Preparation method of continuous interpenetrating porous composite material
The three-dimensional dual continuous interpenetrating porous structure is formed through 3D printing and melt foaming technology, which solves the problem of insufficient interface bonding of porous metal composite materials and significantly improves its mechanical properties and cost-effectiveness.
Patent Information
- Application Number
- CN202411291099.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-29
AI Technical Summary
During the preparation of existing porous metal composite materials, there are fewer interface bonding areas of the composite structure, resulting in low interface interactions during compression and poor comprehensive mechanical properties.
The reverse structure sand pattern with orderly structures is prepared by 3D printing technology, combined with seepage casting and melt foaming technology, a three-dimensional dual continuous interpenetrating porous structure is formed, increasing the interface contact between orderly and disordered structures, and significantly improving the mechanical properties of composite materials. .
The comprehensive mechanical properties of the composite structure are significantly enhanced, including Young's modulus, compression strength, specific strength and energy absorption capacity, exceeding the sum of the numerical values of a single structure and reducing the preparation cost.
Smart Images

Figure CN119035509A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metals, and in particular to a method for preparing a continuous interpenetrating porous composite material. Background Art
[0002] Porous metals are composed of a metal frame and internal pores. They not only have the advantages of porous structures (such as good energy absorption and electromagnetic shielding capabilities), but also have the characteristics of metal materials (such as thermal and electrical conductivity). Therefore, they are widely used in transportation, aerospace, weapons and equipment and other fields. According to the connectivity of the internal pores, porous metals can be divided into ordered porous and disordered porous. Ordered porous refers to repeatable structures with spatial periodicity, such as lattice structures, ordered porous plates, and ordered porous hollow tubes. They are highly designable and have high strength. Disordered porosity refers to a structure in which pores are randomly distributed inside the porous metal, such as open-cell foam metals, closed-cell foam metals, etc. The disordered structure has good energy absorption and electromagnetic shielding capabilities, but its own strength is low. In order to improve the comprehensive mechanical properties of porous metals, people have made many attempts.
[0003] For ordered porous metals, researchers adjust their comprehensive mechanical properties through unit structure design, node reinforcement and gradient structure optimization. However, the shorter stress platform stage of ordered porous metals limits their further application in the industrial field. For disordered porous metals (foam metals), some scholars use the addition of alloy elements, the introduction of gradient disordered structures and particle reinforcement (such as the addition of ceramic particles, carbon nanotubes, and carbon fibers) to improve their compressive strength. However, the above methods have limited effect on improving the compressive strength of foam metals.
[0004] The researchers tried to combine the above two structures into an ordered / disordered porous composite material, hoping to give full play to their respective advantages and realize the integration of structure and function. The study found that the ordered / disordered porous composite material not only has a stronger load-bearing function, but also takes advantage of the functional advantages of disordered foam, realizing the preparation of structural-functional integrated materials that integrate load-bearing, energy absorption, and sound insulation. The researchers used foamed aluminum as a core to fill thin plates, thin-walled tubes, and corrugated structures to form a sandwich structure, which effectively enhanced the comprehensive performance of the porous metal structure. However, cracks always initiate and expand in disordered structures with weak mechanical properties, resulting in the structure being unable to exert the performance advantages of each single structure. As described in the preparation method of a porous composite material disclosed in the Chinese invention patent "An in-situ preparation method of a continuous interpenetrating ordered / disordered porous composite material", whose patent application number is CN 202110912209.5 (application publication number is CN113667856A), the disordered / ordered three-dimensional interpenetrating porous structure retains the advantages of the two porous structures, and the sufficient mutual support of the two structures during the compression process can significantly improve its mechanical properties, showing obvious mechanical property enhancement. Although the three-dimensional bicontinuous interpenetrating porous structure mentioned in the patent has excellent mechanical properties, since the foam aluminum must first be machined in the preparation process, and then the alloy is poured into the ordered pores by infiltration casting, this will result in a very limited range of the connection interface between the ordered structure and the disordered foam metal, that is, only the cut pore wall can contact the cast aluminum solution to form an interface. This preparation sequence cannot fully utilize the in-situ interface advantages of the bicontinuous interpenetrating structure. Therefore, the current preparation method limits the development and application of ordered / disordered porous metal composites. Therefore, continued research and improvement of preparation methods are crucial to addressing the challenges in ordered / disordered porous metal composites, which will help promote the widespread application of such materials and bring more innovation and development opportunities to the industrial field. Summary of the invention
[0005] The main purpose of the present invention is to propose a method for preparing a continuous interpenetrating porous composite material, aiming to solve the problem that in the process of preparing porous composite materials in the prior art, the interface bonding area of the composite structure is small and the interface interaction is low during the compression process, resulting in the prepared porous metal having poor comprehensive mechanical properties.
[0006] To achieve the above object, the present invention provides a method for preparing a continuous interpenetrating porous composite material, comprising the following steps:
[0007] S1. Use 3D printing technology to prepare the reverse structure sand mold with ordered structure;
[0008] S2, preparing ordered structures by infiltration casting;
[0009] S3. A three-dimensional bi-continuous interpenetrating porous structure is prepared by melt foaming + infiltration casting, that is, a continuous interpenetrating porous composite material is obtained.
[0010] Preferably, step S1 specifically includes: making the required structure with three-dimensional software and importing it into a 3D printing operation program in STL format, and obtaining an inverse structure sand mold with an ordered structure after starting the program.
[0011] Preferably, in step S1, the raw material for 3D printing is coated sand, and the particle size distribution range of the coated sand is 75 μm-250 μm.
[0012] Preferably, step S2 specifically includes: coating the bottom surface of the inverse structure sand mold with a layer of adhesive, bonding it to the bottom of the metal mold, placing the inverse structure sand mold and the metal mold at room temperature for 12 to 16 hours, waiting for the adhesive to solidify, placing the inverse structure sand mold and the mold at 180 to 220°C for preheating for 1.5 to 2.5 hours, melting the aluminum alloy in a pit-type melting furnace, and infiltrating the aluminum alloy solution into the inverse structure sand mold at 700-800°C, and after complete cooling, heat treating at 380 to 420°C for 0.8 to 1.2 hours to remove the inverse structure sand mold, and machining to obtain an ordered structure.
[0013] Preferably, the metal mold is of top injection type, with a riser on it to provide a pressure head and shrinkage compensation function; the side of the metal mold is provided with an inclination to facilitate demoulding.
[0014] Preferably, in step S2, the material of the ordered structure is ordered porous aluminum or ordered porous aluminum alloy.
[0015] Preferably, in step S2, the ordered structure is a three-dimensional periodic structure, the periodic structure is a uniform structure or a gradient structure, and the periodic structure is composed of cylinders and / or prisms and / or hollow tubes and / or plates.
[0016] Preferably, in step S2, the ordered structure is a through-hole structure and a periodic structure.
[0017] Preferably, step S3 specifically includes: melting an aluminum alloy ingot in a pit furnace, adding a viscosity enhancer, stirring, and then adding a foaming agent and stirring to obtain a molten metal to be foamed, using an adhesive to bond the ordered structure to the bottom of a metal mold, and then pouring the molten metal to be foamed into the metal mold. The melt fills the holes in the ordered structure under the action of gravity, and then foams to replace the holes in the ordered structure with disordered foam aluminum. After cooling, wire cutting is performed to obtain a three-dimensional double-continuous interpenetrating porous metal structure.
[0018] Preferably, the molten metal to be foamed is foamed aluminum or foamed aluminum alloy; the viscosity enhancer is 3% to 5% by mass of calcium; and the foaming agent is 0.04% to 1.0% by mass of TiH2.
[0019] Compared with the prior art, the beneficial effects of the present invention are:
[0020] (1) The present invention adopts a combination of 3D printing, melt foaming and infiltration casting to obtain a three-dimensional bicontinuous interpenetrating porous composite material. First, a reverse structure sand mold of an ordered structure is obtained by using 3D printing technology, and then an ordered structure is obtained by using infiltration casting. The molten alloy liquid to be foamed is infiltrated into the ordered structure, so that the foamed metal is formed after foaming to replace the ordered structure pores to obtain a three-dimensional bicontinuous interpenetrating porous composite material. This method realizes more interface contacts between single structures, so that the structure shows a good mutual reinforcement effect during the compression process, thereby significantly enhancing the comprehensive mechanical properties of the composite structure.
[0021] (2) The preparation method provided by the present invention not only avoids the problem of expensive equipment and raw materials in additive manufacturing and powder metallurgy, but also improves the comprehensive mechanical properties of the composite structure. Its Young's modulus, compressive strength, specific strength, platform stress and energy absorption capacity are significantly improved compared with those of a single structure, and are higher than the sum of the values of the two. There is a bubble-free layer at the interface of the composite porous structure obtained by this preparation sequence, and its mechanical properties are significantly higher than those of the composite structure obtained by first preparing disordered foam and then preparing ordered structure. This method has a simple process, low cost, and can be promoted and applied on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 It is the reverse structure sand mold diagram of the ordered structure of the present invention, wherein Figure 1 (Left) is the reverse structure sand mold diagram of the ordered structure in Example 1, Figure 1 (right) is the reverse structure sand mold image of the ordered structure in Example 2;
[0024] Figure 2 The detailed size and shape of the metal mold in Example 1 of the present invention;
[0025] Figure 3 is a sample diagram of the ordered structure of the present invention, wherein Figure 3 (Left) is the ordered structure sample diagram in Example 1, Figure 3 (right) is a sample diagram of the ordered structure in Example 2;
[0026] Figure 4Schematic diagram of the composite structure and corresponding characteristic unit physical diagram in Example 1 of the present invention;
[0027] Figure 5 This is an interface morphology diagram of the composite structure prepared in Example 1 of the present invention;
[0028] Figure 6 It is a quasi-static compressive stress-strain curve diagram of the composite structure, ordered porous aluminum, and foamed aluminum in Example 1 of the present invention.
[0029] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0030] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of the technical schemes is contradictory or cannot be achieved, it should be considered that the combination of such technical schemes does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0031] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0032] Embodiment 1 A method for preparing a continuous interpenetrating porous composite material comprises the following steps:
[0033] (1) 3D printing is used to prepare the inverse structure sand mold of the ordered porous structure. The three-dimensional model of the ordered porous aluminum is established using Pro / Engineer three-dimensional modeling software, and its inverse structure is obtained through Boolean operation. The structure is exported as an STL format file, such as Figure 1 (Left) As shown. The file was imported into Magics software for layering, and the sand mold was prepared using a selective sintering system. The particle size of the coated sand used in the experiment was 200μm. The layer spacing set in the selective laser sintering process was 0.25mm, the selective laser sintering power was 60W, the scanning rate was 2000mm / s, the scanning spacing was 0.2mm, and the preheating temperature of the coated sand was 75℃.
[0034] (2) Use infiltration casting to prepare an ordered porous structure. Evenly apply a layer of adhesive on the bottom of the sand mold and bond it to the bottom of the metal mold to prevent the sand mold from floating up during the infiltration process. The metal mold is Figure 2 As shown; place the sand mold and metal mold at room temperature for more than 12 hours to allow the adhesive to fully solidify; preheat the sand mold and mold at 200°C for 2 hours. Melt the cast aluminum 111 alloy (ZL111) in a pit melting furnace, and allow the alloy solution to infiltrate into the sand mold at 730°C; after complete cooling, place the ingot in a heat treatment furnace at 400°C for 1 hour to remove the sand mold, and machine it to obtain an ordered porous structure; the ordered structure is a periodic structure composed of mutually orthogonal circular columns connected by nodes. The diameter of the circular columns is 6mm, and they are arranged in a 4×4×4 pattern in space. The ordered structure sample is shown in Figure 3 (Left) shown.
[0035] (3) A three-dimensional bicontinuous interpenetrating porous structure was prepared by melt foaming + infiltration casting. The ordered structure was bonded to the bottom of the metal mold with an adhesive to prevent the ordered structure from tipping over or floating during the infiltration process; pure aluminum ingots were melted in a pit furnace, and a thickener (Ca, 5wt.%) was added at 740°C and stirred for 5 minutes, and then a foaming agent (TiH2, 0.05wt.%) was added at 690°C and stirred for 1 minute to obtain molten metal to be foamed, and then the molten metal to be foamed was poured into the metal mold. The melt filled the holes in the ordered structure under the action of gravity and its own fluidity, and then foamed to replace the holes in the ordered structure with disordered foamed aluminum; after the ingot was cooled, wire cutting was performed to obtain a three-dimensional bicontinuous interpenetrating porous metal structure.
[0036] Embodiment 2 A method for preparing a continuous interpenetrating porous composite material comprises the following steps:
[0037] (1) 3D printing is used to prepare the inverse structure sand mold of the ordered porous structure. The three-dimensional model of the ordered porous aluminum is established using Pro / Engineer three-dimensional modeling software, and its inverse structure is obtained through Boolean operation. The structure is exported as an STL format file, such as Figure 1 (right) As shown. The file was imported into Magics software for layering, and the selective sintering system was used to prepare the sand mold. The particle size of the coated sand used in the experiment was 75μm. The layer spacing set in the selective laser sintering process was 0.25mm, the selective laser sintering power was 50W, the scanning rate was 2000mm / s, the scanning spacing was 0.2mm, and the preheating temperature of the coated sand was 70℃.
[0038] (2) An ordered porous structure was prepared by infiltration casting. A layer of adhesive was evenly coated on the bottom of the sand mold and bonded to the bottom of the metal mold to prevent the sand mold from floating up during the infiltration process; the sand mold and the metal mold were placed at room temperature for more than 12 hours to allow the adhesive to fully solidify; the sand mold and the mold were preheated at 200°C for 2 hours. The cast aluminum 111 alloy (ZL111) was melted in a pit-type melting furnace, and the alloy solution was infiltrated into the sand mold at 730°C; after complete cooling, the ingot was placed in a heat treatment furnace at 400°C for 1 hour to remove the sand mold, and then machined to obtain an ordered porous structure; the ordered structure is a periodic structure composed of mutually orthogonal circular columns connected by nodes. The diameter of the circular columns is 6 mm, and they are arranged in a 5×5×5 pattern in space. The ordered structure sample is as follows: Figure 3 (right) shown.
[0039] (3) A three-dimensional bicontinuous interpenetrating porous structure was prepared by melt foaming + infiltration casting. The ordered structure was bonded to the bottom of the metal mold with an adhesive to prevent the ordered structure from tipping over or floating during the infiltration process; pure aluminum ingots were melted in a pit furnace, and a thickener (Ca, 5wt.%) was added at 720°C and stirred for 5 minutes, and then a foaming agent (TiH2, 0.05wt.%) was added at 690°C and stirred for 1 minute to obtain molten metal to be foamed, and then the molten metal to be foamed was poured into the metal mold. The melt filled the holes in the ordered structure under the action of gravity and its own fluidity, and then foamed to replace the holes in the ordered structure with disordered foamed aluminum; after the ingot was cooled, wire cutting was performed to obtain a three-dimensional bicontinuous interpenetrating porous metal structure.
[0040] Embodiment 3 A method for preparing a continuous interpenetrating porous composite material comprises the following steps:
[0041] (1) 3D printing was used to prepare the inverse structure sand mold of the ordered porous structure. The three-dimensional model of the ordered porous aluminum was established using Pro / Engineer three-dimensional modeling software, and its inverse structure was obtained through Boolean operation, and the structure was exported as an STL format file. The file was imported into Magics software for layering, and the sand mold was prepared using a selective sintering system. The particle size of the coated sand used in the experiment was 250μm. The layer spacing set in the selective laser sintering process was 0.25mm, the selective laser sintering power was 70W, the scanning rate was 2000mm / s, the scanning spacing was 0.2mm, and the preheating temperature of the coated sand was 80℃.
[0042] (2) An ordered porous structure was prepared by infiltration casting. A layer of adhesive was evenly coated on the bottom of the sand mold and bonded to the bottom of the metal mold to prevent the sand mold from floating up during the infiltration process; the sand mold and the metal mold were placed at room temperature for more than 12 hours to allow the adhesive to fully solidify; the sand mold and the mold were preheated at 200°C for 2 hours. Cast aluminum 111 alloy (ZL111) was melted in a pit melting furnace, and the alloy solution was infiltrated into the sand mold at 740°C; after complete cooling, the ingot was placed in a heat treatment furnace at 400°C for 1 hour to remove the sand mold, and then machined to obtain an ordered porous structure; the ordered structure was a periodic structure composed of mutually orthogonal circular columns connected by nodes, the diameter of the circular columns was 6 mm, and they were arranged in a 5×5×5 pattern in space.
[0043] (3) A three-dimensional bicontinuous interpenetrating porous structure was prepared by melt foaming + infiltration casting. The ordered structure was bonded to the bottom of the metal mold with an adhesive to prevent the ordered structure from tipping over or floating during the infiltration process; pure aluminum ingots were melted in a pit furnace, and a thickener (Ca, 5wt.%) was added at 740°C and stirred for 5 minutes, and then a foaming agent (TiH2, 0.05wt.%) was added at 690°C and stirred for 1 minute to obtain molten metal to be foamed, and then the molten metal to be foamed was poured into the metal mold. The melt filled the holes in the ordered structure under the action of gravity and its own fluidity, and then foamed to replace the holes in the ordered structure with disordered foamed aluminum; after the ingot was cooled, wire cutting was performed to obtain a three-dimensional bicontinuous interpenetrating porous metal structure.
[0044] Test methods and results
[0045] In order to facilitate microscopic characterization and performance testing, the three-dimensional bicontinuous interpenetrating porous metal structure obtained in Example 1 was taken out by wire cutting technology. The characteristic units and their composition are detailed in Figure 4 .
[0046] The microscopic morphology of the interface of the three-dimensional bicontinuous interpenetrating porous metal structure obtained in Example 1 was observed by SEM, and the Figure 5 , it was found that there was an obvious bubble-free layer at the interface, and its width was about 300-400μm. This is because in the preparation process of the order-disorder method, the temperature of the ZL111 alloy is lower than that of the melt to be foamed. When the solution contacts the ZL111 alloy, the solution near the interface solidifies rapidly, and the TiH2 inside does not have time to decompose, thus forming an obvious bubble-free layer. As the distance from the interface increases, the pore diameter in the foamed aluminum tends to increase, which is related to the nucleation and growth process of the bubbles. Obviously, the existence of the bubble-free layer increases the contact area between the ZL111 alloy and the foamed aluminum, and also provides convenient conditions for the formation of metallurgical bonding.
[0047] The mechanical properties of the three-dimensional bicontinuous interpenetrating porous metal structure characteristic unit, ordered framework, and foamed aluminum in Example 1 were analyzed. The results are as follows: Figure 6 As shown. The interpenetrating porous structures have both the longer stress platform stage of aluminum foam and the higher strength of the ordered structure, achieving the ideal mechanical property enhancement effect. It can be clearly seen from the figure that the composite of aluminum foam and the ordered framework significantly improves the mechanical properties of the material, specifically, its mechanical properties are better than the mathematical sum of aluminum foam and the ordered framework. Table 1 shows the corresponding mechanical performance indicators. The porous composite structure prepared by the ordered / disordered method exhibits the highest elastic modulus, compressive strength, specific strength (compressive strength at unit density) and platform stress. Combined with Figure 4 From the microscopic morphology of the interface, it can be seen that the existence of the bubble-free layer can significantly improve the mechanical properties of the material, and the mechanical properties of the sample are greater than the superposition of simple structures, indicating that the dual continuous interpenetrating structure prepared by the present invention can effectively strengthen each component.
[0048] Table 1 Mechanical properties of characteristic units of three-dimensional bicontinuous interpenetrating porous metal structures, ordered frameworks, and aluminum foams
[0049]
[0050] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for preparing a continuous interpenetrating porous composite material, characterized in that: The following steps are involved: S1. Use 3D printing technology to prepare the reverse structure sand mold with ordered structure; S2, preparing ordered structures by infiltration casting; S3. A three-dimensional bi-continuous interpenetrating porous structure is prepared by melt foaming + infiltration casting, that is, a continuous interpenetrating porous composite material is obtained.
2. The method for preparing the continuous interpenetrating porous composite material according to claim 1, characterized in that: Step S1 specifically includes: making the required structure with three-dimensional software and importing it into a 3D printing operation program in STL format, and obtaining an inverse structure sand mold with an ordered structure after starting the program.
3. The method for preparing the continuous interpenetrating porous composite material according to claim 1, characterized in that: In step S1, the raw material for 3D printing is coated sand, and the particle size distribution range of the coated sand is 75 μm-250 μm.
4. The method for preparing the continuous interpenetrating porous composite material according to claim 1, characterized in that: Step S2 specifically includes: coating the bottom surface of the inverse structure sand mold with a layer of adhesive, bonding it to the bottom of the metal mold, placing the inverse structure sand mold and the metal mold at room temperature for 12 to 16 hours, waiting for the adhesive to solidify, placing the inverse structure sand mold and the mold at 180 to 220°C for preheating for 1.5 to 2.5 hours, melting the aluminum alloy in a pit-type melting furnace, and infiltrating the aluminum alloy solution into the inverse structure sand mold at 700-800°C. After complete cooling, heat treatment is performed at 380 to 420°C for 0.8 to 1.2 hours to remove the inverse structure sand mold, and machining to obtain an ordered structure.
5. The method for preparing the continuous interpenetrating porous composite material according to claim 4, characterized in that: The metal mold is of top injection type and is provided with a riser on the top to provide a pressure head and shrinkage compensation function; the side of the metal mold is provided with an inclination to facilitate demoulding.
6. The method for preparing the continuous interpenetrating porous composite material according to claim 1, characterized in that: In step S2, the material of the ordered structure is ordered porous aluminum or ordered porous aluminum alloy.
7. The method for preparing the continuous interpenetrating porous composite material according to claim 1, characterized in that: In step S2, the ordered structure is a three-dimensional periodic structure, the periodic structure is a uniform structure or a gradient structure, and the periodic structure is composed of cylinders and / or prisms and / or hollow tubes and / or plates.
8. The method for preparing the continuous interpenetrating porous composite material according to claim 1, characterized in that: In step S2, the ordered structure is a through-hole structure and a periodic structure.
9. The method for preparing the continuous interpenetrating porous composite material according to claim 1, characterized in that: Step S3 specifically includes: melting an aluminum alloy ingot in a pit furnace, adding a viscosity enhancer, stirring, and then adding a foaming agent and stirring to obtain a molten metal to be foamed, using an adhesive to bond the ordered structure to the bottom of a metal mold, and then pouring the molten metal to be foamed into the metal mold. The melt fills the holes in the ordered structure under the action of gravity, and then foams to replace the holes in the ordered structure with disordered foam aluminum. After cooling, wire cutting is performed to obtain a three-dimensional double-continuous interpenetrating porous metal structure.
10. The method for preparing the continuous interpenetrating porous composite material according to claim 9, characterized in that: The molten metal to be foamed is foamed aluminum or foamed aluminum alloy; the viscosity enhancer is calcium with a mass fraction of 3% to 5%; and the foaming agent is TiH2 with a mass fraction of 0.04% to 1.0%.