Preparation method and application of sulfur and nitrogen co-modified zero-valent iron composite material based on biological vulcanization

By using biosulfide sulfur and nitrogen to comodify zero-valent iron composites in groundwater, the problem of difficult degradation of chlorinated hydrocarbon pollution in groundwater is solved, and the degradation efficiency of trichloroethylene and trichloromethane is significantly improved, achieving high efficiency , environmentally friendly pollution removal effect.

CN119034778AActive Publication Date: 2024-11-29ZHEJIANG UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411011349.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-29
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Chlorinated hydrocarbons in groundwater are seriously polluted, and the existing zero-valent iron technology is prone to agglomeration and reduces its reaction activity, which limits its large-scale application and is difficult to effectively degrade chlorine-containing organic pollutants.

Method used

The preparation method of sulfur and nitrogen-co-modified zero-valent iron composite materials based on biosulfide is adopted, and the sulfate reducing bacteria and nitrogen-modified zero-valent iron are co-cultured in an oxygen-free environment to form sulfur and nitrogen-co-modified zero-valent iron composite materials. Used to repair chlorine-containing organic pollutants. The method includes mixing the sterilized sulfate reducing bacteria culture medium with nitrogen-modified zero-valent iron, inoculating the sulfate reducing bacteria, conducting microbial vulcanization culture, and centrifugation, washing and drying under an inert gas atmosphere.

Benefits of technology

The prepared sulfur and nitrogen co-modified zero-valent iron composite material significantly improves the degradation rate of trichloroethylene and trichloromethane in groundwater. Compared with the use of nitrogen alone to modify zero-valent iron, the degradation efficiency is improved, and the process is simple. Low cost and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034778A_ABST
    Figure CN119034778A_ABST
Patent Text Reader

Abstract

The preparation method of the sulfur and nitrogen co-modified zero-valent iron composite material based on biological vulcanization specifically comprises the following steps: carrying out anaerobic sterilization on a sulfate reducing bacteria culture medium to obtain a sterilized culture solution; mixing the sterilized culture solution with nitrogen-modified zero-valent iron, inoculating sulfate reducing bacteria, and performing microorganism vulcanization culture in an oxygen-free environment to obtain a microorganism composite material; and under the inert gas atmosphere, centrifuging, washing and drying the microbial composite material in ethanol to obtain the sulfur and nitrogen co-modified zero-valent iron composite material. The sulfate reducing bacteria and the nitrogen modified zero-valent iron are jointly cultured in the culture medium, the sulfur and nitrogen co-modified zero-valent iron is finally obtained, and the preparation process is simple, efficient, low in cost and environmentally friendly and can be widely applied to preparation of the sulfur and nitrogen co-modified zero-valent iron.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sewage treatment, and specifically relates to a preparation method and application of a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization. Background Art

[0002] With the acceleration of industrialization and urbanization, the pollution of chlorinated hydrocarbons in groundwater is becoming increasingly serious. Groundwater in many places has been polluted to varying degrees, and the scope of pollution is constantly expanding. Therefore, the prevention and control of chlorinated hydrocarbon pollution in groundwater in contaminated sites is urgent.

[0003] Since groundwater always contains different anions and sulfate-reducing bacteria, it is possible to consider adding bio-friendly iron-based materials to groundwater for biosulfurization to generate FeS, thereby promoting the degradation of chlorinated hydrocarbons in groundwater. Among them, zero-valent iron (ZVI) has attracted widespread attention due to its advantages such as large specific surface area, high reactivity, few intermediates, and environmental friendliness. However, ZVI is prone to agglomeration and passivation, resulting in reduced mobility and reactivity, which limits the large-scale application of zero-valent iron technology. The high corrosion resistance of iron nitride and its catalytic properties can significantly improve the reactivity and selectivity of ZVI technology, so zero-valent iron nitride has good application prospects in groundwater bioremediation. Summary of the invention

[0004] In view of the problem that chlorinated olefins in existing groundwater are difficult to biodegrade, the present invention provides a preparation method and application of a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization, which is simple to operate, pollution-free and highly stable. The specific technical scheme is as follows:

[0005] A method for preparing a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization, the method specifically comprising:

[0006] The sulfate-reducing bacteria culture medium is sterilized anaerobically to obtain a sterilized culture solution; the sterilized culture solution and nitrogen-modified zero-valent iron are mixed, inoculated with sulfate-reducing bacteria, and microbial sulfurization culture is carried out in an anaerobic environment to obtain a microbial composite material; in an inert gas atmosphere, the microbial composite material is centrifuged in ethanol, washed and dried to obtain a sulfur-nitrogen co-modified zero-valent iron composite material.

[0007] Furthermore, the sulfate-reducing bacteria culture medium includes the following components: KH2PO4: 0.5±0.05g / L, NH4Cl: 1±0.05g / L, CaCl2: 0.08±0.005g / L, MgSO4·7H2O: 1.1±0.1g / L, DL-sodium lactate: 2±0.1g / L, sodium thioglycolate: 0.1±0.01g / L, yeast extract: 1±0.05g / L, and vitamin C: 0.1±0.005g / L.

[0008] Furthermore, the addition ratio of the sterile culture solution and the nitrogen-modified zero-valent iron satisfies that the ratio of the amount of sulfate substance in the sterile culture solution to the amount of nitrogen-modified zero-valent iron substance is 0.03-0.2:1.

[0009] Furthermore, the OD of the sulfate-reducing bacteria in the sterilized culture medium is 600 The concentration is 0.01-0.1.

[0010] Furthermore, the conditions for the microbial sulfurization culture are: temperature 28-30°C, static culture, and culture time is 6-7D.

[0011] Furthermore, the inert gas atmosphere is an argon atmosphere.

[0012] The sulfur and nitrogen co-modified zero-valent iron composite material prepared by the above preparation method is used in the repair of groundwater containing chlorine organic pollutants.

[0013] Furthermore, the chlorine-containing organic pollutant is at least one of trichloroethylene and chloroform.

[0014] The present invention cultivates sulfate-reducing bacteria and nitrogen modification together in a culture medium to ultimately obtain sulfur- and nitrogen-co-modified zero-valent iron. The preparation process is simple, efficient, low-cost, and environmentally friendly, and can be widely used in the preparation of sulfur- and nitrogen-co-modified zero-valent iron. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The X-ray diffraction spectrum (XRD) diagram of the iron-based material prepared by the present invention;

[0016] Figure 2 The X-ray photoelectron spectroscopy (XPS) diagram of S2p of the iron-based material prepared in the present invention;

[0017] Figure 3 This is the degradation diagram of the culture medium with S / Fe=0.05 during the preparation of the iron-based material of the present invention; wherein: (A) is SO4 2- The degradation diagram of S 2- The generated graph of Fe 2+ The generated graph of

[0018] Figure 4 This is the degradation diagram of the culture medium with S / Fe=0.1 during the preparation of the iron-based material of the present invention; wherein: (A) is SO4 2- The degradation diagram of S 2- The generated graph of Fe 2+ The generated graph of

[0019] Figure 5The figure is a degradation effect diagram of trichloroethylene degradation by the iron-based material prepared in the present invention; wherein: SN-ZVI represents the sulfur-nitrogen-modified zero-valent iron material prepared in Example 1, and N-ZVI represents the nitrogen-modified zero-valent iron material prepared in Comparative Example 1;

[0020] Figure 6 The figure is a degradation effect diagram of the iron-based material prepared by the present invention in the process of degrading chloroform; wherein: SN-ZVI represents the sulfur-nitrogen-modified zero-valent iron material prepared in Example 1, and N-ZVI represents the nitrogen-modified zero-valent iron material prepared in Comparative Example 1;

[0021] Figure 7 The figure is a degradation effect diagram of trichloroethylene degradation by the iron-based material prepared in the present invention; wherein: SN-ZVI represents the sulfur-nitrogen-modified zero-valent iron material prepared in Example 2, and N-ZVI represents the nitrogen-modified zero-valent iron material prepared in Comparative Example 2;

[0022] Figure 8 This is a diagram showing the degradation effect of the iron-based material prepared in the present invention during the degradation of chloroform; wherein: SN-ZVI represents the sulfur-nitrogen modified zero-valent iron material prepared in Example 2, and N-ZVI represents the nitrogen-modified zero-valent iron material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with the accompanying drawings in order to better understand the technical solution.

[0024] Example 1: Preparation of sulfur and nitrogen co-modified zero-valent iron

[0025] Under anaerobic conditions, the culture medium was dispensed into 100 mL serum bottles, each containing 55 mL of 1.1 g / L SO4 2- The culture medium was sterilized at 121°C for 15 min under high pressure, cooled to room temperature, brought into a glove box, 0.3 g of nitrogen-modified zero-valent iron was placed in the sterilized culture medium, and 5 mL of the resuspended bacterial solution was added. After culturing for 6 days, the culture medium was washed with ethanol in an inert gas atmosphere and dried in a glove box to obtain a sulfur-nitrogen co-modified zero-valent iron material SN-ZVI ([S / Fe]=0.05) with a molar ratio of sulfur to iron of 0.05.

[0026] Example 2: Preparation of sulfur and nitrogen co-modified zero-valent iron

[0027] Under anaerobic conditions, the culture medium was dispensed into 100 mL serum bottles, each containing 55 mL of 2.2 g / L SO4 2-The medium was sterilized at 121°C for 15 minutes, cooled to room temperature, and brought into a glove box. 0.3 g of nitrogen-modified zero-valent iron was placed in the sterilized medium, and 5 mL of the resuspended bacterial solution after centrifugation was added. After 6 days of culture, it was washed with ethanol in an inert gas atmosphere and dried in a glove box. The sulfur-nitrogen co-modified zero-valent iron material SN-ZVI ([S / Fe]=0.1) with a molar ratio of sulfur to iron of 0.1 was obtained.

[0028] Comparative Example 1: Preparation of nitrogen-modified zero-valent iron

[0029] Under anaerobic conditions, the culture medium was dispensed into 100 mL serum bottles, each containing 55 mL of 1.1 g / L SO4 2- The culture medium was sterilized under high pressure at 121°C for 15 min, cooled to room temperature, brought into a glove box, 0.3 g of nitrogen-modified zero-valent iron was placed in the sterilized culture medium, and cultured for 6 days, washed with ethanol in an inert gas atmosphere, and dried in a glove box to obtain nitrogen-modified zero-valent iron material (N-ZVI, [S / Fe] = 0.05).

[0030] Comparative Example 2: Preparation of nitrogen-modified zero-valent iron

[0031] Under anaerobic conditions, the culture medium was dispensed into 100 mL serum bottles, each containing 55 mL of 2.2 g / L SO4 2- The culture medium was sterilized under high pressure at 121°C for 15 min, cooled to room temperature, brought into a glove box, 0.3 g of nitrogen-modified zero-valent iron was placed in the sterilized culture medium, and cultured for 6 days, washed with ethanol in an inert gas atmosphere, and dried in a glove box to obtain nitrogen-modified zero-valent iron material (N-ZVI, [S / Fe] = 0.1).

[0032] The materials obtained in Example 1-2 and Comparative Example 1-2 were washed with oxygen-free ethanol, dried in a glove box for 72 hours, and the samples were ground and collected in sample bottles for later use.

[0033] The XRD patterns of the samples obtained in Example 1 and Comparative Example 1 are as follows: Figure 1 As shown, FeS and Fe3N exist on the surface of SN-ZVI particles prepared in Example 1, indicating that ferrous sulfide is successfully generated during the biosulfurization process. Part of Fe3N is still retained on the surface of N-ZVI particles prepared in Comparative Example 1, indicating that the biosulfurization process will not cause complete loss of iron nitride.

[0034] The element distribution of the materials was further analyzed by XPS. The element distribution in SN-ZVI prepared in Example 1 and N-ZVI prepared in Comparative Example 1 was studied. Figure 2 As shown, there is S on the surface of SN-ZVI prepared in Example 1.2- With S n 2- , indicating the presence of polysulfides inside the material.

[0035] The biosulfurization process of SN-ZVI was monitored and it was found that the SO4 2- The consumption rate is similar to that of the reaction system with only bacteria added. 2- The amount of SO4 generated 2- The consumption of Fe is basically conserved during the reaction. 2+ The amount of generated is small, indicating that polysulfide ( Figure 3 , Figure 4 ).

[0036] Application Example 1: Effect of sulfur and nitrogen co-modified zero-valent iron on the removal of trichloroethylene in groundwater

[0037] Add 26 mL of buffer solution to each of the two groups of 52 mL serum bottles, add 0.26 g of SN-ZVI prepared in Example 1, 0.26 g of N-ZVI prepared in Comparative Example 1, and 19 microliters of 17.9 g / L TCE solution to each to make its initial concentration 100 μM. Finally, send the serum bottles to a 25°C constant temperature incubator and place them on a rotating incubator with a rotation speed of n = 30 rpm for uninterrupted and sufficient mixing reaction.

[0038] At the designed sampling time node, 100 μL of the headspace gas in the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the TCE concentration in the serum bottle at the sampling time node. The experimental results are as follows: Figure 5 As shown in Figure 2, linear fitting shows that the degradation rate of SN-ZVI with [S / Fe] of 0.05 is 1.94 times that of N-ZVI. This indicates that sulfur and nitrogen co-modification of zero-valent iron can greatly improve the removal effect of TCE.

[0039] Application Example 2: Effect of sulfur and nitrogen co-modified zero-valent iron on the removal of chloroform in groundwater

[0040] 26 mL of buffer solution was added to each of the two groups of 52 mL serum bottles, and 0.26 g of SN-ZVI prepared in Example 1 and 0.26 g of N-ZVI prepared in Comparative Example 1 were added respectively. 21 microliters of 14.85 g / L CF solution were added to each of the two groups of 52 mL serum bottles to make the initial concentration 100 μM. Finally, the serum bottles were sent to a 25°C constant temperature incubator and placed on a rotating incubator with a rotation speed of n = 30 rpm for uninterrupted and sufficient mixing reaction.

[0041] At the designed sampling time node, 100 μL of the headspace gas in the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the CF concentration in the serum bottle at the sampling time node. The experimental results are as follows: Figure 6 As shown in Figure 2, linear fitting shows that the degradation rate of SN-ZVI with [S / Fe] of 0.05 is 5.26 times that of N-ZVI. This indicates that sulfur and nitrogen co-modification of zero-valent iron can greatly improve the removal effect of CF.

[0042] Application Example 3: Effect of sulfur and nitrogen co-modified zero-valent iron on the removal of trichloroethylene in groundwater

[0043] Add 26 mL of buffer solution to each of the two groups of 52 mL serum bottles, add 0.26 g of SN-ZVI prepared in Example 2, 0.26 g of N-ZVI prepared in Comparative Example 2, and 19 microliters of 17.9 g / L TCE solution to each to make its initial concentration 100 μM. Finally, send the serum bottles to a 25°C constant temperature incubator and place them on a rotating incubator with a rotation speed of n = 30 rpm for uninterrupted and sufficient mixing reaction.

[0044] At the designed sampling time node, 100 μL of the headspace gas in the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the TCE concentration in the serum bottle at the sampling time node. The experimental results are as follows: Figure 7 As shown in Figure 2, linear fitting shows that the degradation rate of SN-ZVI with [S / Fe] of 0.1 is 2.6 times that of N-ZVI. This indicates that sulfur and nitrogen co-modification of zero-valent iron can greatly improve the removal effect of TCE.

[0045] Application Example 4: Effect of sulfur and nitrogen co-modified zero-valent iron on the removal of chloroform in groundwater

[0046] 26 mL of buffer solution was added to each of the two groups of 52 mL serum bottles, and 0.26 g of SN-ZVI prepared in Example 2 and 0.26 g of N-ZVI prepared in Comparative Example 2 were added respectively. 21 microliters of 14.85 g / L CF solution were added to each of the two groups of 52 mL serum bottles to make the initial concentration 100 μM. Finally, the serum bottles were sent to a 25°C constant temperature incubator and placed on a rotating incubator with a rotation speed of n = 30 rpm for uninterrupted and sufficient mixing reaction.

[0047] At the designed sampling time node, 100 μL of the headspace gas in the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the CF concentration in the serum bottle at the sampling time node. The experimental results are as follows: Figure 8 As shown in Figure 2, linear fitting shows that the degradation rate of SN-ZVI with [S / Fe] of 0.1 is 4.9 times that of N-ZVI. This indicates that sulfur and nitrogen co-modification of zero-valent iron can greatly improve the removal effect of CF.

Claims

1. A method for preparing a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization, characterized in that The method is specifically: The sulfate-reducing bacteria culture medium is sterilized anaerobically to obtain a sterilized culture solution; the sterilized culture solution and nitrogen-modified zero-valent iron are mixed, inoculated with sulfate-reducing bacteria, and microbial sulfurization culture is carried out in an anaerobic environment to obtain a microbial composite material; in an inert gas atmosphere, the microbial composite material is centrifuged in ethanol, washed and dried to obtain a sulfur-nitrogen co-modified zero-valent iron composite material.

2. The method for preparing a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization according to claim 1, characterized in that The sulfate-reducing bacteria culture medium comprises the following components: KH2PO4: 0.5±0.05 g / L, NH4Cl: 1±0.05 g / L, CaCl2: 0.08±0.005 g / L, MgSO4·7H2O: 1.1±0.1 g / L, DL-sodium lactate: 2±0.1 g / L, sodium thioglycolate: 0.1±0.01 g / L, yeast extract: 1±0.05 g / L, and vitamin C: 0.1±0.005 g / L.

3. The method for preparing a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization according to claim 1, characterized in that The addition ratio of the sterile culture solution and the nitrogen-modified zero-valent iron satisfies that the ratio of the amount of sulfate substance in the sterile culture solution to the amount of nitrogen-modified zero-valent iron substance is 0.03-0.2:

1.

4. The method for preparing a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization according to claim 1, characterized in that The OD of the sulfate-reducing bacteria in the sterile culture medium 600 The concentration is 0.01-0.

1.

5. The method for preparing a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization according to claim 1, characterized in that The conditions for the microbial vulcanization culture are: temperature 28-30° C., static culture, and culture time 6-7 days.

6. The method for preparing a sulfur-nitrogen co-modified zero-valent iron composite material based on biosulfurization according to claim 1, characterized in that The inert gas atmosphere is an argon atmosphere.

7. Application of the sulfur-nitrogen co-modified zero-valent iron composite material obtained by the preparation method described in any one of claims 1 to 6 in the remediation of groundwater containing chlorine-containing organic pollutants.

8. The use according to claim 7, characterized in that The chlorine-containing organic pollutant is at least one of trichloroethylene and chloroform.

Citation Information

Patent Citations

  • Preparation method and application of nitrogen-doped zero-valent iron composite material

    CN111847541A

  • Biological preparation method and application of sulfurized zero-valent iron

    CN117904212A