Production method of 500MPa high-strength and high-toughness crescent rib anchor rod steel
By adopting low S/P and low O billet components and full-process constant temperature rolling technology in anchor steel production, combined with cold bed insulation and microtension control, the strength and toughness of anchor steel in high-deep wells are solved. The problem of this problem is to achieve the production of 500MPa crescent rib anchor steel with high strength, high toughness and high impact resistance, improving the safety of coal mine tunnel support.
Patent Information
- Application Number
- CN202411167876.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing 500MPa grade anchor steel is difficult to meet the requirements of high strength, high toughness and high impact pressure in high-deep well coal mines. It is easy to produce harmful tissue and crack defects in conventional processes, resulting in the mechanical properties not meeting the standards and poses safety hazards.
Using low S/P and low O billet components, combined with the full-process constant temperature rolling, controlled rolling and cold-bed insulation technology, the full-line microtension, precise control of the lid sleeve and K1-K3 full-rolling guide technology are used to carry out Smelting and electromagnetic stirring treatment ensure high purity and uniformity of the billet, control the opening rolling, controlled rolling and controlled cooling temperatures within the range of 950-1000℃, and use tungsten carbide rolls and cold bed insulation covers to improve the impact toughness and size of the steel stability.
500MPa high-strength, high-tough crescent rib anchor steel was produced, with a normal temperature impact force of more than 130J, an elongation after breaking reached more than 28%, a tensile strength of more than 710MPa, and a yield strength of more than 530MPa, which meets the high strength of a kilometer-deep well coal mine and High toughness requirements improve the safety of downhole tunnel support.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rolling composite, and in particular to a production method of 500MPa high-strength and high-toughness crescent-rib anchor steel. Background Art
[0002] With the rapid development of the coal industry and the continuous strengthening of safety management, anchor steel support, as a relatively safe and economical form of coal mine support, has gradually been accepted and promoted by various coal mines and has become the primary material for coal mine support. With the continuous excavation of coal seams, coal mine tunnels are getting deeper and deeper, and thousand-meter deep coal mines have put forward requirements for anchor steel with high strength, high toughness and high impact ground pressure resistance. From the standard YB / T 4364-2014 "Hot-rolled ribbed steel bars for anchor rods", it can be seen that the mechanical properties requirements of MG500 grade anchor steel are: yield strength not less than 500Mpa, tensile strength not less than 630Mpa, elongation after fracture not less than 20%, impact absorption energy (KV 2 ) is not less than 40J (test temperature 20℃). However, in actual application, with the increase of mining depth, the requirements for MG500 grade anchor steel are more stringent. The mechanical properties only meet the standards and cannot meet the requirements of high strength, high toughness and high impact pressure resistance.
[0003] MG500-grade anchor products produced by conventional hot rolling technology are very likely to produce harmful structures such as Widmanstatten structure + network cementite, bainite structure, etc. due to the composition of the steel billet and the control of the starting rolling temperature, controlled rolling and controlled cooling temperature. MG500-grade anchor steel is prone to crack defects during secondary reduction + thread rolling processing, and its impact performance, toughness and strength are greatly reduced. It is difficult to meet the standards for various mechanical properties at the same time, posing certain safety hazards to underground tunnel support. Summary of the invention
[0004] In view of the technical problem that it is difficult for 500MPa grade anchor steel in the prior art to simultaneously meet the requirements of high strength, high toughness and high impact ground pressure resistance, the present invention provides a method for producing 500MPa high-strength and high-toughness crescent-rib anchor steel, whose room-temperature impact energy, elongation after fracture, tensile strength and yield strength are significantly better than those of standard YB / T 4364-2014 "Hot-rolled ribbed steel bars for anchor rods", and can be used in kilometer-deep coal mines.
[0005] The technical solution of the present invention is as follows: A production method of 500MPa high-strength and high-toughness crescent rib anchor steel, when the steel billet is heated and rolled in a heating furnace, it successively enters the roughing and intermediate rolling, pre-finishing rolling and finishing rolling areas, and is controlled to cool after rolling; the start rolling temperature, the controlled rolling temperature and the controlled cooling temperature are all controlled within the temperature range of 950-1000°C; after rolling, the steel billet is put on a cooling bed, the temperature of the cooling bed is consistent with the start rolling temperature, an insulation cover is arranged at the inlet side of the cooling bed, the cooling bed is insulated by the insulation cover, the insulation time is controlled within 2 minutes, and the temperature difference between the steel billet entering and leaving the insulation cover is controlled within 50°C; The steel billet is composed of the following elements by weight percentage: C 0.19%-0.25%, Si 0.40%-0.60%, Mn 1.30%-1.50%, S ≤0.03%, P ≤0.03%, V 0.060%-0.080%, O ≤0.005%, and the rest is Fe and unavoidable impurities.
[0006] Furthermore, when the steel billet is heated and rolled in the heating furnace, full-line micro-tension technology, looper precision control technology and K1-K3 full-rolling guide technology are used, providing equipment and technical guarantees for the stability of the entire length dimension.
[0007] Furthermore, the full-line micro-tension technology uses six vertical loopers to ensure that the full-line tension value is controlled at ≤1%.
[0008] Furthermore, the precise control technology of the looper is to control the looper height at 150-250mm, the looper starting time when the head bites in is ≤200ms, and the looper dropping time after the tail leaves the rolling mill is ≤300ms.
[0009] Furthermore, K1 and K2 use tungsten carbide rollers, which have good wear resistance and provide technical guarantee for the qualitative quality of the surface quality and size of the finished product.
[0010] Furthermore, the steel billet is smelted before being heated in a heating furnace for rolling.
[0011] Furthermore, the smelting of the steel billet includes LF refining, strong deoxidation, calcium wire feeding, soft argon blowing, full-process protection pouring, and electromagnetic stirring.
[0012] Calcium feeding wire can control the gas content and composition in molten steel, improve the purity and uniformity of molten steel, and improve the impact toughness of steel.
[0013] Furthermore, the amount of calcium wire added is 1.5-2m / t steel.
[0014] Furthermore, the current of the electromagnetic stirring was 200 A and the frequency was 4 Hz.
[0015] The beneficial effects of the present invention are: The present invention provides a production method of 500MPa high-strength and high-toughness crescent rib anchor steel. By combining low S / P and low O steel billet components, full-process constant temperature rolling + controlled rolling and controlled cooling with cooling bed insulation control, 500MPa high-strength and high-toughness crescent rib anchor steel for coal mine impact pressure resistance at a depth of one kilometer is produced. The steel has excellent full-length dimensional stability and mechanical properties, with an impact energy of more than 130J at room temperature, an elongation after fracture of more than 28%, a tensile strength of more than 710MPa, and a yield strength of more than 530MPa. DETAILED DESCRIPTION
[0016] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0017] Example 1 Rolling Φ18 specification 500MPa high strength and high toughness crescent rib anchor steel A method for producing 500MPa high-strength and high-toughness crescent-shaped rib anchor steel comprises the following steps: (1) Billet smelting: LF refining, strong deoxidation, calcium wire feeding, calcium wire addition amount is 1.5m / t steel, soft argon blowing, full protection pouring, electromagnetic stirring, electromagnetic stirring current is 200A, frequency is 4Hz, and billet is smelted; The steel billet is composed of the following elements by weight percentage: C 0.19%, Si 0.40%, Mn 1.30%, S 0.010%, P0.030%, V 0.060%, O 0.0030%, and the rest is Fe and inevitable impurities.
[0018] (2) Heating and rolling: The steel billet enters the steel rolling heating furnace for heating, and then enters the roughing and intermediate rolling, pre-finishing and finishing rolling areas. During heating, the whole-line micro-tension technology, looper precision control technology and K1-K3 full rolling guide technology are used. K1 and K2 use tungsten carbide rollers with good wear resistance, and controlled cooling is performed after rolling. The micro-tension technology of the whole line uses six vertical loopers to ensure that the tension value of the whole line is controlled at ≤1%; the precise control technology of the looper is to control the looper height at 150-250mm, the looper start time is ≤200ms when the head bites in, and the looper drop time is ≤300ms after the tail leaves the rolling mill; In this process, the technology of constant temperature rolling + controlled rolling and controlled cooling is adopted throughout the whole process, that is, the starting rolling temperature, controlled rolling temperature and controlled cooling temperature are all controlled at the same temperature, which is controlled at 950℃.
[0019] (3) Insulation of cooling bed: The temperature of the cooling bed on the steel billet is 950℃, and an insulation cover is set on the inlet side of the cooling bed (the insulation cover is the same length as the cooling bed, which is 108m, and the insulation cover is 2m wide). The cooling bed is insulated by the insulation cover, and the insulation time is controlled within 2min. The temperature difference of the steel billet entering and leaving the insulation cover is controlled within 50℃. Finally, Φ18 specification 500MPa high-strength and high-toughness crescent rib anchor steel is rolled.
[0020] After testing, the metallographic structure of the Φ18 specification 500MPa high-strength and high-toughness crescent rib anchor steel is ferrite + pearlite, the yield strength is 530MPa, the tensile strength is 750MPa, the yield strength ratio is 0.71, the elongation after fracture is 32%, and the impact energy (20℃) is 130J.
[0021] Example 2 Rolling Φ20 specification 500MPa high strength and high toughness crescent rib anchor steel The difference from Example 1 is that (1) the amount of calcium wire added during smelting the steel billet is 2 m / t steel, and the steel billet is composed of the following elements by weight percentage: C 0.20%, Si 0.60%, Mn 1.45%, S 0.025%, P 0.025%, V 0.072%, O 0.001%, and the rest is Fe and unavoidable impurities. (2) During hot rolling, the start rolling temperature, the controlled rolling temperature and the controlled cooling temperature are all controlled at the same temperature, which is 1000°C. (3) During the cooling bed insulation, the temperature of the cooling bed on the steel billet is 1000°C, and finally a Φ20 specification 500MPa high-strength and high-toughness crescent rib anchor steel is rolled out.
[0022] After testing, the metallographic structure of the Φ20 specification 500MPa high-strength and high-toughness crescent rib anchor steel is ferrite + pearlite, the yield strength is 540MPa, the tensile strength is 710MPa, the yield strength ratio is 0.76, the elongation after fracture is 28%, and the impact energy (20℃) is 140J.
[0023] Example 3 Rolling Φ22 specification 500MPa high strength and high toughness crescent rib anchor steel The difference from Example 1 is that (1) the steel billet is composed of the following elements by weight percentage: C 0.25%, Si 0.50%, Mn 1.5%, S 0.03%, P 0.015%, V 0.075%, O 0.003%, and the rest is Fe and inevitable impurities. (2) During hot rolling, the start rolling temperature, the controlled rolling temperature and the controlled cooling temperature are all controlled at the same temperature, which is 980°C. (3) During the cooling bed insulation, the temperature of the cooling bed on the steel billet is 980°C, and finally a Φ22 specification 500MPa high-strength and high-toughness crescent rib anchor steel is rolled out.
[0024] After testing, the metallographic structure of the Φ22 specification 500MPa high-strength and high-toughness crescent rib anchor steel is ferrite + pearlite, the yield strength is 575MPa, the tensile strength is 741MPa, the yield strength ratio is 0.78, the elongation after fracture is 31%, and the impact energy (20℃) is 135J.
[0025] Comparative Example 1 The difference from Example 1 is that (1) the steel billet in the smelted steel billet is composed of the following elements by weight percentage: C 0.19%, Si 0.40%, Mn 1.30%, S 0.060%, P 0.035%, V 0.075%, O 0.005%, and the rest is Fe and inevitable impurities. (2) During hot rolling, the starting rolling temperature is 950°C, the controlled rolling temperature is 1050°C, and the controlled cooling temperature is 920°C. (3) When the cooling bed is kept warm, the temperature of the cooling bed on the steel billet is 920°C.
[0026] After testing, the metallographic structure of the Φ18 specification 500MPa high-strength and high-toughness crescent rib anchor steel is ferrite + pearlite + bainite structure, the yield strength is 510MPa, the tensile strength is 635MPa, the elongation after fracture is 21%, and the impact energy (20℃) is 50J.
[0027] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.
Claims
1. A method for producing 500MPa high-strength and high-toughness crescent rib anchor steel, characterized in that: When the billet is heated and rolled in the heating furnace, it enters the roughing and intermediate rolling, pre-finishing and finishing rolling areas successively, and is cooled after rolling; the start rolling temperature, the controlled rolling temperature and the controlled cooling temperature are all controlled within the temperature range of 950-1000℃; after rolling, the billet is put on the cooling bed, and the temperature of the cooling bed is consistent with the start rolling temperature. A heat preservation cover is set at the inlet side of the cooling bed, and the heat preservation time is controlled within 2 minutes. The temperature difference of the billet entering and leaving the heat preservation cover is controlled within 50℃; The steel billet is composed of the following elements by weight percentage: C 0.19%-0.25%, Si 0.40%-0.60%, Mn 1.30%-1.50%, S ≤0.03%, P ≤0.03%, V 0.060%-0.080%, O≤0.005%, and the rest are Fe and inevitable impurities.
2. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 1, characterized in that: When the steel billet is heated and rolled in the heating furnace, the full-line micro-tension technology, looper precision control technology and K1-K3 full rolling guide technology are adopted.
3. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 2, characterized in that: The full-line micro-tension technology uses six vertical loopers to ensure that the full-line tension value is controlled at ≤1%.
4. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 2, characterized in that: The precise control technology of the looper is to control the looper height at 150-250mm, the looper starting time when the head bites in is ≤200ms, and the looper dropping time after the tail leaves the rolling mill is ≤300ms.
5. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 2, characterized in that: K1 and K2 use tungsten carbide rollers.
6. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 1, characterized in that: The steel billet is smelted before being heated in a heating furnace for rolling.
7. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 6, characterized in that: The smelting of steel billets includes LF refining, strong deoxidation, calcium wire feeding, soft argon blowing, full-process protection pouring, and electromagnetic stirring.
8. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 7, characterized in that: The amount of calcium wire added is 1.5-2m / t steel.
9. The method for producing a 500MPa high-strength and high-toughness crescent-rib anchor steel as claimed in claim 7, characterized in that: The current of electromagnetic stirring was 200A and the frequency was 4 Hz.
Citation Information
Patent Citations
High-toughness MG500 anchor rod reinforcing steel bar and production method thereof
CN106399848A
Production method of high-toughness MG500 hot rolled anchor rod reinforcing steel bars
CN109280755A
Special high-strength anti-seismic reinforcing steel bar for railway and production process thereof
CN114150223A
Hot rolling process method for equal-height rib right-handed rotation anchor rod steel bars
CN114160575A
Hot rolling process method of crescent rib left-handed anchor rod steel bar
CN114472512A