then ultrasonically treated for 30 min. 26.3 mg NH4VO3 and 47.8 mg RuCl3 were added to the suspension and ultrasonically treated for 30 min again. Then, the suspension was placed in a 50° C. water bath and kept stirring continuously until the solvent evaporated. The sample was dried overnight in a vacuum oven at 60° C. and then reduced at 300° C. for 3 hours under 10% H2 / Ar. Afterwards, the prepared sample was repeatedly washed and centrifuged with deionized water to wash away residual ions and then dried overnight in a vacuum oven at 60° C. Finally, the sample was reduced at 700° C. in a 10% H2 / Ar atmosphere for 3 hours to finally obtain a ruthenium and vanadium dual-doped cerium-manganese-based catalyst (the mass ratio of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide was 3.84:1.87:0.96:0.73).
[0054] (4) Catalyst activity test
[0055] The prepared catalyst was weighed and loaded into a catalyst performance evaluation reaction device, and the weighed mass was 2.113g. The inner diameter of the quartz tube in the evaluation reaction device was 30mm, and simulated gas was introduced for activity evaluation. The simulated gas composition was: NO (400ppm), NH3 (400ppm), o-dichlorobenzene (40ppm), O2 (11%), N2 as carrier gas, the total gas flow rate was 1000mL / min, and the catalytic reaction test temperature range was 200-400℃. The test results showed that at 200℃, the NO removal efficiency after 15min was 93.7%, and the o-dichlorobenzene removal efficiency was 87.2%. After two hours of reaction, the catalyst was weighed and gained 0.225g, and the weight gain ratio was 10.6%.
[0056] Comparative Example 1
[0057] (1) Preparation of Mn-MOF catalyst
[0058] The conditions are the same as step (1) in Example 1;
[0059] (2) Mn μ CeO x Catalyst preparation
[0060] The conditions are the same as step (2) in Example 1;
[0061] (3) Catalyst activity test
[0062] The test conditions were the same as step (4) in Example 1, and the catalyst weighed 2.472 g. The test results showed that within the temperature range of 200-400°C, the NO removal efficiency was as low as 60.2% and as high as 75.3%; the o-dichlorobenzene removal efficiency was as low as 52.6% and as high as 67.1%. After two hours of reaction, the catalyst gained 1.284 g, with a weight gain ratio of 51.94%.
[0063] (4) Contrast effect
[0064] Compared with Example 1, no ruthenium and vanadium dual doping was performed. The NO removal rate and o-dichlorobenzene removal efficiency of the sample decreased significantly, which may be due to the lack of ruthenium and vanadium dual doping, and the reduction of active sites led to a decrease in catalyst activity. At the same time, the hydrophobicity of the catalyst decreased, resulting in a significant weight gain after two hours of reaction.
[0065] Comparative Example 2
[0066] (1) Preparation of Mn-MOF catalyst
[0067] The conditions are the same as step (1) in Example 1;
[0068] (2) Mn μ CeO x Catalyst preparation
[0069] The conditions are the same as step (2) in Example 1;
[0070] (3) Ru doping
[0071] In step (3), NH4VO3 is not added, and other conditions are the same as step (3) in Example 1;
[0072] (4) Catalyst activity test
[0073] The test conditions were the same as step (4) in Example 1, and the catalyst weighed 1.812 g. The test results showed that within the temperature range of 200-400°C, the NO removal efficiency was as low as 63.3% and as high as 75.3%; the o-dichlorobenzene removal efficiency was as low as 59.6% and as high as 70.3%. After two hours of reaction, the catalyst gained 0.338 g, with a weight gain ratio of 18.4%.
[0074] (5) Contrast effect
[0075] Compared with Example 1, the prepared catalyst was only doped with Ru. The NO conversion rate of the sample reached more than 70%, and the removal efficiency of o-dichlorobenzene decreased significantly, which may be due to the lack of vanadium doping and the reduction of active sites, resulting in a decrease in the activity of the catalyst.
[0076] Comparative Example 3
[0077] (1) Preparation of Mn-MOF catalyst
[0078] The conditions are the same as step (1) in Example 3;
[0079] (2) Mn μ CeO x Catalyst preparation
[0080] The conditions are the same as step (2) in Example 3;
[0081] (3) V doping
[0082] In step (3), RuCl3 is not added, and other conditions are the same as step (3) in Example 3;
[0083] (4) Catalyst activity test
[0084] The test conditions were the same as step (4) in Example 3, and the catalyst weighed 2.483 g. The test results showed that within the temperature range of 200-400°C, the NO removal efficiency was as low as 70.5% and as high as 82.3%; the o-dichlorobenzene removal efficiency was as low as 62.6% and as high as 73.2%. After two hours of reaction, the catalyst gained 0.878 g, with a weight gain ratio of 35.3%.
[0085] (5) Contrast effect
[0086] Compared with Example 1, the prepared catalyst was only doped with V. The NO removal rate and o-dichlorobenzene removal efficiency of the sample decreased significantly, and the catalyst gained weight significantly after the reaction. Analysis showed that the reason may be that the lack of Ru doping caused the hydrophobicity of the catalyst to decrease, resulting in a decrease in catalytic performance.
Claims
1. A method for preparing a ruthenium-vanadium dual-doped cerium-manganese catalyst for denitration and removal of VOCs, characterized in that: The preparation method of the catalyst is as follows: (1) Preparation of Mn-MOF A manganese salt and a high molecular polymer are dissolved in a solvent to form a solution A, a 1,3,5-benzoic acid solution is slowly added to the solution A and allowed to stand for 10 to 16 hours, a precipitate is collected and washed and dried, and the obtained sample is marked as Mn-MOF; (2) Mn μ CeO x Catalyst preparation The Mn-MOF powder is added to the cerium salt solution and mixed, and then centrifuged, washed, dried and calcined in sequence to obtain Mn μ CeO x catalyst, wherein μ represents the molar ratio of Mn / Ce; (3) Ru, V dual doping Mn μ CeO x The catalyst is added to the solvent and mixed to obtain a suspension, and then the vanadium salt and the ruthenium salt are added to the suspension and mixed again. After mixing, it is dried and calcined twice to obtain the final product RuV / Mn μ CeO x .
2. The preparation method according to claim 1, characterized in that: The high molecular polymer described in step (1) is polyvinyl pyrrolidone, and the mass ratio of manganese salt, high molecular polymer and 1,3,5-benzoic acid is 0.1-1:1-4:0.5-1.
5.
3. The preparation method according to claim 1, characterized in that: The drying in step (1) is carried out in a vacuum drying oven, the drying temperature is 70 to 90° C., and the drying time is 10 to 14 hours.
4. The preparation method according to claim 1, characterized in that: In step (2), the calcination temperature is 300-600° C. and the calcination time is 2-4 hours.
5. The preparation method according to claim 1, characterized in that: In step (3), the first drying temperature is 40-70° C., the calcination time is 2-4 hours, the calcination temperature is 250-400° C., and the calcination atmosphere is 5-15% H2 / Ar atmosphere.
6. The preparation method according to claim 1, characterized in that: In step (3), the second drying temperature is 40-70° C., the calcination time is 2-4 hours, the calcination temperature is 600-800° C., and the calcination atmosphere is 5-15% H2 / Ar atmosphere.
7. The preparation method according to claim 1, characterized in that: The manganese salt described in step (1) is Mn(OAc)2·4H2O, and the cerium salt is Ce(NO3)3·6H2O; the vanadium salt described in step (3) is NH4VO3, and the ruthenium salt is Rucl3·3H2O.
8. The preparation method according to claim 1, characterized in that: RuV / Mn μ CeO x The mass ratio of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide is 1-5:1-5:0.1-5:0.1-5; Preferably, the mass ratio of cerium oxide, manganese oxide, ruthenium oxide and vanadium oxide is 2-4:1-2:0.1-1.5:0.1-1.
9. A ruthenium and vanadium dual-doped cerium-manganese catalyst for denitration and removal of VOCs, characterized in that: The catalyst is prepared by the method described in any one of claims 1 to 8.
10. The catalyst prepared in claim 1 is used as a catalyst for the synergistic removal of VOCs and NO x Application in this area.
Citation Information
Patent Citations
Preparation method and application of vanadium-doped umbrella-shaped manganese-cerium composite oxide catalyst
CN109201042A
Ce-Mn bimetallic oxide with high water resistance as well as preparation method and application of Ce-Mn bimetallic oxide
CN116726909A
Sea urchin-shaped rare earth-based catalyst for simultaneous denitration and VOCs removal and preparation method thereof
CN117019172A
Nano-flower-shaped rare earth-based catalyst for simultaneous denitration and VOCs removal and preparation method of nano-flower-shaped rare earth-based catalyst
CN117205918A