EO hydroesterification heterogeneous catalyst and preparation method thereof
By using cobalt or palladium as a heterogeneous catalyst composed of metal components and organic phosphine nitrogen porous polymer in the EO hydrogenation reaction, the problems of difficulty in separation and insufficient stability of cobalt homogeneous catalysts are solved, and efficient catalyst selection is achieved and stability, suitable for industrial production.
Patent Information
- Application Number
- CN202411217988.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-02
AI Technical Summary
The separation of reaction materials of cobalt homogeneous catalysts in the existing EO hydrogenation reaction is difficult, which hinders large-scale application. The preparation and separation process of heterogeneous catalysts is complicated, and the catalyst stability and recycling are insufficient.
Using a heterogeneous catalyst composed of metal components (cobalt or palladium) and an organic phosphine nitrogen porous polymer, a porous organic with a block structure is obtained by solvent polymerization of vinyl and phenyl organic phosphine, pyridine and p-methylstyrene. The polymer, supported metal components, forms a stable heterogeneous catalyst, reducing the cost of separation between the catalyst and the reactants and improving the stability of the catalyst.
The efficient EO hydrogenation reaction is achieved, which improves the selectivity and stability of the catalyst, is suitable for industrial production, and reduces the separation cost between the catalyst and the reactants.
Smart Images

Figure CN119034810A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heterogeneous catalysis, and in particular relates to the preparation and application of a heterogeneous catalyst for EO hydrogenation. Background Art
[0002] Polytrimethylene terephthalate (PTT) is a new polyester polymer material with great development prospects developed after polyethylene terephthalate (PET) in the 1950s and polybutylene terephthalate (PBT) in the 1970s. The main use of 1,3-propylene glycol is to be used as a polymerization monomer to generate polytrimethylene terephthalate through the polymerization reaction of terephthalic acid. At the same time, it is also a raw material for the production of antifreeze, anti-slip agents, plasticizers, cosmetics, and surfactants. At present, there are three main processes for 1,3-propylene glycol: the ethylene oxide hydroformylation hydrogenation method industrialized by Shell Company in the United States in 1996; the acrolein hydration hydrogenation method successfully developed by Degussa Company in Germany in 1995; and the microbial fermentation method represented by DuPont Company in the United States. There is no obvious difference in production capacity among the above three methods, but each has its own characteristics. The process conditions of acrolein hydration hydrogenation method are mild, the technical difficulty is not great, the hydrogenation process is mature, and the equipment requirements are not high. However, the raw material acrolein of this route is highly toxic and flammable and explosive, which is difficult to store and transport, and the cost is also high. The microbial fermentation method is characterized by "green chemistry", using renewable resources, clean production environment, mild reaction conditions, simple operation, and low pollution, but the product concentration is low and the production efficiency is difficult to improve. Ethylene oxide has the advantages of abundant sources and low prices, and the ethylene oxide method is highly favored, but the intermediate 3-hydroxypropanal in the ethylene oxide hydroformylation method is extremely unstable, and the catalytic separation technology is complex. A high-pressure reactor greater than 10 MPa is required, which has high equipment requirements, high comprehensive technical difficulty, and high investment cost. In comparison, the ethylene oxide hydroesterification method produces 1,3-propylene glycol and generates 3-hydroxypropionic acid methyl ester, which avoids the production of 3-hydroxypropanal and becomes a new research direction for the ethylene oxide method.
[0003] Patent US6191321 uses Co2(CO)8 / 1,10-phenanthroline catalyst, reacts at 90℃ and 7.6 MPa for 18h, the conversion rate of ethylene oxide is only 11%, and the selectivity of methyl 3-hydroxypropionate is 74%. Patent US6521801 uses cobalt salt catalyst coordinated by nitrogen-containing heterocyclic compounds, and the conversion rate of ethylene oxide is 94% at 75℃ and 6 MPa, and the selectivity of methyl 3-hydroxypropionate is 78%. Patent CN101020635A uses carbonyl cobalt catalyst, and the conversion rate of ethylene oxide is 80-98% at 50-100℃ and 3-7 MPa, and the selectivity of methyl 3-hydroxypropionate is only 80%. Patents CN107349962 and CN107417527 use Co2(CO)8 / imidazole as catalysts, react at 75°C and 2 MPa for 5 h, and the conversion rate of ethylene oxide is 87%, and the yield of methyl 3-hydroxypropionate is 83%. Patents CN 107456995 and CN107459451 use catalysts composed of ionic liquids and cuprous halide or cobalt chloride, react at 60-75°C and 5-6 MPa, and the conversion rate of ethylene oxide is 71%-89%, and the selectivity of methyl 3-hydroxypropionate is 83%-86%.
[0004] In the EO hydroesterification reaction, most of the current processes use carbonyl cobalt homogeneous catalytic systems, which can have high catalytic activity and selectivity for the target product under mild reaction conditions. However, the separation of cobalt homogeneous catalysts from the reaction materials is difficult, which hinders the large-scale application of homogeneous catalytic systems in the EO hydroesterification reaction. With the advancement of homogeneous solid-support technology, researchers have begun to study the technology of heterogeneous catalysts for EO hydroesterification.
[0005] Patent CN1125712A uses 5%-40% of low-concentration olefins with 2-6 carbon atoms as raw materials, and supports the carbonyl Rh-P homogeneous catalyst on polymer microspheres or alumina carriers. Patent CN102281948A reports a polymer-supported transition metal catalyst complex and a method of use, and prepares a soluble polymer-supported rhodium catalyst with a narrow molecular weight distribution. However, the catalyst preparation, catalytic reaction and catalyst separation processes are complicated. Catalyst preparation requires first controlling the functional monomers and synthetic soluble polymers such as styrene, then introducing ligands, and finally loading the Rh catalyst. Compressed gas needs to be added during the catalytic reaction. The catalyst is separated from the reaction mixture by nanofiltration, and the reaction results are not ideal. Patent CN106431926B reports that carbonyl cobalt is loaded in 4-vinylpyridine and styrene, methyl styrene, (methyl) acrylate, ethyl (methyl) acrylate, butyl (methyl) acrylate, ethyl vinylbenzene and other comonomers with a molecular weight of 60,000-1,600,000,000, in a 4-vinylpyridine monomer unit block copolymer. However, there is a problem of low conversion of methyl trihydroxypropionate, and no data on catalyst cycle stability are mentioned. Patent CN113713862B uses divalent cobalt salt to load on a polymer generated by solvent thermal polymerization of an organophosphine ligand of vinyl to form a cobalt-based heterogeneous catalyst, and is applied to EO formylation reaction. The patent does not mention data on catalyst cycle stability. Therefore, the development of a heterogeneous solid-supported catalyst system with stable performance has important practical application significance. Summary of the invention
[0006] In order to solve the above problems, the present invention aims to provide a heterogeneous catalyst for EO hydroesterification reaction.
[0007] To achieve the above object, the present invention adopts the following technical solution: A multiphase catalyst for EO hydroesterification, the catalyst consists of a metal component and an organic phosphine-nitrogen porous polymer; the metal component is one of cobalt and palladium, and the organic phosphine-nitrogen porous polymer is a porous organic polymer with a block structure obtained by solvent polymerization of an organic phosphine containing vinyl and phenyl, pyridine containing vinyl and p-methylstyrene.
[0008] Furthermore, the above metal components account for 0.1-20.0% of the total weight of the heterogeneous catalyst.
[0009] Furthermore, the specific surface area of the organic phosphorus nitrogen porous polymer is 600-1200 m 2 / g, pore volume 0.1-5.0 cm 3 / g, and the pore size distribution is 0.1-200 nm.
[0010] A method for preparing a heterogeneous catalyst for EO hydroesterification comprises the following steps: (1) Adding a solvent and a free radical initiator to an organic phosphine containing vinyl and phenyl groups, pyridine containing vinyl groups and p-methylstyrene, and stirring at room temperature for 1-5 hours to form a prepolymer solution; (2) pouring the prepolymer solution of step (1) into a hydrothermal reactor, performing a hot melt polymerization reaction at 100-150°C for 2-25 hours, cooling to room temperature and filtering, soaking in anhydrous ethanol, washing, filtering, and drying at 50°C for 5 hours to obtain an organic phosphine nitrogen porous polymer; (3) The precursor of the metal component is dissolved in a solvent to obtain a solution containing the metal component, and an organic phosphorus nitrogen porous polymer is added. After stirring at room temperature for 0.5-20 h, the temperature is raised to 50-80°C and stirring is continued for 0.5-20 h. After cooling to room temperature, the solution is filtered and dried at 50°C for 5 h to obtain a multiphase catalyst containing an organic phosphorus nitrogen porous polymer loaded with metal active components.
[0011] Furthermore, the free radical initiator in step (1) is one of dibenzoyl peroxide and azobisisobutyronitrile; the ratio of the amount of the free radical initiator to the total weight of the organic phosphine containing vinyl and phenyl, the pyridine containing vinyl and p-methylstyrene is 1:1000-1:10.
[0012] Furthermore, the solvent in step (1) is one or more of benzene, toluene, tetrahydrofuran, methanol, ethanol, methyl acetate, and methyl tert-butyl ether.
[0013] Furthermore, in step (3), the precursors of the metal components cobalt and palladium are one or more of Co(NO3)2, CoCl2, Co(OAc)2, Co(acac)2, Co(OH)2, PdCl2, Pd(NO3)2, H2PdCl4, Pd(OAc)2; and the solvent is one or more of methanol, ethanol, methyl acetate, and methyl tert-butyl ether.
[0014] The present invention also provides an application of the above-mentioned multiphase catalyst in EO hydroesterification reaction, and the specific operation steps are: under the conditions of the multiphase catalyst, ethylene oxide, carbon monoxide and methanol are subjected to hydroesterification reaction in a kettle reactor, the reaction temperature is 30-100°C, the reaction pressure is 0.1-10.0 MPa, the reaction time is 3-25 h, the molar ratio of the loaded metal of ethylene oxide and the multiphase catalyst is 20-200:1; the weight proportion of the metal component in the reaction system is 0.2 wt%-0.5 wt%.
[0015] The present invention uses an organic phosphine monomer (organic phosphine containing vinyl and phenyl) as a comonomer. A pair of lone pairs of electrons of the P atom can be used as electron pair donors to form a σ bond with the metal, and there is an empty d orbital to form a π bond with the metal, and a stable coordination bond is formed with the metal, thereby improving the stability of the catalyst and preventing the loss of the metal in the reaction. At the same time, a nitrogen monomer (pyridine containing vinyl) is used as a comonomer to introduce the N structure into the reaction system. The N structure on the carrier and the metal coordinate under the reaction conditions to form a Lewis acid site, thereby promoting the ring opening of ethylene oxide, thereby increasing the reaction rate, and also avoiding the problem that the traditional homogeneous catalyst adds nitrogen promoters such as imidazole and pyridine in the EO hydrogen esterification reaction, which causes the promoter to be difficult to separate after the reaction. Finally, p-methylstyrene is used as a polymer structure coupling agent, and a porous polymer with a specific block structure is formed by adding a suitable proportion of coupling agents, thereby adjusting the distribution sites of the nitrogen and phosphorus structures and promoting the reaction activity and product selectivity. The invention ternary copolymerizes a promoter required for EO hydrogen esterification, a phosphine ligand for stabilizing metals and p-methylstyrene to obtain an organic phosphine nitrogen porous polymer, and then loads metal to obtain a multiphase catalyst, thereby improving the binding ability of the metal on the organic carrier and reducing the separation cost of the catalyst from reactants and products.
[0016] The beneficial effects produced by the present invention are: (1) Compared with the existing homogeneous catalyst preparation technology, the use of new heterogeneous catalysts reduces the separation cost of catalysts from reactants and products while ensuring the selectivity of catalyst products.
[0017] (2) Compared with existing multiphase catalysts, it has higher catalyst stability and can be reused after the reaction, making it suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 : Schematic diagram of the structure of the organic phosphine nitrogen porous polymer prepared in Example 1.
[0019] Figure 2 : The conversion of EO and the selectivity of 3-HPM in the EO hydroesterification reaction of Example 1 and Examples 6-8.
[0020] Figure 3 : Comparative Examples 3-6: EO conversion and 3-HPM selectivity in EO hydroesterification reaction. DETAILED DESCRIPTION
[0021] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.
[0022] Example 1 In a fume hood, 4.8 g of diphenyl (4-vinylphenyl) phosphine, 2.8 g of 4-vinyl pyridine and 2.6 g of p-methylstyrene were weighed and added to a 250 ml polymerization flask, and 100 ml of tetrahydrofuran and 0.20 g of azobisisobutyronitrile as a free radical initiator were added, and stirred at room temperature for 2 h to form a prepolymer solution; the prepolymer solution was poured into a hydrothermal autoclave and subjected to a hot melt polymerization reaction at 100 °C for 15 h; after the reaction was completed, the hydrothermal autoclave was cooled to room temperature, the polymer in the autoclave was filtered, and then anhydrous ethanol was added for soaking, washing, and suction filtration, and then dried in a 50 °C oven for 5 h to obtain an organic phosphorus nitrogen porous polymer (specific surface area 850 m 2 / g, pore volume 1.2 cm 3 / g, pore size distribution 0.5-100 nm).
[0023] Weigh 0.95 g of cobalt acetate and dissolve it in 100 ml of methanol, add 3.0 g of the organic nitrogen-phosphorus porous polymer prepared above, stir at room temperature for 2 h, heat to 50-80 °C and continue stirring for 10 h, cool to room temperature and filter, place the filtered solid in a 50 °C oven and dry for 5 h to obtain a heterogeneous catalyst of organic phosphorus-nitrogen porous polymer loaded with cobalt.
[0024] All the above catalysts were transferred to a 200 ml reactor, which was purged with nitrogen three times, and carbon monoxide, 0.15 mol ethylene oxide, and 100 ml methanol were added to make the system pressure 6 MPa; the reaction was carried out at 40 °C for 20 hours. After the reaction, the reactor was cooled to 0 °C, the pressure was slowly released to normal pressure, and the reactor was purged with nitrogen three times. Samples were taken for analysis, and the EO conversion rate and 3-HPM selectivity are shown in Table 1.
[0025] Example 2 In a fume hood, 4.8 g of diphenyl (4-vinylphenyl) phosphine, 2.8 g of 4-vinyl pyridine and 2.6 g of p-methylstyrene were weighed and added to a 250 ml polymerization flask, and 100 ml of tetrahydrofuran and 0.30 g of dibenzoyl peroxide as a free radical initiator were added, and stirred at room temperature for 2 h to form a prepolymer solution; the prepolymer solution was poured into a hydrothermal kettle, and a hot melt polymerization reaction was carried out at 100 ° C for 15 h, and then cooled to room temperature. After filtering the polymer in the kettle, anhydrous ethanol was added for soaking, washing, and suction filtration, and then placed in a 50 ° C oven for drying for 5 h to obtain an organic phosphorus nitrogen porous polymer (specific surface area 826 m 2 / g, pore volume 1.06cm 3 / g, pore size distribution 0.5-120 nm).
[0026] Weigh 0.95 g of cobalt acetate and dissolve it in 100 ml of methanol, add 3.0 g of the organic nitrogen-phosphorus porous polymer prepared above, stir at room temperature for 2 h, heat to 50-80 °C and continue stirring for 10 h, cool to room temperature and filter, place the filtered solid in a 50 °C oven and dry for 5 h to obtain a heterogeneous catalyst of organic phosphorus-nitrogen porous polymer loaded with cobalt.
[0027] The catalytic process conditions were the same as those in Example 1. The EO conversion and 3-HPM selectivity are shown in Table 1.
[0028] Example 3 In a fume hood, 5.8 g of tri(4-vinylphenyl)phosphine, 2.8 g of 4-vinylpyridine and 2.6 g of p-methylstyrene were weighed and added to a 250 ml polymerization flask, and 100 ml of tetrahydrofuran and 0.20 g of azobisisobutyronitrile as a free radical initiator were added, and stirred at room temperature for 2 h to form a prepolymer solution. The prepolymer solution was poured into a hydrothermal kettle, and a hot melt polymerization reaction was carried out at 100 ° C for 15 h, and then cooled to room temperature. After filtering the polymer in the kettle, anhydrous ethanol was added for soaking, washing, and suction filtration, and then placed in a 50 ° C oven for drying for 5 h to obtain an organic phosphorus nitrogen porous polymer (specific surface area 920 m 2 / g, pore volume 1.13 cm 3 / g, pore size distribution 0.5-100 nm).
[0029] Weigh 0.95 g of cobalt acetate and dissolve it in 100 ml of methanol, add 3.0 g of the organic nitrogen-phosphorus porous polymer prepared above, stir at room temperature for 2 h, heat to 50-80 °C and continue stirring for 10 h, cool to room temperature and filter, place the filtered solid in a 50 °C oven and dry for 5 h to obtain a heterogeneous catalyst of organic phosphorus-nitrogen porous polymer loaded with cobalt.
[0030] The catalytic process conditions were the same as those in Example 1. The EO conversion and 3-HPM selectivity are shown in Table 1.
[0031] Example 4 In a fume hood, 5.8 g of tri(4-vinylphenyl)phosphine, 2.8 g of 4-vinylpyridine and 2.6 g of p-methylstyrene were weighed and added to a 250 ml polymerization flask, and 100 ml of tetrahydrofuran and 0.20 g of azobisisobutyronitrile as a free radical initiator were added, and stirred at room temperature for 2 h to form a prepolymer solution. The prepolymer solution was poured into a hydrothermal kettle, and the thermosol polymerization reaction was carried out at 100 °C for 15 h, and then cooled to room temperature. After filtering the polymer in the kettle, anhydrous ethanol was added for soaking, washing, and suction filtration, and then placed in a 50 °C oven for drying for 5 h to obtain a phosphine nitrogen porous organic polymer (specific surface area 920 m 2 / g, pore volume 1.13 cm 3 / g, pore size distribution 0.5-100 nm).
[0032] Weigh 0.50 g of cobalt hydroxide and dissolve it in 100 ml of methanol, add 3.0 g of the organic nitrogen-phosphorus porous polymer prepared above, stir at room temperature for 2 h, heat to 50-80 °C and continue stirring for 10 h, cool to room temperature and filter, and place the filtered solid in a 50 °C oven to dry for 5 h to obtain a heterogeneous catalyst of organic phosphorus-nitrogen porous polymer loaded with cobalt.
[0033] The catalytic process conditions were the same as those in Example 1. The EO conversion and 3-HPM selectivity are shown in Table 1.
[0034] Example 5 In a fume hood, 4.8 g of diphenyl (4-vinylphenyl) phosphine, 2.6 g of p-methylstyrene and 2.8 g of 4-vinylpyridine were weighed and added into a 250 ml polymerization flask, and 100 ml of tetrahydrofuran and 0.20 g of azobisisobutyronitrile as a free radical initiator were added, and stirred at room temperature for 2 h to form a prepolymer solution; the prepolymer solution was poured into a hydrothermal kettle, and the thermosol polymerization reaction was carried out at 50 ° C for 15 h, and then cooled to room temperature. After filtering the polymer in the kettle, anhydrous ethanol was added for soaking, washing, and suction filtration, and then placed in a 50 ° C oven for 5 h to obtain an organic phosphorus nitrogen porous polymer (specific surface area 650 m 2 / g, pore volume 0.89 cm 3 / g, pore size distribution 0.8-180 nm).
[0035] Weigh 0.95 g of cobalt acetate and dissolve it in 100 ml of methanol, add 3.0 g of the organic nitrogen-phosphorus porous polymer prepared above, stir at room temperature for 2 h, heat to 50-80 °C and continue stirring for 10 h, cool to room temperature and filter, place the filtered solid in a 50 °C oven and dry for 5 h to obtain a heterogeneous catalyst of organic phosphorus-nitrogen porous polymer loaded with cobalt.
[0036] The catalytic process conditions were the same as those in Example 1. The EO conversion and 3-HPM selectivity are shown in Table 1.
[0037] Example 6 The catalyst after the reaction in Example 1 was centrifuged and recovered, and the recovered catalyst was dissolved in 100 ml of methanol. The obtained catalyst solution was directly transferred to a 200 ml reactor, and the reactor was purged with nitrogen three times. Carbon monoxide and ethylene oxide were added to make the system pressure 6 MPa; the reaction was carried out at 40 ° C for 20 h. After the reaction was completed, the reactor was cooled to 0 ° C, the pressure was slowly released to normal pressure, and the reactor was purged with nitrogen three times. Sampling analysis, EO conversion rate and 3-HPM selectivity are shown in Table 1.
[0038] Example 7 The catalyst after the reaction in Example 6 was centrifuged and recovered, and the recovered catalyst was dissolved in 100 ml of methanol. The obtained catalyst was catalyzed again, and the catalytic process conditions were the same as in Example 6. The EO conversion rate and 3-HPM selectivity are shown in Table 1.
[0039] Example 8 The catalyst after the reaction in Example 7 was centrifuged and recovered, and the recovered catalyst was dissolved in 100 ml of methanol. The obtained catalyst was catalyzed again, and the catalytic process conditions were the same as those in Example 6. The EO conversion rate and 3-HPM selectivity are shown in Table 1.
[0040] Comparative Example 1 In a fume hood, weigh 10 g of diphenyl (4-vinylphenyl) phosphine and add it to a 250 ml polymerization flask, add 100 ml of tetrahydrofuran and 0.20 g of azobisisobutyronitrile as a free radical initiator, and stir at room temperature for 2 h to form a prepolymer solution; pour the prepolymer solution into a hydrothermal kettle and perform a hot melt polymerization reaction at 100 °C for 15 h; cool to room temperature, filter the polymer in the kettle, add anhydrous ethanol to soak, wash, filter, and place in a 50 °C oven to dry for 5 h to obtain an organic phosphine porous polymer (specific surface area 960m 2 / g, pore volume 1.25 cm 3 / g, pore size distribution 0.2-100 nm).
[0041] Weigh 0.95 g of cobalt acetate and dissolve it in 100 ml of methanol, add 3.0 g of the organic porous polymer prepared above, stir at room temperature for 2 h, heat to 50-80 °C and continue stirring for 10 h, cool to room temperature and filter, and place the filtered solid in a 50 °C oven to dry for 5 h to obtain a heterogeneous catalyst of organic phosphine porous polymer loaded with cobalt.
[0042] The catalytic process conditions were the same as those in Example 1. The EO conversion and 3-HPM selectivity are shown in Table 1.
[0043] Comparative Example 2 In a fume hood, 6 g of diphenyl (4-vinylphenyl) phosphine and 3.5 g of 4-vinyl pyridine were weighed and added to a 250 ml polymerization flask, and 100 ml of tetrahydrofuran and 0.20 g of azobisisobutyronitrile as a free radical initiator were added, and stirred at room temperature for 2 h to form a prepolymer solution; the prepolymer solution was poured into a hydrothermal kettle and subjected to a hot melt polymerization reaction at 100 °C for 15 h; the prepolymer solution was cooled to room temperature, the polymer in the kettle was filtered, and then anhydrous ethanol was added for soaking, washing, and suction filtration, and then dried in a 50 °C oven for 5 h to obtain an organic phosphine nitrogen porous polymer (specific surface area 830 m 2 / g, pore volume 1.16cm 3 / g, pore size distribution 0.5-200 nm).
[0044] Weigh 0.95 g of cobalt acetate and dissolve it in 100 ml of methanol, add 3.0 g of the organic porous polymer prepared above, stir at room temperature for 2 h, heat to 50-80 °C and continue stirring for 10 h, cool to room temperature and filter, place the filtered solid in a 50 °C oven and dry for 5 h to obtain a heterogeneous catalyst of organic phosphine nitrogen porous polymer loaded with metal cobalt.
[0045] The catalytic process conditions were the same as those in Example 1. The EO conversion and 3-HPM selectivity are shown in Table 1.
[0046] Comparative Example 3 Alumina was used as the catalyst carrier. 0.95 g of cobalt acetate was dissolved in 3 ml of aqueous solution and impregnated onto 10 g of alumina carrier using an equal volume impregnation method. The impregnated catalyst was dried at 120 °C and then heated to 500 °C for calcination for 4 h. The calcined catalyst was placed in a tubular furnace and reduced with hydrogen at a reduction temperature of 300 °C to obtain a cobalt-loaded alumina catalyst (specific surface area 330 m 2 / g, pore volume 0.5 cm 3 / g, pore size distribution 0.4-500 nm).
[0047] The catalytic process conditions were the same as those in Example 1. The EO conversion and 3-HPM selectivity are shown in Table 1.
[0048] Comparative Example 4 The catalyst after the reaction in Comparative Example 3 was centrifuged and recovered, and the recovered catalyst was dissolved in 100 ml of methanol. The obtained catalyst was catalyzed again, and the catalytic process conditions were the same as those in Example 6. The EO conversion rate and 3-HPM selectivity are shown in Table 1.
[0049] Comparative Example 5 The catalyst after the reaction in Example 4 was centrifuged and recovered, and the recovered catalyst was dissolved in 100 ml of methanol. The obtained catalyst was catalyzed again, and the catalytic process conditions were the same as those in Example 6. The EO conversion rate and 3-HPM selectivity are shown in Table 1.
[0050] Comparative Example 6 The catalyst after the reaction in Example 5 was centrifuged and recovered, and the recovered catalyst was dissolved in 100 ml of methanol. The obtained catalyst was catalyzed again, and the catalytic process conditions were the same as those in Example 6. The EO conversion rate and 3-HPM selectivity are shown in Table 1.
[0051] Table 1 EO conversion and 3-HPM selectivity in Examples and Comparative Examples As can be seen from Table 1, the organic phosphine nitrogen porous polymers of Examples 1-2 can all show good 3-HPM selectivity in the EO hydrogenation reaction after loading metal Co, and the organic phosphine nitrogen porous polymer prepared by azobisisobutyronitrile initiator has a higher catalyst activity after loading metal Co. In Example 3, diphenyl (4-vinylphenyl) phosphine is replaced with tri (4-vinylphenyl) phosphine as a polymerization monomer to prepare an organic phosphine nitrogen porous polymer, and the obtained porous polymer has a large specific surface area. After loading metal Co, it can also show good 3-HPM selectivity and catalyst activity in the EO hydrogenation reaction. Example 4 replaces the metal salt cobalt acetate with cobalt hydroxide, and the result can also show good 3-HPM selectivity and catalyst activity in the EO hydrogenation reaction. Compared with Example 1, Example 5 reduces the temperature of the hot solvent polymerization method, and the 3-HPM selectivity and activity of the catalyst obtained are reduced to varying degrees. Examples 6-8 recover the catalyst after the reaction of Example 1 and reuse it. The catalyst activity of the EO hydrogenation reaction decreases slightly, but the selectivity remains stable ( Figure 2 ).
[0052] By comparing Comparative Examples 1-3 with Example 1, it can be seen that the catalysts obtained by using diphenyl (4-vinylphenyl) phosphine monomer alone and without adding coupling agent p-methylstyrene to obtain a large surface porous organic polymer and using aluminum oxide as an organic carrier to load metal Co all showed poor 3-HPM selectivity and catalyst activity in the EO hydroesterification reaction. Comparative Examples 4-6 recovered the catalyst after the reaction in Comparative Example 3 and reused it, and the EO hydroesterification catalyst activity and 3-HPM selectivity were significantly reduced ( Figure 3 ).
[0053] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A heterogeneous catalyst for EO hydroesterification, characterized in that: The catalyst consists of a metal component and an organic phosphine-nitrogen porous polymer; the metal component is one of cobalt and palladium, and the organic phosphine-nitrogen porous polymer is a porous organic polymer with a block structure obtained by solvent polymerization of an organic phosphine containing vinyl and phenyl, pyridine containing vinyl and p-methylstyrene.
2. The multiphase catalyst according to claim 1, characterized in that: The metal component accounts for 0.1-20.0% of the total weight of the heterogeneous catalyst.
3. The multiphase catalyst according to claim 1, characterized in that: The specific surface area of the organic phosphorus nitrogen porous polymer is 600-1200 m 2 / g, pore volume 0.1-5.0 cm 3 / g, and the pore size distribution is 0.1-200 nm.
4. A method for preparing a heterogeneous catalyst as claimed in claim 1, characterized in that: The steps include: (1) Adding a solvent and a free radical initiator to an organic phosphine containing vinyl and phenyl groups, pyridine containing vinyl groups and p-methylstyrene, and stirring at room temperature for 1-5 hours to form a prepolymer solution; (2) pouring the prepolymer solution of step (1) into a hydrothermal autoclave, performing a hot melt polymerization reaction at 100-150°C for 2-25 h, cooling to room temperature and filtering, soaking in anhydrous ethanol, washing, filtering, and drying at 50°C for 5 h to obtain an organic phosphine nitrogen porous polymer; (3) Dissolve the metal component precursor in a solvent to obtain a solution containing the metal component, add the organic phosphorus nitrogen porous polymer, stir at room temperature for 0.5-20 h, raise the temperature to 50-80 ° C and continue stirring for 0.5-20 h, cool to room temperature and filter, and dry at 50 ° C for 5 h to obtain a multiphase catalyst of the organic phosphorus nitrogen porous polymer loaded with metal active components.
5. The preparation method according to claim 4, characterized in that: The molar ratio of the organic phosphine containing vinyl and phenyl groups, the pyridine containing vinyl groups and p-methylstyrene used in step (1) is 1:(0.5-5):(0.5-2); the free radical initiator is one of dibenzoyl peroxide and azobisisobutyronitrile; the ratio of the amount of the free radical initiator to the total weight of the organic phosphine containing vinyl and phenyl groups, the pyridine containing vinyl groups and p-methylstyrene is 1:1000-1:
10.
6. The preparation method according to claim 4, characterized in that: The solvent in step (1) is one or more of benzene, toluene, tetrahydrofuran, methanol, ethanol, methyl acetate, and methyl tert-butyl ether.
7. The preparation method according to claim 4, characterized in that: In step (3), the metal component precursor is one or more of Co(NO3)2, CoCl2, Co(OAc)2, Co(acac)2, Co(OH)2, PdCl2, Pd(NO3)2, H2PdCl4, Pd(OAc)2; the solvent is one or more of methanol, ethanol, methyl acetate, and methyl tert-butyl ether.
8. Use of the heterogeneous catalyst according to claim 1 in EO hydroesterification reaction, characterized in that: Under the conditions of the heterogeneous catalyst, ethylene oxide, carbon monoxide and methanol are subjected to a hydroesterification reaction in a tank reactor, the reaction temperature is 30-100°C, the reaction pressure is 0.1-10.0 MPa, the reaction time is 3-25 h, the molar ratio of ethylene oxide to the metal component in the heterogeneous catalyst is 20-200:1; the weight proportion of the metal component in the reaction system is 0.2 wt%-0.5 wt%.
Citation Information
Patent Citations
Prepn process of 3-hydroxy propionate and propylene glycol
CN101020635A
Polymer-supported transition metal catalyst complexes and their application methods
CN102281948A
Methods for synthesizing 3-hydroxypropionate
CN106431926B
Polyvinyl-imidazole-supported cobalt carbonyl catalyst, preparation method and application of catalyst
CN107349962A
Method for preparing methyl 3-hydroxypropionate from ethylene oxide
CN107417527A