Preparation method of composite bipolar membrane with interlocking structure
The bipolar membrane is prepared by combining casting method and spraying method to form a cation and anion exchange layer with an interlocking structure, which solves the problem of insufficient bonding tightness of bipolar membranes in the prior art, improves the electrodialysis efficiency and stability, and realizes the Lower resistance and energy consumption.
Patent Information
- Application Number
- CN202411203855.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, there are few reports on the preparation of bipolar membranes in combination with spraying and casting methods, and the binding tightness and stability of the anion exchange layer and cation exchange layer of the bipolar membrane are insufficient, which affects the efficiency and stability of the electrodialysis process. sex.
The cation exchange layer was prepared by casting method and spraying method. The chloromethylated polysulfone anion exchange layer was prepared by quaternary amination treatment to form a bipolar film with interlocking structures. Combining the advantages of the two methods, the film layer thickness and resistance were regulated. Improve hydrolysis efficiency and operating stability.
The tight bonding of the bipolar membrane anion and cation exchange layer is achieved, reducing resistance and energy consumption, improving hydrolysis efficiency and operating stability, and enhancing the acid-base stability and current efficiency of the membrane.
Smart Images

Figure CN119034828A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of ion exchange membranes, and in particular is a method for preparing an interlocking structure composite bipolar membrane. Background Art
[0002] Bipolar membrane is a layered ion exchange membrane with a special structure. It consists of two layers of polymer layers with fixed opposite charges, one is a negatively charged cation exchange layer that allows anions to pass through, and the other is a positively charged anion exchange layer that allows cations to pass through, and an intermediate catalyst layer. Under positive pressure, ions in the main solution migrate into the membrane and combine at the interface layer to form water molecules. Under reverse bias, ions in the intermediate layer pass through the cation exchange layer and the anion exchange layer respectively, and migrate into the main solution under the drive of the electric field. When the ions in the membrane are exhausted, the water molecules in the intermediate layer are polarized and dissociated into hydrogen ions and hydroxide ions. Based on the characteristics of water generation under positive pressure and water dissociation under reverse pressure, bipolar membranes can be used in a variety of electrochemical applications, such as fuel cells, flow batteries, carbon dioxide reduction, water electrolysis to produce hydrogen, resource recovery, and acid-base production (Journal of Physical Chemistry, 1956, 60(4): 435–439).
[0003] The regulation of the bipolar membrane interface layer is mainly achieved by changing the type of intermediate catalyst and the construction method of the membrane layer. The main construction methods are spraying, casting, hot pressing, bonding, casting, electrodeposition, electrospinning, and the introduction of ion exchange groups on both sides of the base membrane. Among them, the spraying method is a common method for preparing bipolar membranes. This method uses a spray gun to disperse the solution into mist droplets under the action of electrostatic attraction, centrifugal force or gas pressure, spray the intermediate layer and the polymer solution with the opposite charge to the base membrane on the base membrane, and form a bipolar membrane after drying. The spraying film forming process is to atomize the material and distribute it on a certain cross section to form a liquid surface, and then form a solid surface through phase inversion or solvent volatilization. The atomization process can maintain uniform dispersion and produce an ultra-thin interface layer. The casting method is to dissolve the polymer in a solvent and cast it in a flat glass mold. After the solvent evaporates, it is peeled off to obtain a thin film. The membrane preparation process by spraying can help two substances with interactive forces to combine with each other to form a membrane, flexibly adjust the contact state of the two substances during film formation, control the film thickness by adjusting the concentration and number of spraying solvents, and shorten the film formation time to control the film thickness at the nanometer level.
[0004] However, there are relatively few reports on the preparation technology of bipolar membranes prepared by combining the spraying method with the tape casting method. The combination of the spraying method and the tape casting method has the advantages of a relatively simple preparation process and relatively more stable performance after the membrane is formed. In addition, the anion exchange layer and the cation exchange layer of the bipolar membrane are tightly combined and have good stability. The combination of the tape casting method and the spraying method can successfully prepare many bipolar membranes with excellent performance in the field of membrane preparation due to its energy saving, high efficiency, excellent membrane performance and large-area preparation. Summary of the invention
[0005] In order to solve the above technical problems existing in the prior art, the present invention provides an interlocking structure composite bipolar membrane and a preparation method thereof. First, the polymer (PAES-NH2) required for making the cation exchange layer and the polymer (CMPSF) required for the anion exchange layer are synthesized, and then the cation exchange layer is prepared by a casting method, and the anion exchange layer solution is sprayed by an automatic spraying device, and then the bipolar membrane is quaternized and dried to obtain a bipolar membrane with an anion and cation exchange layers having an interlocking structure. The specific technical scheme is as follows:
[0006] A method for preparing an interlocking structure composite bipolar membrane comprises the following steps:
[0007] Step (1): Preparation of amino-containing polyarylethersulfone
[0008] A certain amount of 4,4'-difluorodiphenyl sulfone monomer, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, hexafluorobisphenol A monomer and potassium carbonate are weighed and dissolved in a high boiling point polar aprotic solvent. Under nitrogen protection, at a certain reaction temperature and reaction time, the monomers are precipitated in the solvent after the reaction is completed. The monomers are vacuum dried at a certain temperature to obtain a polyarylethersulfone (PAES-NH2) containing amino groups in the main chain, whose chemical structure is shown in formula (I); in formula (I), x and y represent the molar percentages of two links, which are x% and y%, respectively, and x+y=100; wherein x=1-100, y=1-100; wherein the molar ratio of 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to hexafluorobisphenol A monomer is 1-80%:99-20%.
[0009]
[0010] Step (2): Preparation of sulfonated polyarylethersulfone
[0011] A certain amount of the amino-containing polyarylethersulfone (PAES-NH2) polymer obtained in step (1) is weighed, dissolved in a high-boiling point polar aprotic solvent at a certain temperature under nitrogen protection, a certain amount of 1,3-propanesultone is added as a sulfonating agent, and the reaction is carried out at a certain temperature and reaction time under nitrogen protection. After the reaction is completed, the polyarylethersulfone is precipitated in isopropanol, washed several times with isopropanol and deionized water, and dried under vacuum at a certain temperature to obtain a sulfonated polyarylethersulfone, a possible chemical structure of which is shown in formula (II);
[0012]
[0013] Step (3): Preparation of chloromethylated polysulfone
[0014] A certain amount of polysulfone is weighed and placed in a four-necked round-bottom flask equipped with a stirrer and a temperature controller, and the polysulfone is dissolved in a certain amount of chloroform. After the polysulfone is completely dissolved, paraformaldehyde, trimethylsilyl chloride and anhydrous tin tetrachloride are added to the above solution and mixed. Under nitrogen protection, the reaction is fully carried out at a certain reaction temperature and reaction time. After the reaction is completed, the reaction is filtered through a sand core funnel, poured into a large amount of ethanol for precipitation, and after being fully washed with deionized water, the chloromethylated polymer is vacuum dried at a certain temperature to obtain a chloromethylated polymer, whose chemical structure is shown in formula (III);
[0015]
[0016] Step (4): Preparation of cation exchange layer solution
[0017] A certain amount of sulfonated polyarylethersulfone polymer was weighed, added into a certain amount of solvent, stirred and dissolved at room temperature, and then filtered through a G3 sand core funnel to obtain a cation exchange layer solution with a certain mass fraction (wt%).
[0018] Step (5): Preparation of anion exchange layer solution
[0019] A certain amount of chloromethylated polysulfone was weighed, added into a certain amount of solvent, stirred and dissolved at room temperature, and then filtered through a G3 sand core funnel to obtain an anion exchange layer solution with a certain mass fraction (wt%).
[0020] Step (6): Preparation of bipolar membrane
[0021] The cation exchange layer solution prepared in step (4) is cast on a clean glass mold, placed in a vacuum oven at a suitable temperature and dried for a period of time to obtain a cation exchange layer; a certain mass fraction of the anion exchange layer solution prepared in step (5) is injected through a gas-tight syringe, a suitable distance is set between the nozzle and the glass plate, a certain amount of the cation exchange layer spray solution is sprayed at a single time at a certain spraying rate, atomized under the action of ultrasound to generate nano-scale droplets, sprayed several layers, and the solvent is dried to obtain a bipolar membrane, which is quaternized and placed in a vacuum oven at a suitable temperature and dried for a period of time to obtain a bipolar membrane with an interlocking structure.
[0022] Preferably, the reaction temperature in step (1) is 100-180° C., the reaction time is 3-24 hours, the high boiling point polar aprotic solvent can be N-methylpyrrolidone, and the solvent for precipitation can be isopropanol.
[0023] Preferably, the amount of the polyarylethersulfone described in step (2) is 1 to 3 g, the amount of the solvent is 15 to 40 mL, the amount of 1,3-propanesultone is 2 to 4 mL, the high boiling point polar aprotic solvent can be selected from N-methylpyrrolidone, the dissolution temperature is 40 to 60° C., the reaction time is 9 to 18 h, the vacuum drying temperature is 60 to 80° C., and the vacuum drying time is 18 to 24 h.
[0024] Preferably, in step (3), the amount of polysulfone is 8 to 12 g, the amount of chloroform is 450 to 500 mL, the amount of paraformaldehyde is 12 to 15 g, the amount of trimethylchlorosilane is 55 to 60 mL, the amount of anhydrous tin tetrachloride is 0.2 to 0.6 mL, the reaction temperature can be 40 to 60° C., the reaction time can be 40 to 70 h, the vacuum drying temperature is 50 to 70° C., and the vacuum drying time is 18 to 24 h.
[0025] Preferably, the amount of the sulfonated polyarylethersulfone in step (4) is 2-4 g, the amount of the solvent is 20-50 mL, and the solvent can be N-methylpyrrolidone.
[0026] Preferably, the amount of the chloromethylated polysulfone in step (5) is 2-6 g, the amount of the solvent is 30-60 mL, and the solvent can be dimethyl sulfoxide.
[0027] Preferably, the mass fraction (wt) of the anion exchange layer spraying solution described in step (6) is 2-8%, the distance between the nozzle and the glass mold is 4-15 cm, the liquid feeding rate of the gas-tight syringe is 200-400 μL / min, the amount of a single spraying is 150-260 μL, the number of spraying cycles is 3-8 times, the quaternary amination agent can be selected from trimethylamine, the temperature of the vacuum oven can be set to 60-80° C., and the vacuum drying time is 12-24 h.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention uses a tape casting method to prepare a sulfonated poly(arylethersulfone) cation exchange layer and a spray coating method to prepare a chloromethylated polysulfone anion exchange layer, and the two form an interlocking structure, so that the anion and cation exchange layers of the bipolar membrane are more closely combined, and the anion and cation layers are not easy to be separated during the bipolar membrane electrodialysis process.
[0030] (2) The use of the spraying method to prepare the bipolar membrane can easily adjust the concentration and number of spraying solvents to control the membrane thickness, shorten the film formation time to control the membrane thickness and reduce the bipolar membrane thickness, thereby reducing the resistance and energy consumption of the bipolar membrane and improving the hydrolysis efficiency and operating stability of the bipolar membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a possible structural schematic diagram of the interlocking structure composite bipolar membrane of the present invention.
[0032] Figure 2 It is a schematic flow chart of the method for preparing the interlocking structure composite bipolar membrane of the present invention.
[0033] Figure 3 It is a schematic diagram of the structure of each membrane layer of the interlocking structure composite bipolar membrane of the present invention. DETAILED DESCRIPTION
[0034] To further illustrate the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific examples, but it should be understood that these descriptions are only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention.
[0035] Embodiment 1:
[0036] (1) Preparation of amino-containing polyarylethersulfone:
[0037] Weigh 5.09g (20.00mmol) of 4,4'-difluorodiphenyl sulfone monomer, 4.39g (12.00mmol) of 2,2'-bis (3-amino 4-hydroxyphenyl) hexafluoropropane monomer and 2.69g (8.00mmol) of hexafluorobisphenol A, add 60mL of NMP to a 250mL round-bottom flask equipped with a water separator, and add 5.54g of K2CO3 as a salt-forming agent and 40mL of toluene as a water-carrying agent under nitrogen protection, react at 145℃ for 4h, and heat to 165℃ for 3h. When the solution cools to room temperature, pour it into 400mL of isopropanol, stir at high speed, and flocculate to obtain a precipitate. After separation by suction filtration, a brown solid is obtained, which is repeatedly washed with isopropanol and water for many times, and vacuum dried at 70℃ for 24h to obtain 12.18g of amino-containing polyarylethersulfone (PAES-NH2), with a molecular weight of 56000.
[0038] (2) Preparation of sulfonated polyarylethersulfone:
[0039] Weigh 2.5 g of PAES-NH2 prepared in step (1) and place it in a three-necked flask, add 35 mL of NMP, set the oil bath temperature to 50 ° C and dissolve it under nitrogen protection, after the polymer is fully dissolved, add 3.85 g of 1,3-propanesultone, set the temperature to 70 ° C, stir and react for 13 hours, cool to room temperature, and precipitate in isopropanol to obtain a white tough precipitate. After washing with deionized water several times, vacuum dry at 80 ° C for 24 hours to obtain 3.06 g of sulfonated polyarylethersulfone.
[0040] (3) Preparation of chloromethylated polysulfone:
[0041] Weigh 10 g of polysulfone into a four-necked round-bottom flask equipped with a stirrer and a temperature controller, dissolve it in 500 mL of chloroform at room temperature, and after it is completely dissolved, add 13.58 g of paraformaldehyde, 57.38 mL of trimethylsilyl chloride and 0.54 mL of anhydrous tin tetrachloride to the above solution and mix. Under N2 protection, stir and react at 50 ° C for 60 h. After the reaction, a light yellow solution is formed. The solution is filtered through a sand core funnel and poured into 700 mL of ethanol for precipitation. 18.23 g of a white product is precipitated, which is chloromethylated polysulfone. After being fully washed with deionized water, it is vacuum dried at 60 ° C for 24 h to obtain chloromethylated polysulfone.
[0042] (4) Preparation of cation exchange layer solution:
[0043] 1 g of sulfonated poly(arylethersulfone) was weighed and added to 15 mL of N-methylpyrrolidone. After dissolving at room temperature, the solution was filtered through a G3 sand core funnel to obtain a 6.08 wt % cation exchange layer solution.
[0044] (5) Preparation of anion exchange layer spray solution:
[0045] 1 g of chloromethylated polysulfone was weighed and dissolved in a three-necked flask containing 40 mL of dimethyl sulfoxide. After dissolving at room temperature to form a clear and transparent solution, the solution was filtered through a G3 sand core funnel to obtain a 2.20 wt% anion exchange layer spray solution.
[0046] (6) Preparation of bipolar membrane:
[0047] The cation exchange layer solution prepared in step (4) is cast on a clean glass mold, placed in a vacuum oven at 60°C for 10 hours to obtain a cation exchange layer; the 2.20wt% anion exchange layer solution prepared in step (5) is injected through a gas-tight syringe, 10 cm is set between the nozzle and the glass plate, 200μL of the anion exchange layer spray solution is sprayed at a spray rate of 200μL / min, atomized under ultrasonic action to generate nano-scale droplets, sprayed 2 layers, placed in a vacuum oven at 60°C for 20 hours to obtain a bipolar membrane, immersed in a 1.6wt% trimethylamine solution at 60°C for 10 hours for quaternization treatment, placed in a vacuum oven set at 60°C for 20 hours to obtain an interlocking structure bipolar membrane, whose possible structure is as follows Figure 1 shown.
[0048] The bipolar membrane was immersed in a 0.5 mol / L NaCl solution for 24 hours and then the I–V curve and acid-base production were measured. The bipolar membrane prepared in Example 1 was measured to have a thickness of 141 μm and a surface resistance of 2.87 Ω·cm 2 ; Water absorption rate is 14.3%; Swelling rate is 8.8%; Weight loss of acid-base stability is 3.17%; IEC loss of acid-base stability is 2.79%; Transmembrane voltage is 1.15V; Acid-base conversion rate is 96.2%; Current efficiency is 93.4%; Burst strength is 13.06kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577 (2019) 153–164; Journal of Materials Chemistry A 9 (2021) 5485–5496).
[0049] Embodiment 2:
[0050] (1) The preparation of amino-containing polyarylethersulfone is consistent with that in Example 1.
[0051] (2) The preparation of sulfonated poly(arylethersulfone) is consistent with that in Example 1.
[0052] (3) The preparation of chloromethylated polysulfone is consistent with that in Example 1.
[0053] (4) The preparation of the cation exchange layer is consistent with that in Example 1.
[0054] (5) Preparation of anion exchange layer solution:
[0055] 1.5 g of chloromethylated polysulfone was weighed and dissolved in a three-necked flask containing 40 mL of dimethyl sulfoxide. After dissolving at room temperature to form a clear and transparent solution, it was filtered through a G3 sand core funnel to obtain a 3.30 wt% anion exchange layer spray solution.
[0056] (6) Preparation of bipolar membrane:
[0057] The cation exchange layer solution prepared in step (4) is cast on a clean glass mold, placed in a vacuum oven at 60°C for 10 hours to obtain a cation exchange layer; the 3.30wt% anion exchange layer solution prepared in step (5) is injected through a gas-tight syringe, 10 cm is set between the nozzle and the glass plate, 200μL of the anion exchange layer spray solution is sprayed at a spray rate of 200μL / min, atomized under ultrasonic action to generate nanometer-sized droplets, sprayed 2 layers, placed in a vacuum oven at 60°C for 20 hours to obtain a bipolar membrane, immersed in a 1.6wt% trimethylamine solution at 60°C for 10 hours for quaternization treatment, placed in a vacuum oven set at 60°C for 20 hours to obtain a bipolar membrane with an interlocking structure.
[0058] The bipolar membrane was immersed in a 0.5 mol / L NaCl solution for 24 hours and then the I–V curve and acid-base production were measured. The bipolar membrane prepared in Example 2 was measured to have a thickness of 148 μm and a surface resistance of 3.38 Ω·cm 2 ; Water absorption rate is 17.8%; Swelling rate is 11.8%; Weight loss of acid-base stability is 5.34%; IEC loss of acid-base stability is 4.71%; Transmembrane voltage is 1.40V; Acid-base conversion rate is 92.8%; Current efficiency is 89.5%; Burst strength is 11.46kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577 (2019) 153–164; Journal of Materials Chemistry A 9 (2021) 5485–5496).
[0059] Embodiment 3:
[0060] (1) The preparation of amino-containing polyarylethersulfone is consistent with that in Example 1.
[0061] (2) The preparation of sulfonated poly(arylethersulfone) is consistent with that in Example 1.
[0062] (3) The preparation of chloromethylated polysulfone is consistent with that in Example 1.
[0063] (4) The preparation of the cation exchange layer is consistent with that in Example 1.
[0064] (5) Preparation of anion exchange layer solution:
[0065] 2 g of chloromethylated polysulfone was weighed and dissolved in a three-necked flask containing 40 mL of dimethyl sulfoxide. After dissolving at room temperature to form a clear and transparent solution, the solution was filtered through a G3 sand core funnel to obtain a 4.35 wt% anion exchange layer spray solution.
[0066] (6) Preparation of bipolar membrane:
[0067] The cation exchange layer solution prepared in step (4) is cast on a clean glass mold, placed in a vacuum oven at 60°C for 10 hours to obtain a cation exchange layer; the 4.35wt% anion exchange layer solution prepared in step (5) is injected through a gas-tight syringe, 10 cm is set between the nozzle and the glass plate, 200μL of the anion exchange layer spray solution is sprayed at a spray rate of 200μL / min, atomized under ultrasonic action to generate nanometer-sized droplets, sprayed 2 layers, placed in a vacuum oven at 60°C for 20 hours to obtain a bipolar membrane, immersed in a 1.6wt% trimethylamine solution at 60°C for 10 hours for quaternization treatment, placed in a vacuum oven set at 60°C for 20 hours to obtain a bipolar membrane with an interlocking structure.
[0068] The bipolar membrane was immersed in a 0.5 mol / L NaCl solution for 24 hours and then the I–V curve and acid-base production were measured. The bipolar membrane prepared in Example 3 was measured to have a thickness of 151 μm and a surface resistance of 3.47 Ω·cm 2 ; water absorption rate is 16.9%; swelling rate is 10.1%; weight loss of acid-base stability is 4.86%; IEC loss of acid-base stability is 3.11%; transmembrane voltage is 1.31V; acid-base conversion rate is 93.4%; current efficiency is 90.7%; burst strength is 12.16kg·cm –2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577 (2019) 153–164; Journal of Materials Chemistry A 9 (2021) 5485–5496).
[0069] Embodiment 4:
[0070] (1) The preparation of amino-containing polyarylethersulfone is consistent with that in Example 1.
[0071] (2) The preparation of sulfonated poly(arylethersulfone) is consistent with that in Example 1.
[0072] (3) The preparation of chloromethylated polysulfone is consistent with that in Example 1.
[0073] (4) The preparation of the cation exchange layer is consistent with that in Example 1.
[0074] (5) Preparation of anion exchange layer solution:
[0075] 1.2 g of chloromethylated polysulfone was weighed and dissolved in a three-necked flask containing 40 mL of dimethyl sulfoxide. After dissolving at room temperature to form a clear and transparent solution, the solution was filtered through a G3 sand core funnel to obtain a 2.65 wt% anion exchange layer spray solution.
[0076] (6) Preparation of bipolar membrane:
[0077] The cation exchange layer solution prepared in step (4) is cast on a clean glass mold, placed in a vacuum oven at 60°C for 10 hours to obtain a cation exchange layer; the 2.65wt% anion exchange layer solution prepared in step (5) is injected through a gas-tight syringe, 10 cm is set between the nozzle and the glass plate, 200μL of the anion exchange layer spray solution is sprayed at a spray rate of 200μL / min, atomized under ultrasonic action to generate nanometer-sized droplets, sprayed 2 layers, placed in a vacuum oven at 60°C for 20 hours to obtain a bipolar membrane, immersed in a 1.6wt% trimethylamine solution at 60°C for 10 hours for quaternization treatment, placed in a vacuum oven set at 60°C for 20 hours to obtain a bipolar membrane with an interlocking structure.
[0078] The bipolar membrane was immersed in a 0.5 mol / L NaCl solution for 24 hours and then the I–V curve and acid-base production were measured. The bipolar membrane prepared in Example 4 was measured to have a thickness of 146 μm and a surface resistance of 3.27 Ω·cm 2 ; Water absorption rate is 15.4%; Swelling rate is 9.8%; Weight loss of acid-base stability is 3.42%; IEC loss of acid-base stability is 2.82%; Transmembrane voltage is 1.26V; Acid-base conversion rate is 94.6%; Current efficiency is 91.6%; Burst strength is 12.67kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577 (2019) 153–164; Journal of Materials Chemistry A 9 (2021) 5485–5496).
[0079] Embodiment 5:
[0080] Similar to Example 4, except that in step (5), 3 layers of 200 μL of 2.44 wt % anion exchange layer spray solution are sprayed.
[0081] The bipolar membrane was immersed in a 0.5 mol / L NaCl solution for 24 hours and then the I–V curve and acid-base production were measured. The bipolar membrane prepared in Example 5 was measured to have a thickness of 144 μm and a surface resistance of 3.12 Ω·cm 2 ; Water absorption rate is 14.8%; Swelling rate is 9.1%; Weight loss of acid-base stability is 3.31%; IEC loss of acid-base stability is 2.41%; Transmembrane voltage is 1.21V; Acid-base conversion rate is 95.2%; Current efficiency is 92.4%; Burst strength is 12.95kg·cm -2(For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577 (2019) 153–164; Journal of Materials Chemistry A 9 (2021) 5485–5496).
[0082] Embodiment 6:
[0083] Similar to the embodiment, the difference is that in step (5), 3 layers of 200 μL of 2.0 wt % anion exchange layer spray solution are sprayed.
[0084] The bipolar membrane was immersed in a 0.5 mol / L NaCl solution for 24 hours and then the I–V curve and acid-base production were measured. The thickness of the bipolar membrane prepared in Example 6 was 139 μm and the surface resistance was 2.52 Ω·cm 2 ; Water absorption rate is 13.3%; Swelling rate is 8.1%; Weight loss of acid-base stability is 3.08%; IEC loss of acid-base stability is 2.69%; Transmembrane voltage is 1.01V; Acid-base conversion rate is 96.3%; Current efficiency is 93.7%; Burst strength is 13.41kg·cm -2 (For specific testing methods, please refer to the literature reports: Journal of Membrane Science 577 (2019) 153–164; Journal of Materials Chemistry A 9 (2021) 5485–5496).
[0085]
[0086] Table 1 Performance test data of interlocking structure composite bipolar membranes of various embodiments.
Claims
1. A method for preparing an interlocking structure composite bipolar membrane, comprising the following steps: Step (1): Preparation of amino-containing polyarylethersulfone A certain amount of 4,4'-difluorodiphenyl sulfone monomer, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, hexafluorobisphenol A monomer and potassium carbonate are weighed and dissolved in a high boiling point polar aprotic solvent. Under nitrogen protection, at a certain reaction temperature and reaction time, the reaction is precipitated in the solvent after the reaction is completed, and vacuum dried at a certain temperature to obtain a polyarylethersulfone containing amino groups in the main chain, whose chemical structure is shown in formula (I); in formula (I), x and y represent the molar percentages of two links, which are x% and y%, respectively, and x+y=100; wherein x=1-100, y=1-100; wherein the feeding molar ratio of 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and hexafluorobisphenol A monomer is 1-80%:99-20%. Step (2): Preparation of sulfonated polyarylethersulfone A certain amount of the amino-containing polyarylethersulfone (PAES-NH2) polymer obtained in step (1) is weighed and dissolved in a high-boiling point polar aprotic solvent at a certain temperature under nitrogen protection, a certain amount of 1,3-propanesultone is added as a sulfonating agent, and the reaction is carried out at a certain temperature and reaction time under nitrogen protection. After the reaction is completed, the polyarylethersulfone is precipitated in isopropanol, washed several times with isopropanol and deionized water, and dried under vacuum at a certain temperature to obtain a sulfonated polyarylethersulfone, a possible chemical structure of which is shown in formula (II): Step (3): Preparation of chloromethylated polysulfone A certain amount of polysulfone is weighed and placed in a four-necked round-bottom flask equipped with a stirrer and a temperature controller, and the polysulfone is dissolved in a certain amount of chloroform. After complete dissolution, paraformaldehyde, trimethylsilyl chloride and anhydrous tin tetrachloride are added to the above solution and mixed. Under nitrogen protection, the reaction is fully carried out at a certain reaction temperature and reaction time. After the reaction is completed, it is filtered through a sand core funnel, poured into a large amount of ethanol for precipitation, and after being fully washed with deionized water, it is vacuum dried at a certain temperature to obtain a chloromethylated polymer, and its chemical structure is shown in formula (III): Step (4): Preparation of cation exchange layer solution Weigh a certain amount of sulfonated polyarylethersulfone polymer, add it to a certain amount of solvent, stir and dissolve it at room temperature, and then filter it through a G3 sand core funnel to obtain a cation exchange layer solution with a certain mass fraction; Step (5): Preparation of anion exchange layer solution Weigh a certain amount of chloromethylated polysulfone, add it to a certain amount of solvent, stir and dissolve it at room temperature, and then filter it through a G3 sand core funnel to obtain an anion exchange layer solution with a certain mass fraction; Step (6): Preparation of bipolar membrane The cation exchange layer solution prepared in step (4) is cast on a clean glass mold, placed in a vacuum oven at a suitable temperature and dried for a period of time to obtain a cation exchange layer; a certain mass fraction of the anion exchange layer solution prepared in step (5) is injected through a gas-tight syringe, a suitable distance is set between the nozzle and the glass plate, and a certain amount of the cation exchange layer spray solution is sprayed at a single time at a certain spraying rate, atomized under the action of ultrasound to generate nano-scale droplets, sprayed several layers, and the solvent is dried to obtain a bipolar membrane, which is quaternized and placed in a vacuum oven at a suitable temperature and dried for a period of time to obtain an interlocking structure bipolar membrane, as shown in Figure 1.
2. The method for preparing the interlocking structure composite bipolar membrane according to claim 1, characterized in that: The reaction temperature in step (1) is 100-180° C., the reaction time is 3-24 hours, the high boiling point polar aprotic solvent can be N-methylpyrrolidone, and the solvent for precipitation can be isopropanol.
3. The method for preparing the interlocking structure composite bipolar membrane according to claim 1, characterized in that: The amount of the polyarylethersulfone described in step (2) is 1 to 3 g, the amount of the solvent is 15 to 40 mL, the amount of 1,3-propanesultone is 2 to 4 mL, the high boiling point polar aprotic solvent can be selected from N-methylpyrrolidone, the dissolution temperature is 40 to 60 ° C, the reaction time is 9 to 18 h, the vacuum drying temperature is 60 to 80 ° C, and the vacuum drying time is 18 to 24 h.
4. The method for preparing the interlocking structure composite bipolar membrane according to claim 1, characterized in that: In step (3), the amount of polysulfone is 8-12 g, the amount of chloroform is 450-500 mL, the amount of paraformaldehyde is 12-15 g, the amount of trimethylchlorosilane is 55-60 mL, the amount of anhydrous tin tetrachloride is 0.2-0.6 mL, the reaction temperature can be 40-60° C., the reaction time can be 40-70 h, the vacuum drying temperature is 50-70° C., and the vacuum drying time is 18-24 h.
5. The method for preparing the interlocking structure composite bipolar membrane according to claim 1, characterized in that: The amount of the sulfonated polyarylethersulfone described in step (4) is 2-4 g, and the amount of the solvent is 20-50 mL, and the solvent can be N-methylpyrrolidone.
6. The method for preparing the interlocking structure composite bipolar membrane according to claim 1, characterized in that: The amount of the chloromethylated polysulfone described in step (5) is 2-6 g, and the amount of the solvent is 30-60 mL, and the solvent can be dimethyl sulfoxide.
7. The method for preparing the interlocking structure composite bipolar membrane according to claim 1, characterized in that: The mass fraction of the anion exchange layer spraying solution described in step (6) is 2-8%, the distance between the nozzle and the glass mold is 4-15 cm, the liquid feeding rate of the airtight syringe is 200-400 μL / min, the amount of a single spraying is 150-260 μL, the number of spraying cycles is 3-8 times, the quaternary amination agent can be selected from trimethylamine, the temperature of the vacuum oven can be set to 60-80° C., and the vacuum drying time is 12-24 h.
Citation Information
Cited By
Bipolar membrane and preparation method thereof
CN120550646A