Preparation process of CLF steel rolled plate
Through the process routes of vacuum smelting, self-consumption remelting, forging, rolling and performance heat treatment, the problem of differences in mechanical properties of CLF-1 steel rolled plates is solved, and the grains are refined and the structural structure is optimized, which improves the overall mechanical properties of the material. , meets the requirements of nuclear fusion engineering.
Patent Information
- Application Number
- CN202411271436.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-29
AI Technical Summary
There are differences in mechanical properties of CLF-1 steel rolled plates, mainly due to the different microstructure and processing technology of the material, especially in the grain size and the width of the martensite slats, resulting in the yield strength of the rolled plates above 15mm and The impact performance is unstable and it is difficult to meet the strict requirements of future nuclear fusion engineering.
The process routes of vacuum smelting, self-consumption remelting, forging, rolling, performance heat treatment and machining are adopted to refine grains and promote the transformation of austenite to martensite by controlling temperature, rolling deformation and cooling methods. Avoid excessive phase change in grain size to ensure consistency and stability of material properties.
By refining the grains and optimizing the structure, the overall mechanical properties of the CLF-1 steel rolled plate are improved, the yield strength and tensile strength stability are ensured, and the strict requirements for steel materials in nuclear fusion engineering are met.
Smart Images

Figure BDA0005038832480000061 
Figure BDA0005038832480000071 
Figure BDA0005038832480000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal processing, in particular to a preparation process of a CLF steel rolled plate. Background Art
[0002] CLF-1 is mainly used as a component material for the International Thermonuclear Experimental Reactor (ITER) and other future fusion reactors. At present, the problems of CLF-1 steel rolled plates are mainly concentrated on the differences in mechanical properties, which are caused by differences in the microstructure of the material and the different processing techniques. From the perspective of composition and microstructure analysis, the differences in mechanical properties of CLF-1 steel rolled plates are due to the differences in grain size and martensite lath width; for rolled plates less than 15 mm, the performance indicators are relatively stable after heat treatment, and the yield strength indicators of rolled plates above 15 mm are significantly different, and there are also differences in grain size and impact indicators. Therefore, how to improve and optimize the preparation process of CLF-1 steel rolled plates, thereby improving the overall performance of CLF-1 steel, and thus meeting the strict requirements of future nuclear fusion projects for steel materials, is an urgent problem to be solved. Summary of the invention
[0003] This application adopts a preparation process of CLF steel rolled plate, and the process route is as follows:
[0004] Vacuum smelting → consumable remelting → forging → rolling → performance heat treatment → machining → acceptance.
[0005] To expand, the specific operations of the above-mentioned processes are:
[0006] Melting and consumable remelting are the same as CN108165884A.
[0007] During forging, forging heating is carried out according to the specifications of the steel ingot: when the raw material specifications are 260-750mm, the charging temperature is ≤700℃, the shortest heating time is 8-14h, the holding time at 850℃ is 2-4h, the heating temperature is 1200℃, and the holding time is 2-6h.
[0008] The specific specifications and processing technology are:
[0009] When the raw material specification is 260-360mm, the furnace temperature is ≤700℃, the shortest heating time is 8h, the holding time at 850℃ is 2h, the heating temperature is 1200℃, and the holding time is 2.5h;
[0010] When the raw material specification is 361-470mm, the furnace temperature is ≤650℃, the shortest heating time is 10h, the holding time at 850℃ is 2.5h, the heating temperature is 1200℃, and the holding time is 3.5h;
[0011] When the raw material specification is 471~590mm, the charging temperature is ≤650℃, the shortest heating time is 12h, the holding time at 850℃ is 3h, the heating temperature is 1200℃, and the holding time is 4.5h;
[0012] When the raw material specifications are 591-750mm, the charging temperature is ≤600℃, the shortest heating time is 14h, the insulation time at 850℃ is 3.5h, the heating temperature is 1200℃, and the insulation time is 5.5h.
[0013] During rolling, the billet is heated according to its specifications: the billet specifications are 40-200mm, the charging temperature is ≤550℃, the heating time is 120-220min, the heating temperature is 1150-1170℃, the minimum holding time is 50-100min, and the finishing temperature is 1040-1070℃.
[0014] The specific specifications and processing technology are:
[0015] The specifications of the rolled billet are 40-90 mm, the charging temperature is ≤550°C, the heating time is 120 min, the heating temperature is 1150°C, the minimum holding time is 60 min, and the finishing temperature is 1060°C;
[0016] The specifications of the rolled billet are 91-140mm, the charging temperature is ≤550℃, the heating time is 160min, the heating temperature is 1150℃, the minimum holding time is 75min, and the finishing temperature is 1060℃;
[0017] The specifications of the rolled billet are 141-200mm, the charging temperature is ≤550℃, the heating time is 200min, the heating temperature is 1150℃, the minimum holding time is 60min, and the finishing temperature is 1060℃.
[0018] During the performance heat treatment, quenching is carried out according to the specifications of the rolled plate: the holding temperature is 970-990°C, the rolled plate specification is <90mm, the shortest holding time is 50-180min, and the cooling method is water cooling.
[0019] The specific specifications and processing technology are:
[0020] The holding temperature is 970-990℃, the plate specification is ≤10mm, the shortest holding time is 50min, and the cooling method is water cooling;
[0021] The holding temperature is 970-990℃, the rolled plate specification is >10-35mm, the shortest holding time is 60min, and the cooling method is water cooling;
[0022] The holding temperature is 970-990℃, the rolled plate specification is >35-50mm, the shortest holding time is 85min, and the cooling method is water cooling;
[0023] The holding temperature is 970-990℃, the rolled plate specification is >50-85mm, the shortest holding time is 100min, and the cooling method is water cooling.
[0024] During the performance heat treatment, tempering is carried out according to the specifications of the rolled plate: the holding temperature is 730-750℃, the rolled plate specification is <90mm, the shortest holding time is 90-180min, and the cooling method is air cooling.
[0025] The specific specifications and processing technology are:
[0026] The holding temperature is 730-750℃, the plate specification is ≤10mm, the shortest holding time is 90min, and the cooling method is air cooling;
[0027] The holding temperature is 730-750℃, the rolled plate specification is >10-35mm, the shortest holding time is 120min, and the cooling method is air cooling;
[0028] The holding temperature is 730-750℃, the rolled plate specification is >35-50mm, the shortest holding time is 150min, and the cooling method is air cooling;
[0029] The holding temperature is 730-750℃, the rolled plate specification is >50-85mm, the shortest holding time is 180min, and the cooling method is air cooling.
[0030] In the present invention, forging blank annealing: annealing temperature is 740-800°C, and annealing holding time is calculated based on effective size 2.4min / 1mm+30min.
[0031] In the present invention, the final rolling temperature is controlled to be ≥850°C during rolling, and the rolling reduction is controlled to be ≥25% in at least one pass.
[0032] In the present invention, for products that need two-heat rolling, the finishing heating temperature is controlled at 1060° C., and the total deformation of the finishing rolling is ≥30%.
[0033] In the present invention, the annealing temperature is 730-760° C., and the shortest annealing holding time is calculated based on the thickness size of 2.4 min / 1 mm+20 min.
[0034] The beneficial effects achieved by the present invention are:
[0035] The preparation process of the CLF steel rolled plate provided by the present invention controls each process of the CLF steel rolled plate, thereby ensuring proper temperature control in the process, avoiding differences in organizational properties caused by uneven temperature, such as avoiding grain growth. The total deformation amount of rolling is used to achieve the purpose of grain refinement; by controlling the final rolling temperature, the austenite can be dynamically or statically recrystallized, thereby achieving the purpose of grain refinement. By air cooling after rolling, the diffusion time in the phase change process can be reduced, thereby refining the grains, and at the same time promoting the transformation of austenite to martensite, so as to prepare the organization for performance heat treatment after annealing. In addition, by controlling the quenching and holding time, the grain size growth is avoided, which leads to excessive phase change and makes the material brittle. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0037] Example 1
[0038] 1. Melting
[0039] 1.1 Melting method: vacuum induction furnace + consumable remelting (VIM + VAR). The electrode blank can also be prepared by electric furnace or induction furnace, and the consumable electrode can be remelted in the slag pool of the mold by using the resistance heat generated when the current passes through the slag layer. The method is the same as CN108165884A.
[0040] 1.2 Chemical components used for smelting, see Table 1.
[0041] Table 1
[0042] element Required value (wt%) Target value (wt%) Cr 8.2~8.8 8.5 C 0.085-0.135 1.1 W 1.3~1.7 1.5 Ta 0.05~0.15 1.0 Mn 0.3~0.7 0.5 V 0.2~0.4 0.3 N 0.015~0.040 0.03 O ≤0.01 ≤0.006 P ≤0.005 S ≤0.005 Ti ≤0.01 B ≤0.005 Al ≤0.03 Si ≤0.05 Nb ≤0.005 Mo ≤0.005 Ni ≤0.01 Cu ≤0.01 Co ≤0.01 Ag ≤0.005 As+Sn+Sb+Zr ≤0.005 Fe margin
[0043] 1.3 After the steel ingot is smelted and demoulded, it is annealed and heat treated.
[0044] 1.4 The surface of vacuum consumable steel ingots should be machined, and there should be no defects such as cracks, scars, spatter, pits, etc. visible to the naked eye.
[0045] 1.5 The chemical composition of the steel ingot shall meet the requirements of Table 1 after retesting.
[0046] 1.6 The shrinkage compensation of steel ingot is good; the surface quality of steel ingot meets the relevant requirements of 1.4.
[0047] 2. Forging
[0048] 2.1 Forging Heating
[0049] 2.1.1 During the heating process, the furnace door and all parts should be in a well-closed state, and the positive air pressure in the furnace should be maintained.
[0050] 2.1.2 The flame is not allowed to be sprayed directly onto the surface of steel ingots or billets.
[0051] 2.1.3 The operating parameters of various ingot specifications during forging heating are shown in Table 2.
[0052] Table 2
[0053]
[0054] Note: Before 850℃, control the heating rate to ≤60℃ / h.
[0055] 2.2 Forging
[0056] 2.2.1 First of all, we must look carefully at the forging production flow card and process diagram, and accurately grasp the brand, specifications and process requirements of the production on that shift.
[0057] 2.2.2 Carefully check whether the equipment of the unit is normal. If the equipment is not normal, the material cannot be forged.
[0058] 2.2.3 The amount of material fed during forging should be uniform, and the center line of the billet should be roughly consistent with the center line of the ingot.
[0059] 2.2.4 The forging process should be regular and the billet should be turned to one side as much as possible to make the temperature of the billet uniform and ensure the axis is consistent.
[0060] 2.2.5 The billet forging ratio is greater than or equal to 4.5.
[0061] 2.2.6 Ensure that the head and tail of the steel ingot are cut off, the large head end cutting amount ≥ 6%, the small head cutting amount ≥ 5%
[0062] 2.2.7 After forging, the forging blank is annealed at an annealing temperature of (740-800°C) and the annealing holding time is calculated based on the effective size of 2.4min / 1mm+30min.
[0063] 3. Rolling
[0064] 3.1 Rolling heating
[0065] 3.1.1 Before loading into the furnace, the forging blank is ground and there are no defects such as cracks and folds on the surface. The depth-to-width ratio of the ground part meets 1:6 and has a smooth transition.
[0066] 3.1.2 The heating equipment is in good condition; use reducing atmosphere for heating to reduce iron oxide scale; and prevent overheating and overburning.
[0067] 3.1.3 The rolling heating temperature is strictly controlled according to Table 3 to form a suitable austenite structure. The rolling slab heating process parameters are shown in Table 3.
[0068] Table 3 Billet heating process parameters
[0069]
[0070] 3.1.4 Ensure uniform temperature during heating to avoid differences in tissue properties caused by uneven temperature.
[0071] 3.2 Rolling
[0072] 3.2.1 Control the total rolling deformation ≥ 40%; Rolling is carried out below the austenite non-recrystallization temperature, and the grains are refined by large reduction and increase in deformation bands.
[0073] 3.2.2 The final rolling temperature is ≥850℃; but the final rolling temperature cannot be too high to prevent grain growth.
[0074] 3.2.3 Control the rolling reduction: the reduction of at least one pass is ≥ 25%. Adjust the finishing reduction according to the billet temperature and billet size. Control the final rolling temperature at 850℃~870℃ to make the austenite undergo dynamic or static recrystallization, refine the grains, and optimize the organizational state.
[0075] 3.2.2 For products that require two-stage rolling, the finishing heating temperature is controlled at 1060℃, and the total deformation of finishing rolling is ≥30%.
[0076] 3.2.3 After rolling, the steel is spread out and air-cooled to reduce the diffusion time during the phase transformation process, thereby refining the grains and promoting the transformation of austenite to martensite, thus preparing the organization for the performance heat treatment after annealing.
[0077] 3.2.4 After rolling, the rolled plate shall be annealed at a temperature of 730-760°C. The shortest annealing holding time shall be calculated based on the thickness of the plate: 2.4min / 1mm+20min.
[0078] 4.Performance heat treatment
[0079] CLF-1 performance heat treatment is a process that changes the internal organization and structure of the material through heating, insulation and cooling to obtain the required performance. CLF-1 performance heat treatment can significantly improve the quality and performance of CLF-1 products and meet the strict requirements of nuclear fusion engineering for materials.
[0080] 4.1 Rolled plate properties Surface finishing should be carried out before heat treatment, and there should be no iron oxide scale, cracks, etc. on the surface after finishing.
[0081] 4.2 When using an electric furnace for heating, the condition of the heat treatment furnace and thermal instruments must be kept in good condition, the furnace must be cleaned, and oxide scale, steel head and iron filings must not be left on the furnace bed.
[0082] 4.3 The carbon content of the support pads and packaging materials should be less than 0.15% to prevent alloy contamination.
[0083] 4.4 During the heat treatment process, high-precision temperature measurement equipment should be used to monitor the temperature in real time.
[0084] 4.5 Strictly control the quenching and holding time according to the process. While ensuring the shortest holding time, the longest holding time shall not exceed 2 times of the shortest holding time. Too long holding time may cause the grain size to grow and may also lead to excessive phase change, making the material brittle.
[0085] 4.6 The process specifications for performance heat treatment are shown in Table 4.
[0086] Table 4 Process specifications for performance heat treatment
[0087]
[0088]
[0089] 4.6 Quenching and air cooling may cause the CLF-1 material to soften and increase ductility, resulting in insufficient strength indicators. Therefore, CLF-1 rolled plates are water-cooled to speed up the cooling rate, improve the strength, and have good comprehensive mechanical properties after tempering.
[0090] 5. Machining
[0091] 5.1 Magnetic lifting or lifting equipment with strong magnetism is prohibited for CLF-1 plate rolling mill processing and lifting. Cloth lifting belts should be used for loading and unloading.
[0092] 5.2 Select the appropriate machine tool according to the size and processing accuracy requirements of the workpiece.
[0093] 5.3 Select appropriate processing parameters and conduct real-time monitoring and adjustment to ensure processing quality.
[0094] 5.4 Rolled plates with a thickness of less than 25 mm and a width of more than 500 mm should be processed twice. The first processing should leave 3 mm on one side, and then use heat aging, vibration aging and natural aging treatment to relax the residual stress inside the workpiece and stabilize it. The second processing should be carried out according to the required size and tolerance.
[0095] 5.5 The machining surface roughness meets Ra6.3.
[0096] 6. Inspection
[0097] 6.1 Performance requirements of rolled plate CLF-1
[0098] See Table 5.
[0099] 6.2 Forging ratio comparison
[0100] The performance comparison of steel ingots with the same furnace number and specification at different forging ratios is shown in Table 6.
[0101] It can be seen from Table 6 that when the forging ratio of CLF-1 billet reaches 4.5, the segregation phenomenon inside the material can be effectively reduced, making the distribution of alloy elements more uniform, and significantly improving the strength and toughness of the material. The appropriate forging ratio can break up the coarse cast grains and form a fine and uniform grain structure, thereby improving the mechanical properties of the material. The appropriate forging ratio of CLF-1 billet is 4.5-5.5.
[0102] 6.3 Comparison of rolling control performance
[0103] The performance comparison of different rolling control methods with the same furnace number and specification is shown in Table 7.
[0104] It can be seen from the above table that insufficient deformation during final annealing during rolling will lead to a significant decrease in the mechanical properties of the CLF-1 material, and the grain size cannot meet the requirements, thus reducing the overall performance of the CLF-1.
[0105] If the final rolling temperature is too high, the austenite grains will grow rapidly and form a coarse grain structure. This structure will easily lead to uneven internal stress distribution during the cooling process, thereby reducing the mechanical properties of the CLF-1 material. Coarse grains will reduce the grain boundary area, making the toughness of the CLF-1 material lower; coarse grains will weaken the material's ability to resist deformation when subjected to stress, which is manifested as a decrease in yield strength and tensile strength.
[0106] From the results of Table 6-Table 7, we can see that:
[0107] 1. The forging ratio of forging is controlled at 4.5-5.5 to ensure the uniformity of mechanical properties of the rolled plate;
[0108] 2. Control the total rolling deformation ≥ 40%, and meet the deformation of 25% in a single pass. Control the final rolling temperature at 850-870℃, which can control the grain size of the rolled plate to be fine, prepare the organization for the final heat treatment, and ensure the comprehensive mechanical properties of the finished rolled plate.
[0109]
[0110]
[0111]
Claims
1. A process for preparing CLF steel rolled plate, It is characterized in that The steps include: Vacuum smelting → consumable remelting → forging → rolling → performance heat treatment → machining → acceptance; The forging ratio is controlled at 4.5-5.5 during forging, and the final rolling temperature is controlled at 850-870°C during rolling.
2. The process for preparing the CLF steel rolled plate according to claim 1, It is characterized in that The preparation process comprises at least one of the features (1) to (3): (1) During forging, forging heating is performed according to the specifications of the steel ingot: when the raw material specifications are 260-750 mm, the charging temperature is ≤700°C, the shortest heating time is 8-14 h, the holding time at 850°C is 2-4 h, the heating temperature is 1200°C, and the holding time is 2-6 h; (2) During rolling, the billet is heated according to the billet specifications: the billet specifications are 40-200 mm, the charging temperature is ≤550°C, the heating time is 120-220 min, the heating temperature is 1140-1160°C, the minimum holding time is 50-100 min, and the finishing temperature is 1050-1070°C; (3) During the performance heat treatment, quenching is performed according to the specifications of the rolled plate: the holding temperature is 970-990°C, the rolled plate specification is <90mm, the shortest holding time is 50-100min, and the cooling method is water cooling; (4) During the performance heat treatment, tempering is carried out according to the specifications of the rolled plate: the holding temperature is 730-750°C, the rolled plate specification is less than 90mm, the shortest holding time is 90-180min, and the cooling method is air cooling.
3. The process for preparing the CLF steel rolled plate according to claim 2, It is characterized in that (1) During forging, forging heating is performed according to the specifications of the steel ingot: (1-1) When the raw material specification is 260-360mm, the furnace temperature is ≤700℃, the shortest heating time is 8h, the holding time at 850℃ is 2h, the heating temperature is 1200℃, and the holding time is 2.5h; (1-2) When the raw material specification is 361~470mm, the charging temperature is ≤650℃, the shortest heating time is 10h, the holding time at 850℃ is 2.5h, the heating temperature is 1200℃, and the holding time is 3.5h; (1-3) When the raw material specifications are 471-590 mm, the furnace temperature is ≤650°C, the shortest heating time is 12 h, the holding time at 850°C is 3 h, the heating temperature is 1200°C, and the holding time is 4.5 h; (1-4) When the raw material specifications are 591~750mm, the furnace temperature is ≤600℃, the shortest heating time is 14h, the 850℃ insulation time is 3.5h, the heating temperature is 1200℃, and the insulation time is 5.5h.
4. The process for preparing the CLF steel rolled plate according to claim 2, It is characterized in that (2) During rolling, the slab is heated according to the slab specifications: (2-1) The billet specification is 40-90 mm, the charging temperature is ≤550°C, the heating time is 120 min, the heating temperature is 1150°C, the minimum holding time is 60 min, and the finishing temperature is 1060°C; (2-2) The billet specification is 91-140 mm, the furnace temperature is ≤550°C, the heating time is 160 min, the heating temperature is 1150°C, the minimum holding time is 75 min, and the finishing temperature is 1060°C; (2-3) The specifications of the rolled billet are 141~200mm, the charging temperature is ≤550℃, the heating time is 200min, the heating temperature is 1150℃, the minimum holding time is 60min, and the finishing temperature is 1060℃.
5. The process for preparing the CLF steel rolled plate according to claim 2, It is characterized in that (3) During the performance heat treatment, quenching is carried out according to the specifications of the rolled plate: (3-1) The holding temperature is 970-990℃, the plate specification is ≤10mm, the shortest holding time is 45min, and the cooling method is water cooling; (3-2) The holding temperature is 970-990℃, the plate specification is >10-35mm, the shortest holding time is 60min, and the cooling method is water cooling; (3-3) The holding temperature is 970-990℃, the plate specification is >35-50mm, the shortest holding time is 85min, and the cooling method is water cooling; (3-4) The holding temperature is 970-990°C, the rolled plate specification is >50-85mm, the shortest holding time is 100min, and the cooling method is water cooling.
6. The process for preparing the CLF steel rolled plate according to claim 2, It is characterized in that (4) During the performance heat treatment, tempering is carried out according to the specifications of the rolled plate: (4-1) The holding temperature is 730-750℃, the rolled plate specification is ≤10mm, the shortest holding time is 90min, and the cooling method is air cooling; (4-2) The holding temperature is 730-750℃, the rolled plate specification is >10-35mm, the shortest holding time is 120min, and the cooling method is air cooling; (4-3) The holding temperature is 730-750℃, the rolled plate specification is >35-50mm, the shortest holding time is 150min, and the cooling method is air cooling; (4-4) The holding temperature is 730-750℃, the rolled plate specification is >50-85mm, the shortest holding time is 180min, and the cooling method is air cooling.
7. The process for preparing CLF steel rolled plate according to any one of claims 1 to 6, It is characterized in that Forging billet annealing: annealing temperature is 740-800℃, annealing holding time is calculated based on effective size 2.4min / 1mm+30min.
8. The process for preparing CLF steel rolled plate according to any one of claims 1 to 6, It is characterized in that During rolling, the final rolling temperature is controlled to be ≥850°C, and the rolling reduction is controlled: the reduction in at least one pass is ≥25%.
9. The process for preparing the CLF steel rolled plate according to claim 7, It is characterized in that For products that require two-stage rolling, the finishing heating temperature is controlled at 1060°C, and the total deformation of finishing rolling is ≥30%; and / or, the annealing temperature is 730-760°C, and the shortest annealing holding time is calculated based on the thickness size of 2.4min / 1mm+20min.
10. A CLF steel rolled plate obtained by the preparation process as claimed in any one of claims 1 to 9.
Citation Information
Patent Citations
Novel dispersion-strengthened low-activation radiation-resistant martensitic steel and heat treatment technology thereof
CN107130185A
Method for preparing oxide dispersion strengthened F / M steel through smelting and casting process
CN107824771A
Preparation method of anti-irradiation low activation steel strengthened by nano-precipitation phase
CN109594009A
High-temperature high-strength and high-plasticity ferrite martensite steel and preparation method thereof
CN117431370A