Method for correcting defect depth of base metal in surfacing process

By setting rectangular grooves of different depths on the test pieces and performing surfacing treatment, the defect depth changes caused by the surfacing process are solved, and the accuracy of ultrasonic detection and database accuracy are improved. .

CN119035860APending Publication Date: 2024-11-29CHINA NUCLEAR POWER ENGINEERING COMPANY LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411402121.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The surfacing process causes changes in the depth of the surface defect of the base material, affecting the accuracy of ultrasonic detection technology, and the standard sample fails, making it impossible to accurately measure the depth of the rectangular grooves.

Method used

Set up multiple rectangular grooves of different depths on the test piece to simulate defects, and then cut and reveal cross-sections after surfacing, measure the depth after surfacing, calculate the defect depth correction value, and correct the defect depth of the base material to be surfacing .

Benefits of technology

Through accurate defect depth correction, a more accurate database was established, which improved the accuracy of the ultrasonic inspection technology of the base material under the surfacing layer and the minimum defect detection ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035860A_ABST
    Figure CN119035860A_ABST
Patent Text Reader

Abstract

The invention provides a method for correcting the defect depth of a base metal under a surfacing process, which comprises the following steps: a plurality of rectangular cutting grooves with different depths are formed in a test piece for simulating defects, and the material of the test piece is the same as that of the base metal to be surfaced; surfacing treatment is conducted on the surface of the test piece in the direction perpendicular to the length direction of the rectangular cutting groove, and the test piece subjected to surfacing treatment is obtained; cutting the test piece after surfacing so as to expose the cross sections of the rectangular cutting grooves with different depths; measuring the cross section of the rectangular cutting groove under different depths to obtain the depth of the rectangular cutting groove after surfacing under each depth; and according to the depth of the rectangular cutting groove after surfacing under each depth, a defect depth correction value is obtained, and the defect depth of the to-be-surfaced base metal is corrected according to the defect depth correction value. By means of the method, a more accurate database can be obtained, and the effectiveness and accuracy of the test of the UT inspection technology minimum defect detection capacity of the base metal under the surfacing layer are guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material welding and nondestructive testing, and in particular to a method for correcting the depth of a base material defect in a surfacing welding process. Background Art

[0002] Important equipment in nuclear power plants, such as reactor pressure vessels, steam generators, and pressurizers, usually use special low-alloy steel as the container structure material because they have to withstand high temperature, high pressure, and radiation. However, low alloys will corrode when in contact with the loop coolant. Usually, an austenitic stainless steel alloy layer is formed on the parent material surface of the inner wall of the container by cladding to prevent corrosion, thereby ensuring the performance of the power plant equipment and extending the life of the equipment.

[0003] The implementation of the cladding process generally ensures the welding quality by selecting appropriate cladding materials and optimizing welding processes. However, the cladding process will also affect the surface of the parent material of the equipment. It is possible that cracks will occur on the surface of the parent material due to defects on the surface of the parent material or improper control of the welding process. When the power station is in operation, the internal surface of the container is subjected to high temperature and high pressure. The stress on the inner surface of the low-alloy steel of the container is the greatest. If there are tiny defects on the surface of the parent material, they will expand into cracks under the action of stress and extend from the inside to the outside. According to feedback from the engineering practice of a nuclear power plant abroad, crack-like defects were found on the surface of the parent material under the cladding layer.

[0004] Crack defects are the most harmful to the safe operation of equipment. When the crack reaches a certain depth, it will cause the parent material to crack or break, seriously affecting nuclear safety. Therefore, after the surface cladding of the parent material on the inner wall of the equipment is completed and after operation, it is necessary to carry out ultrasonic testing (UT) of the parent material under the cladding layer to detect whether there are dangerous defects such as cracks caused by the cladding process or operation.

[0005] A key step in UT inspection technology is to calibrate the equipment, that is, to use the inspection data of standard samples with known defects to calibrate the ultrasonic inspection equipment to ensure that it can correctly identify and measure defects. The standard sample provides a known reference point to help inspectors understand how defects of different types and sizes appear on ultrasonic images. In actual operation, the standard sample usually contains a series of artificial defects of different sizes and types, which are embedded in the material for ultrasonic testing. By analyzing the ultrasonic response of these known defects, a database can be established for comparison of unknown defects found in actual inspections.

[0006] Since the cladding process is a process of metal remelting and reconstruction, the rectangular groove (open groove) prefabricated on the surface of the parent material to be clad will be affected by the cladding process, resulting in the change of the prefabricated defect size (especially the depth direction size) due to the cladding process, and the rectangular groove can no longer be accurately measured after cladding (the open groove becomes a buried groove), that is, the simulated defect size under the cladding layer cannot be accurately obtained, resulting in the standard sample no longer being "standard", thus affecting the accuracy of the UT inspection technology. Summary of the invention

[0007] In view of the above defects of the prior art, the present invention provides a method for correcting the defect depth of a base material in a cladding process to solve the technical problem of inaccurate benchmark data of UT inspection technology.

[0008] To achieve the above-mentioned purpose and other related purposes, the present invention provides a method for correcting the defect depth of a base material under a surfacing process, comprising: setting a plurality of rectangular grooves of different depths on a test piece for simulating defects, wherein the material of the test piece is the same as the material of the base material to be surfacing; performing surfacing treatment on the surface of the test piece along a length direction perpendicular to the rectangular groove to obtain a surfacing test piece; cutting the surfacing test piece to reveal the cross-sections of the rectangular grooves of different depths; measuring the cross-sections of the rectangular grooves at different depths to obtain the depth of the rectangular grooves after surfacing at each depth; obtaining a defect depth correction value according to the depth of the rectangular grooves after surfacing at each depth, and correcting the defect depth of the base material to be surfacing according to the defect depth correction value.

[0009] In one embodiment of the present invention, a plurality of rectangular grooves of different depths are arranged at intervals along a length direction perpendicular to the rectangular groove, and there is at least one section along the length direction perpendicular to the rectangular groove that can cut each rectangular groove into two parts.

[0010] In one embodiment of the present invention, the depths of the rectangular grooves of different depths gradually increase or decrease along a length direction perpendicular to the rectangular grooves, and the depth difference between any two adjacent rectangular grooves is equal.

[0011] In one embodiment of the present invention, a plurality of rectangular grooves of different depths are arranged on the test piece, including: a plurality of groups of the rectangular grooves are arranged at intervals along a first direction on the test piece, each group of the rectangular grooves is composed of a plurality of rectangular grooves of different depths arranged at intervals perpendicular to the first direction, and the first direction is the length or width direction of the test piece.

[0012] In one embodiment of the present invention, the cross-sections of the rectangular grooves at different depths are measured to obtain the depth of the rectangular grooves after surfacing at each depth, including: measuring the cross-sections of multiple groups of rectangular grooves at different depths to obtain the depths of the multiple groups of rectangular grooves at different depths after surfacing; and obtaining the depth of the rectangular grooves after surfacing at each depth based on the depths of the rectangular grooves of the same depth in multiple groups after surfacing.

[0013] In one embodiment of the present invention, a plurality of rectangular grooves of different depths are provided on the test piece, including: obtaining the length of each rectangular groove according to a preset depth of each rectangular groove, and a preset minimum multiple and a preset maximum multiple; obtaining the width of all the rectangular grooves according to a minimum value of the depth of the rectangular groove, and a preset ratio; and providing a plurality of rectangular grooves of different depths on the test piece according to the preset depth, length and width of each rectangular groove.

[0014] In one embodiment of the present invention, the surfacing thickness of the test piece when the surfacing treatment is performed on the surface of the test piece is greater than or equal to a set threshold.

[0015] In one embodiment of the present invention, in the step of measuring the cross-section of the rectangular groove at different depths to obtain the depth of the rectangular groove after surfacing at each depth, for any rectangular groove: measure the two side surfaces corresponding to the cross-section of the rectangular groove to obtain two depth values ​​of the rectangular groove, and take the average of the two depth values ​​as the depth of the rectangular groove after surfacing.

[0016] In one embodiment of the present invention, a defect depth correction value is obtained according to the depth of the rectangular groove after surfacing at each depth, including: obtaining the difference in penetration depth of the rectangular groove at each depth according to the depth of the rectangular groove after surfacing at each depth; obtaining the defect depth correction value according to the difference in penetration depth of the rectangular groove at each depth.

[0017] In one embodiment of the present invention, correcting the defect depth of the base material to be built-up according to the defect depth correction value includes: correcting the defect depth of the base material to be built-up according to the sum of a preset defect depth and the defect depth correction value.

[0018] Beneficial effects of the present invention: The present invention proposes a method for correcting the defect depth of a base material under a cladding process. The method constructs a test piece of the same material as the base material to be clad, simulates multiple defects on the test piece and performs cladding treatment, and then cuts it to expose the depth of the rectangular groove after cladding at different depths, thereby obtaining a defect depth correction value, and finally uses the correction value to correct the defect depth of the base material to be clad, thereby obtaining a more accurate database, thereby ensuring the effectiveness and accuracy of the minimum defect detection capability test of the base material UT inspection technology under the cladding layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 A flow chart of a method for correcting a base material defect depth provided by an embodiment of the present invention;

[0021] Figure 2 A schematic diagram of the structure of a test piece provided by an embodiment of the present invention;

[0022] Figure 3 A flow chart of setting a rectangular groove provided in one embodiment of the present invention;

[0023] Figure 4 A schematic diagram of the structure of a test piece after being cut open provided by an embodiment of the present invention;

[0024] Figure 5 A flow chart of depth calculation of a rectangular groove after surfacing provided by an embodiment of the present invention;

[0025] Figure 6 A defect depth correction value calculation flow chart provided in one embodiment of the present invention. DETAILED DESCRIPTION

[0026] The following describes the embodiments of the present invention through specific specific embodiments, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. It should be noted that the following embodiments and the features in the embodiments can be combined with each other without conflict. In addition to the specific methods, equipment, and materials used in the embodiments, according to the technical personnel in this technical field's grasp of the prior art and the records of the present invention, any methods, equipment, and materials of the prior art that are similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to implement the present invention.

[0027] It should be understood that the terms used in the embodiments of the present invention are for describing specific embodiments rather than for limiting the scope of protection of the present invention. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art.

[0028] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions under which the present invention can be implemented, so they have no substantive technical significance. Any modification of the structure, change in the proportional relationship, or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effects and purposes that can be achieved by the present invention. In addition, the drawings only show the components related to the present invention rather than the number, shape, and size of the components in actual implementation. The type, quantity, and proportion of each component in actual implementation can be changed arbitrarily, and the component layout type may also be more complicated.

[0029] In the following description, numerous details are discussed to provide a more thorough explanation of the embodiments of the present invention. However, it is obvious to those skilled in the art that the embodiments of the present invention can be implemented without these specific details. In some of the embodiments, well-known structures and devices are shown in the form of block diagrams rather than in detail to avoid making the embodiments of the present invention difficult to understand.

[0030] The flowchart and block diagram in the accompanying drawings illustrate the system architecture, functions and operations that may be implemented according to the methods and computer program products of various embodiments disclosed in the present invention. In this regard, each box in the flowchart or block diagram can represent a module, a program segment, or a part of a code, and the module, the program segment, or a part of the code contains one or more executable instructions for implementing the specified logical function. It should also be noted that in some alternative implementations, the functions marked in the box can also occur in a different order from the order marked in the accompanying drawings. For example, two boxes represented in succession can actually be executed substantially in parallel, and they can sometimes be executed in the opposite order, depending on the functions involved. It should also be noted that each box in the block diagram and / or the flowchart, and the combination of the boxes in the block diagram and / or the flowchart can be implemented with a dedicated hardware-based system that performs the specified function or operation, or can be implemented with a combination of dedicated hardware and computer instructions.

[0031] See also Figure 1 , Figure 1 A method for correcting the depth of a base material defect in a cladding process provided by an embodiment of the present invention includes steps S100 to S500.

[0032] Step S100, multiple rectangular grooves of different depths are set on the test piece to simulate defects, wherein the material of the test piece is the same as the material of the base material to be welded. Considering the importance of nuclear power plant equipment, welding range, welding difficulty and other factors, the inner wall welding part of the nozzle of the reactor pressure vessel is selected as the typical test object of this test, and the material of the base material to be welded is low alloy steel (16MND5).

[0033] The size of the test piece should be selected according to the principle of minimum material extraction, and the smaller the size of the test piece should be, the better it is to ensure that there is no interference with defects. Figure 2 Taking the rectangular groove as an example, the size of the test piece is 180mm×120mm×90mm (length×width×height), and it is planned to design five rectangular grooves (simulated defects), with the interval between defects being 30mm and the distance from the two end faces being 30mm.

[0034] A plurality of rectangular grooves of different depths are usually arranged at the largest surface of the test piece. In theory, these rectangular grooves can be arranged in any manner, but in order to facilitate subsequent cutting and measurement, the rectangular grooves of different depths should be aligned as much as possible. The rectangular grooves of different depths can be arranged at intervals along the length direction parallel to the rectangular grooves, or can be arranged at intervals along the length direction perpendicular to the rectangular grooves.

[0035] See also Figure 2 In a specific embodiment of the present invention, a plurality of rectangular grooves of different depths are arranged at intervals along a length direction perpendicular to the rectangular groove, which is convenient for subsequent cutting. At least one cut surface along a length direction perpendicular to the rectangular groove can cut each rectangular groove into two parts. It should be noted that for the plurality of groups of rectangular grooves mentioned below (for example Figure 2 Here, “each rectangular groove can be cut into two parts” means “each rectangular groove in each group of rectangular grooves can be cut into two parts”. If there is only one rectangular groove at each depth, then it should be ensured that there is at least one cutting surface that can cut all rectangular grooves into two parts. Specifically, it can be as follows Figure 2 As shown in the figure, the center lines of the multiple rectangular grooves with different depths are aligned; or one of the wide sides of the multiple rectangular grooves with different depths can be aligned.

[0036] In order to clearly illustrate the length, width and depth of the rectangular groove, Figure 2 There are three sides marked in the figure, side A, side B and side C. The direction parallel to side A is the length direction of the rectangular groove, also called the groove direction of the rectangular groove; the direction parallel to side B is the width direction of the rectangular groove; the direction parallel to side C is the depth direction of the rectangular groove.

[0037] In a specific embodiment of the present invention, the depths of the plurality of rectangular grooves of different depths gradually increase or decrease along the length direction perpendicular to the rectangular grooves, and the depth difference between any two adjacent rectangular grooves is equal. For example, the depths of the plurality of rectangular grooves of different depths are 2 mm, 4 mm, 6 mm, 8 mm, and 10 mm, respectively, which are used to simulate crack defects of five specific sizes, and the sensitivity of different defect depths to the surfacing process is also considered.

[0038] See also Figure 2 In a specific embodiment of the present invention, a plurality of rectangular grooves of different depths are arranged on the test piece, including: a plurality of groups of rectangular grooves are arranged at intervals along a first direction on the test piece, each group of rectangular grooves is composed of a plurality of rectangular grooves of different depths arranged at intervals perpendicular to the first direction, and the first direction is the length or width direction of the test piece. The plurality of groups of rectangular grooves are arranged according to the same process parameters. Figure 2 In the test, the first direction is the width direction of the test piece, and there are two groups of rectangular grooves, each group of rectangular grooves is composed of 5 rectangular grooves of different depths. The reason for setting multiple groups of rectangular grooves is to ensure the accuracy and representativeness of the test results.

[0039] See also Figure 3 In a specific embodiment of the present invention, a plurality of rectangular grooves of different depths are provided on the test piece, including steps S101 to S103.

[0040] Step S101, according to the preset depth of each rectangular groove, and the preset minimum multiple and maximum multiple, the length of each rectangular groove is obtained. The preset depth of each rectangular groove is set in advance according to the mechanical calculation requirements, for example, the preset depth is 2mm, 4mm, 6mm, 8mm, 10mm.

[0041] Rectangular grooves mainly simulate crack-like hazardous defects, and their key dimension information is the depth of the rectangular grooves, and the length is often expressed in multiples of the depth. Therefore, in this embodiment, based on the preset depth, the preset minimum multiple and maximum multiple are combined to calculate the length of the rectangular groove. The preset minimum multiple can be, for example, 2 times, and the maximum multiple can be, for example, 3 times. When the depth of the rectangular groove is different, the length also changes accordingly. For example, the length of a rectangular groove with a depth of 2mm can be a value between 4 and 6mm, and the length of a rectangular groove with a depth of 10mm can be a value between 20 and 30mm.

[0042] Step S102, according to the minimum value of the depth of the rectangular groove and the preset ratio, the width of all the rectangular grooves is obtained. The widths of rectangular grooves of different depths can be the same. The main dimension of the rectangular groove is the depth. For crack-like defects, the width is generally small. Therefore, in this embodiment, the width of the rectangular groove is calculated according to the minimum value of the depth of the rectangular groove. In the above example, the minimum depth of the rectangular groove is 2mm, and the preset ratio can be any value less than or equal to 0.3, for example, if the preset ratio is equal to 0.1, then the width of the rectangular groove calculated according to the preset ratio is 0.2mm.

[0043] Step S103: according to the preset depth, length and width of each rectangular groove, a plurality of rectangular grooves of different depths are arranged on the test piece. After the depth, length and width of each rectangular groove are known, combined with the arrangement method in the above embodiment, a test piece that meets the requirements can be processed.

[0044] Step S200, performing a surfacing process on the surface of the test piece along the length direction perpendicular to the rectangular cut groove to obtain a surfacing test piece. The filler material in the surfacing process may be, for example, austenitic stainless steel (type 308L / 309L), and the surfacing method may be, for example, tungsten inert gas (TIG) welding, which is an arc welding technology that uses a tungsten electrode and an inert gas (usually argon or helium) to protect the welding area. TIG welding is well known for its high quality, high precision and high operator skill requirements, and is often used for welding thin sheet metal and occasions where heat input needs to be strictly controlled.

[0045] In a specific embodiment of the present invention, the thickness of the surfacing when the surface of the test piece is surfacing treated is greater than or equal to a set threshold. The design thickness of the surfacing layer is usually based on the required mechanical properties, corrosion resistance or wear resistance. Ensuring that the surfacing thickness reaches or exceeds this threshold can ensure that the welded structure meets the design and functional requirements. When performing non-destructive testing such as ultrasonic testing, it is necessary to ensure that the thickness of the surfacing layer allows ultrasonic waves to effectively penetrate and reflect, so as to accurately detect defects in the parent material under the surfacing layer. If the surfacing layer is too thin, deeper defects may not be effectively detected. For example, for a test piece of the above size, the set threshold can be 7mm.

[0046] Step S300: Cut the test piece after surfacing to reveal the cross-section of the rectangular grooves of different depths. The purpose of revealing the cross-section of the rectangular grooves is to subsequently measure the actual depth of the rectangular grooves after surfacing. Taking the above test piece as an example, the structure after cutting is as follows: Figure 4As shown, at this time, the cross-sections of all rectangular cut grooves have been revealed, and the next measurement operation can be carried out. Since the material of the test piece is relatively hard, it can be cut by wire cutting. Wire cutting is a processing technology that uses a moving thin metal wire (usually copper wire or molybdenum wire) as a tool electrode to cut the material through the principle of electric spark discharge.

[0047] Step S400, measuring the cross-section of the rectangular groove at different depths to obtain the depth of the rectangular groove after surfacing at each depth. During the measurement, a qualified measuring instrument (such as a vernier caliper, a ruler, etc.) can be used to accurately measure the depth of the rectangular groove on the test piece after the wire cutting.

[0048] See also Figure 5 In a specific embodiment of the present invention, step S400 includes: S401, measuring the cross-sections of multiple groups of rectangular grooves of different depths to obtain the depths of multiple groups of rectangular grooves of different depths after surfacing; S402, according to the depths of the rectangular grooves of the same depth in the multiple groups after surfacing, obtaining the depth of the rectangular grooves at each depth after surfacing. After setting multiple groups of rectangular grooves, there will be multiple measurement results of rectangular grooves at the same depth, so it is necessary to process through step S402 to obtain the depth of the rectangular grooves at each depth after surfacing. For example, it can be calculated by taking the average value, that is, the average value of the depths of the rectangular grooves of the same depth in the multiple groups after surfacing is used as the depth of the rectangular grooves at each depth after surfacing.

[0049] In a specific embodiment of the present invention, in step S400, for any rectangular groove: two side surfaces corresponding to the cross section of the rectangular groove are measured to obtain two depth values ​​of the rectangular groove, and the average value of the two depth values ​​is used as the depth of the rectangular groove after surfacing welding. Figure 4 In theory, the dimensions measured on the two sides corresponding to the cross section of the rectangular groove should be the same, but due to the existence of measurement errors, the measurement results may be slightly different. Therefore, in this embodiment, two depth values ​​can be obtained by measuring both sides once, and then the average of the two depth values ​​can be calculated.

[0050] In a specific embodiment of the present invention, the above two solutions can be combined, that is, the depths of multiple groups of rectangular grooves are measured simultaneously, and the two side surfaces of each group of rectangular grooves are measured.

[0051] Table 1: Test results of the effect of TIG cladding process on target defect depth

[0052]

[0053] In Table 1, surface 1 and surface 2 correspond to the measurement values ​​of the two side surfaces corresponding to the first set of rectangular grooves after cutting, and surface 3 and surface 4 correspond to the measurement values ​​of the two side surfaces corresponding to the second set of rectangular grooves after cutting. The average value in Table 1 is the depth of the rectangular groove after surfacing at each depth obtained in step S400.

[0054] Step S500, according to the depth of the rectangular groove after surfacing welding at each depth, a defect depth correction value is obtained, and the defect depth of the base material to be surfacing is corrected according to the defect depth correction value. The defect depth correction value is a value that has nothing to do with the depth of the rectangular groove, so it is necessary to calculate the defect depth correction value according to the depth of the rectangular groove after surfacing welding at each depth.

[0055] See also Figure 6 In a specific embodiment of the present invention, according to the depth of the rectangular groove after surfacing at each depth, a defect depth correction value is obtained, including: S501, according to the depth of the rectangular groove after surfacing at each depth, the difference in penetration of the rectangular groove at each depth is obtained; S502, according to the difference in penetration of the rectangular groove at each depth, a defect depth correction value is obtained. Taking the above Table 1 as an example, the depth of the rectangular groove after surfacing at each depth corresponds to the data in the row of the mean value, and different depths correspond to different values; the difference in penetration is the difference between the depth of the rectangular groove and the depth of the rectangular groove after surfacing; finally, the defect depth correction value is calculated based on the difference in penetration, for example, the calculation can be performed by taking the average value. In Table 1, the defect depth correction value is 1.566mm.

[0056] In a specific embodiment of the present invention, the defect depth of the base material to be surfacing is corrected according to the defect depth correction value, including: correcting the defect depth of the base material to be surfacing according to the sum of the preset defect depth and the defect depth correction value. After obtaining the defect depth correction value, in order to ensure that the depth size of the target defect (rectangular cut groove) under the subsequent product surfacing layer can meet the requirements of 2mm, 4mm, 6mm, 8mm, and 10mm after surfacing, the rectangular cut groove (open groove) depth should be processed on the surface of the base material to be surfacing according to the correction schemes of 2+1.566mm, 4+1.566mm, 6+1.566mm, 8+1.566mm, and 10+1.566mm to correct the influence of the TIG surfacing process on the target defect depth.

[0057] After the correction, the defect size under the cladding layer of the rectangular groove processed according to the correction scheme is closest to the standard requirements of 2mm, 4mm, 6mm, 8mm, and 10mm after cladding treatment. Therefore, the ultrasonic test data corresponding to the rectangular groove of 2+1.566mm is regarded as the ultrasonic test result corresponding to the standard 2mm defect; the same applies to other sizes.

[0058] It should be noted that the step division of the above methods is only for clear description. When implemented, they can be combined into one step or some steps can be split and decomposed into multiple steps. As long as they contain the same logical relationship, they are all within the scope of protection of this patent; adding insignificant modifications to the algorithm or process or introducing insignificant designs without changing the core design of the algorithm and process are all within the scope of protection of this patent.

[0059] In general, a more accurate database can be obtained through the above correction method. Based on this accurate database, the effectiveness and accuracy of the minimum defect detection capability test of the parent material UT inspection technology are naturally improved.

[0060] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for correcting the depth of base material defects in a cladding process, characterized in that: include: A plurality of rectangular grooves of different depths are provided on the test piece to simulate defects, wherein the material of the test piece is the same as that of the base material to be surfacing welded; Performing surfacing welding on the surface of the test piece along a length direction perpendicular to the rectangular cut groove to obtain a surfacing welded test piece; cutting the test piece after surfacing to reveal cross sections of the rectangular cut grooves of different depths; Measuring the cross-section of the rectangular groove at different depths to obtain the depth of the rectangular groove after surfacing welding at each depth; According to the depth of the rectangular groove after surfacing at each depth, a defect depth correction value is obtained, and the defect depth of the base material to be surfacing is corrected according to the defect depth correction value.

2. The method for correcting the depth of base material defects in cladding process according to claim 1, characterized in that: A plurality of rectangular grooves of different depths are arranged at intervals along a length direction perpendicular to the rectangular groove, and at least one cutting surface exists along the length direction perpendicular to the rectangular groove to cut each rectangular groove into two parts.

3. The method for correcting the depth of base material defects in cladding process according to claim 2, characterized in that: The depths of the rectangular grooves of different depths gradually increase or decrease along the length direction perpendicular to the rectangular grooves, and the depth difference between any two adjacent rectangular grooves is equal.

4. The method for correcting the depth of base material defects in cladding process according to claim 1, characterized in that: Set up multiple rectangular grooves of different depths on the test piece, including: A plurality of groups of rectangular grooves are arranged at intervals along a first direction on the test piece, each group of rectangular grooves is composed of a plurality of rectangular grooves of different depths arranged at intervals perpendicular to the first direction, and the first direction is the length or width direction of the test piece.

5. The method for correcting the depth of base material defects in cladding process according to claim 4, characterized in that: Measuring the cross-section of the rectangular groove at different depths to obtain the depth of the rectangular groove after surfacing at each depth includes: Measuring the cross sections of the rectangular grooves of multiple groups with different depths to obtain the depths of the rectangular grooves of multiple groups with different depths after surfacing welding; According to the depths of the rectangular grooves of the same depth in multiple groups after surfacing welding, the depths of the rectangular grooves after surfacing welding at each depth are obtained.

6. The method for correcting the depth of base material defects in cladding process according to claim 1, characterized in that: Set up multiple rectangular grooves of different depths on the test piece, including: Obtaining the length of each rectangular groove according to the preset depth of each rectangular groove, and the preset minimum multiple and maximum multiple; According to the minimum value of the depth of the rectangular grooves and a preset ratio, the widths of all the rectangular grooves are obtained; According to the preset depth, length and width of each rectangular groove, a plurality of rectangular grooves with different depths are arranged on the test piece.

7. The method for correcting the depth of base material defects in cladding process according to claim 1, characterized in that: When the surface of the test piece is subjected to surfacing treatment, the surfacing thickness is greater than or equal to a set threshold value.

8. The method for correcting the depth of base material defects in cladding process according to claim 1, characterized in that: In the step of measuring the cross-section of the rectangular groove at different depths to obtain the depth of the rectangular groove after surfacing at each depth, for any rectangular groove: Two side surfaces corresponding to the cross section of the rectangular groove are measured to obtain two depth values ​​of the rectangular groove, and the average value of the two depth values ​​is used as the depth of the rectangular groove after surfacing welding.

9. The method for correcting the depth of base material defects in cladding process according to claim 1, characterized in that: According to the depth of the rectangular groove after surfacing at each depth, the defect depth correction value is obtained, including: According to the depth of the rectangular groove after surfacing at each depth, the penetration difference of the rectangular groove at each depth is obtained; The defect depth correction value is obtained according to the difference in the penetration depth of the rectangular groove at each depth.

10. The method for correcting the depth of base material defects in cladding process according to claim 1, characterized in that: Correcting the defect depth of the base material to be clad according to the defect depth correction value includes: The defect depth of the base material to be surfacing is corrected according to the sum of the preset defect depth and the defect depth correction value.

Citation Information

Cited By

  • Method and device for detecting defects of lower base metal of surfacing layer on inner wall of connecting pipe and related equipment

    CN120870358A

  • Method and device for detecting defects under a parent material of a weld overlay on an inner wall of a pipe, and related equipment

    CN120870358B

  • Method for correcting defect depth of base material under surfacing process

    WO2026076812A1