Preparation method of nano-selenium solution

By using a combination of specific stabilizers and reducing agents in the preparation of nanoselenium solution, the problem of inaccurate nanoselenium stability and particle size control is solved, high bioavailability in the fermentation process of probiotics is achieved, and nanoselenium is promoted. Applications in various fields.

CN119038498APending Publication Date: 2024-11-29JIANGSU TARGET BIOMEDICINE RES INST
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411094413.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-29

Smart Images

  • Figure CN119038498A_ABST
    Figure CN119038498A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a nano-selenium solution. The preparation method comprises the following steps: (1) adding a stabilizer into a beaker; (2) slowly adding an aqueous solution containing a reducing agent into the beaker, and keeping magnetic stirring in the adding process until the stabilizing agent is completely dissolved; (3) slowly adding a sodium selenite aqueous solution into the solution obtained in the step (2), and magnetically stirring the solution obtained in the step (2) in the adding process; and (4) after the sodium selenite aqueous solution is added, immediately adjusting the pH value to a preset range by using a sodium hydroxide solution, and then continuously magnetically stirring for 30 minutes to prepare a red nano-selenium solution. The combination of the stabilizer and the reducing agent can effectively prevent aggregation and oxidation of the nano-selenium particles in the preparation process, so that the stability of the nano-selenium is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of biotechnology, and in particular to a method for preparing a nano-selenium solution. Background Art

[0002] Selenium is one of the trace elements necessary for the human body. It has many important biological functions such as anti-oxidation, detoxification, anti-inflammation, cell protection and repair, immune function regulation, and cancer prevention. It has good preventive and therapeutic effects on various diseases such as heart disease, cancer, and senile diseases (Rayman MP. Lancet. 2012; 379: 1256-1268). Epidemiological research results show that the body's selenium content is negatively correlated with the incidence of cancer, and selenium supplementation can effectively inhibit the formation of tumors (Schmidt RL et al. Croat Med J. 2012; 53: 535-550). Clark et al.'s clinical control trial results on cancer patients showed that selenium supplementation can reduce the incidence of lung cancer, prostate cancer, rectal cancer, and other cancers, and the mortality rate of cancer patients after selenium supplementation is significantly reduced (Zeng Het al. J Nutr Biochem. 2008; 19: 1-7).

[0003] Selenium in its natural state mainly exists in three forms: inorganic selenium, organic selenium and elemental selenium. Among them, red nano-selenium has higher safety and bioavailability, and shows wide application potential in many fields, especially in biomedicine, food additives, agriculture and environmental protection. However, the existing preparation methods of nano-selenium solutions have some limitations, such as insufficient stability, easy aggregation and transformation into gray-black inert elemental selenium and loss of activity, and inaccurate particle size control affecting bioavailability. These problems limit the efficiency and effect of nano-selenium in practical applications. Especially in the probiotic fermentation process, the excessively high particle size of nano-selenium affects its uptake by probiotics. The complex environment in the probiotic fermentation system puts higher requirements on the stability and bioavailability of nano-selenium.

[0004] Therefore, developing a new preparation process for nano-selenium solution to improve its stability and probiotic utilization has become the focus of research in this field. Summary of the invention

[0005] In order to solve the problems of the prior art, the object of the present invention is to provide a method for preparing a nano-selenium solution.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme: A method for preparing a nano-selenium solution of the present invention comprises the following steps:

[0007] (1) Add stabilizer to a beaker;

[0008] (2) slowly adding the aqueous solution containing the reducing agent into the beaker, and maintaining magnetic stirring during the addition process until the stabilizer is completely dissolved;

[0009] (3) slowly adding the sodium selenite aqueous solution to the solution obtained in step (2), during which the solution in step (2) is under magnetic stirring;

[0010] (4) After the sodium selenite aqueous solution is added, the pH is immediately adjusted to a predetermined range using a sodium hydroxide solution, and then the magnetic stirring is continued for 30 minutes to obtain red nano-selenium.

[0011] Furthermore, in step (1), the stabilizer is selected from at least one of epigallocatechin gallate (EGCG), chitosan, gum arabic, bovine serum albumin (BSA) or sodium hyaluronate.

[0012] Furthermore, in step (2), the reducing agent is selected from at least one of reduced glutathione GSH or vitamin C (Vc).

[0013] Furthermore, in step (1), the concentration range of epigallocatechin gallate EGCG is 0.1mM-40mM; the concentration range of chitosan is 0.01%-0.7%, and the molecular weight range of chitosan is 100KD-1000KD; the concentration range of gum arabic is 0.04%-0.4%, and the molecular weight range of gum arabic is 200KD-2000KD; the concentration range of bovine serum albumin BSA is 0.4mg / ml-60mg / ml; the concentration range of sodium hyaluronate is 0.02%-0.25%, and the molecular weight range of sodium hyaluronate is 200KD-2000KD.

[0014] Furthermore, in step (2), the final concentration of the reducing agent in the reaction system is 5mM-50mM (GSH) and 5mM-100mM (Vc).

[0015] Furthermore, in step (3), the final concentration of sodium selenite in the reaction system is 5 mM.

[0016] Furthermore, in step (4), in the step of adjusting the pH, the pH value ranges from 5.0 to 9.0.

[0017] Furthermore, the peak value of the nano-selenium particle size distribution prepared by the above steps can be accurately controlled within the range of 20nm-60nm, and the particle size is mainly distributed within the range of 10nm-150nm.

[0018] The invention discloses a nano-selenium solution prepared by a method, wherein the nano-selenium exhibits good stability under probiotic fermentation conditions.

[0019] Beneficial effects: The stabilizer and reducing agent combination used in the present invention can effectively prevent the aggregation and oxidation of nano-selenium particles during the preparation process, thereby improving the stability of nano-selenium.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] (1) The present invention successfully prepares nano-selenium with a particle size distribution peak value accurately controlled within a range of 20 nm to 60 nm and a particle size mainly distributed within a range of 10 nm to 150 nm by optimizing the selection of stabilizers and reducing agents and precisely controlling the reaction conditions.

[0022] (2) Precise particle size control: By adjusting the concentration of the stabilizer and the reaction conditions, the present invention can precisely control the particle size of nano-selenium to be between 10 nm and 150 nm, and the distribution peak value to be between 20 nm and 60 nm, so that it has better bioavailability during the probiotic fermentation process.

[0023] (3) Suitable for fermentation process: The stability study of the nano-selenium of the present invention under simulated probiotic fermentation conditions showed that the nano-selenium can remain stable under fermentation conditions and the aggregation of nano-selenium is greatly improved, which is of great significance for improving the growth rate and biological activity of probiotics.

[0024] (4) Broad application prospects: The preparation method of the nano-selenium solution of the present invention is not only suitable for laboratory-scale preparation, but also provides the possibility for industrial production, which helps to promote the application and development of nano-selenium in various fields. The preparation method of the nano-selenium solution of the present invention has significant advantages in improving the stability of nano-selenium and the accuracy of particle size control, and provides a new technical approach for the application of nano-selenium in probiotic fermentation and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0026] Figure 1 This is a graph showing the particle size detection results of nano-selenium prepared using EGCG as a stabilizer according to the present invention.

[0027] Figure 2 This is a graph showing the particle size detection results of nano-selenium prepared using chitosan (molecular weight of about 100KD) as a stabilizer according to the present invention.

[0028] Figure 3This is a graph showing the particle size detection results of nano-selenium prepared using chitosan (molecular weight of about 1000KD) as a stabilizer according to the present invention.

[0029] Figure 4 This is a graph showing the particle size detection results of nano-selenium prepared using gum arabic (molecular weight of about 200KD) as a stabilizer according to the present invention.

[0030] Figure 5 This is a graph showing the particle size detection results of nano-selenium prepared using gum arabic (molecular weight of about 2000KD) as a stabilizer according to the present invention.

[0031] Figure 6 This is a graph showing the particle size detection results of nano-selenium prepared using BSA (0.4 mg / ml) as a stabilizer according to the present invention.

[0032] Figure 7 This is a graph showing the particle size detection results of nano-selenium prepared using BSA (60 mg / ml) as a stabilizer according to the present invention.

[0033] Figure 8 This is a graph showing the particle size detection results of nano-selenium prepared using sodium hyaluronate (molecular weight 200KD) as a stabilizer according to the present invention.

[0034] Fig. 9 This is a graph showing the particle size detection results of nano-selenium prepared using sodium hyaluronate (molecular weight 2000KD) as a stabilizer according to the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0037] In the present application, "-less than one" means one or more, and "more than one" means two or more. "The following - less than one item" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "a, b, or c - less than one item", or "a, b, and c - less than one item", can all mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0038] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0039] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0040] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0041] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0042] The first aspect of the present invention provides a method for preparing a nano-selenium solution, comprising the following steps:

[0043] (1) Add stabilizer to a beaker;

[0044] (2) slowly adding the aqueous solution containing the reducing agent into the beaker, and maintaining magnetic stirring during the addition process until the stabilizer is completely dissolved;

[0045] (3) slowly adding the sodium selenite aqueous solution to the solution obtained in step (2), during which the solution in step (2) is under magnetic stirring;

[0046] (4) After the sodium selenite aqueous solution is added, the pH is immediately adjusted to a predetermined range using a sodium hydroxide solution, and then the magnetic stirring is continued for 30 minutes to obtain a nano-selenium solution.

[0047] In some embodiments, in step (1), the stabilizer is epigallocatechin gallate (EGCG).

[0048] In some embodiments, in step (1), the stabilizer is chitosan.

[0049] In some embodiments, in step (1), the stabilizer is gum arabic.

[0050] In some embodiments, in step (1), the stabilizer is bovine serum albumin (BSA).

[0051] In some embodiments, in step (1), the stabilizer is sodium hyaluronate.

[0052] In some embodiments, in step (2), the reducing agent is reduced glutathione GSH.

[0053] In some embodiments, in step (2), the reducing agent is vitamin C (Vc).

[0054] In some embodiments, in step (1), the concentration of the stabilizer ranges from 0.1 mM to 40 mM (for EGCG).

[0055] In some embodiments, in step (1), the concentration of the stabilizer ranges from 0.01% to 0.7% (for chitosan).

[0056] In some embodiments, in step (1), the concentration of the stabilizer ranges from 0.04% to 0.4% (for gum arabic).

[0057] In some embodiments, in step (1), the concentration of the stabilizer ranges from 0.04% to 0.4% (for gum arabic).

[0058] In some embodiments, in step (1), the concentration of the stabilizer ranges from 0.4 mg / ml to 60 mg / ml (for BSA).

[0059] In some embodiments, in step (1), the concentration of the stabilizer ranges from 0.02% to 0.25% (for sodium hyaluronate).

[0060] In some embodiments, in step (2), the final concentration of the reducing agent in the reaction system is 5 mM-50 mM (GSH).

[0061] In some embodiments, in step (2), the final concentration of the reducing agent in the reaction system is 5 mM-100 mM (Vc).

[0062] In step (3), the final concentration of sodium selenite in the reaction system is 5 mM.

[0063] In some embodiments, in step (1), the molecular weight of the stabilizer ranges from 100KD to 1000KD (for chitosan).

[0064] In some embodiments, in step (1), the molecular weight of the stabilizer ranges from 200KD to 2000KD (for gum arabic).

[0065] In some embodiments, in step (1), the molecular weight of the stabilizer ranges from 200KD to 2000KD (for sodium hyaluronate).

[0066] In step (4), in the step of adjusting the pH, the pH value ranges from 5.0 to 9.0.

[0067] In some embodiments, the peak value of the particle size distribution of the nano-selenium prepared by the above steps can be precisely controlled within a range of 20 nm-60 nm, and the particle size is mainly distributed within a range of 10 nm-150 nm.

[0068] The second aspect of the present invention provides a nano-selenium solution prepared by the method, wherein the nano-selenium exhibits good stability under probiotic fermentation conditions.

[0069] Example 1

[0070] Preparation method of nano-selenium solution using EGCG as stabilizer

[0071] Weigh 4.5 mg of EGCG into a 25 ml beaker, add 8 ml of 20 mM Vc, and stir magnetically for 5 min; add 2 ml of 25 mM sodium selenite aqueous solution and stir. The total volume of the solution is 10 ml. Immediately adjust the solution to pH 2.5 with dilute hydrochloric acid, and control the adjustment and pH stabilization process within 30 min; then adjust the pH to 8.5 with 5 M and 0.2 M sodium hydroxide solutions, and control the adjustment and pH stabilization process within 20 min to obtain nano-selenium.

[0072] The particle size distribution peak of the prepared nano-selenium was precisely controlled at about 45nm by using a particle size potential analyzer (Malvern Nano ZSE), and the particle size was mainly distributed in the range of 10nm-150nm. Figure 1 .

[0073] Example 2

[0074] Preparation method of nano-selenium solution using chitosan (molecular weight about 100KD) as stabilizer

[0075] Measure 5 ml of 0.2% chitosan (molecular weight about 100KD) solution into a 25 ml beaker, add 1 ml of pure water and 2 ml of 350 mM Vc aqueous solution, and mix by magnetic stirring; add 2 ml of 25 mM sodium selenite aqueous solution, mix by magnetic stirring at room temperature, and then immediately adjust the pH to 7.2 with 1 M NaOH, adjust the pH and stir for a total of 30 minutes to prepare a nano-selenium solution.

[0076] The particle size distribution peak of the prepared nano-selenium can be accurately controlled within the range of 20nm-60nm by using a particle size potential analyzer (Malvern Nano ZSE), and the particle size is mainly distributed within the range of 10nm-150nm. Figure 2 .

[0077] Example 3

[0078] Preparation method of nano-selenium solution using chitosan (molecular weight about 500KD) as stabilizer

[0079] Measure 5 ml of 0.2% chitosan (molecular weight about 500KD) solution into a 25 ml beaker, add 1 ml of pure water and 2 ml of 350 mM Vc aqueous solution, and mix by magnetic stirring; add 2 ml of 25 mM sodium selenite aqueous solution, mix by magnetic stirring at room temperature, and then immediately adjust the pH to 7.2 with 1 M NaOH, adjust the pH and stir for a total of 30 minutes to prepare a nano-selenium solution.

[0080] The particle size of the prepared nano-selenium was mainly distributed in the range of 10nm-150nm, with a peak value of 20nm-60nm, and the results were consistent with Figure 2 , 3 Highly similar.

[0081] Example 4

[0082] Preparation method of nano-selenium solution using chitosan (molecular weight about 1000KD) as stabilizer

[0083] Measure 5 ml of 0.2% chitosan (molecular weight about 1000KD) solution into a 25 ml beaker, add 1 ml of pure water and 2 ml of 350 mM Vc aqueous solution, and mix by magnetic stirring; add 2 ml of 25 mM sodium selenite aqueous solution, mix by magnetic stirring at room temperature, and then immediately adjust the pH to 7.2 with 1 M NaOH, adjust the pH and stir for a total of 30 minutes to prepare a nano-selenium solution.

[0084] The particle size distribution peak of the prepared nano-selenium can be accurately controlled within the range of 20nm-60nm by using a particle size potential analyzer (Malvern Nano ZSE), and the particle size is mainly distributed within the range of 10nm-150nm. Figure 3 .

[0085] Example 5

[0086] Preparation method of nano-selenium solution using gum arabic (molecular weight about 200KD) as stabilizer

[0087] Pipette 0.4 ml of 1% gum arabic (molecular weight about 200KD) aqueous solution into a 25 ml beaker, add 7.2 ml of pure water, add 0.4 ml of 200 mM Vc aqueous solution, and stir magnetically evenly; add 2 ml of 25 mM sodium selenite aqueous solution, stir magnetically for 5 minutes, and then immediately adjust the pH to 6.5 with 1 M NaOH, adjust the pH and subsequently stir for a total of 30 minutes to prepare a nano-selenium solution.

[0088] The particle size of the prepared nano-selenium was mainly distributed in the range of 10nm-150nm, and the distribution peak was controlled in the range of 20nm-60nm. The results are as follows Figure 4 .

[0089] Example 6

[0090] Preparation method of nano-selenium solution using gum arabic (molecular weight about 600KD) as stabilizer

[0091] Pipette 0.4 ml of 1% gum arabic (molecular weight about 600KD) aqueous solution into a 25 ml beaker, add 7.2 ml of pure water, add 0.4 ml of 200 mM Vc aqueous solution, and stir magnetically evenly; add 2 ml of 25 mM sodium selenite aqueous solution, stir magnetically for 5 minutes, and then immediately adjust the pH to 6.5 with 1 M NaOH, adjust the pH and subsequently stir for a total of 30 minutes to prepare a nano-selenium solution.

[0092] The particle size distribution peak of the prepared nano-selenium was precisely controlled at 20nm-60nm (40nm) by using a particle size potential analyzer (Malvern Nano ZSE), and the particle size was mainly distributed in the range of 10nm-150nm. Figure 4 , 5 Highly similar.

[0093] Example 7

[0094] Preparation method of nano-selenium solution using gum arabic (molecular weight about 2000KD) as stabilizer

[0095] Pipette 0.2 ml of 1% gum arabic (molecular weight about 2000KD) aqueous solution into a 25 ml beaker, add 7.4 ml of pure water, add 0.4 ml of 200 mM Vc aqueous solution, and stir magnetically evenly; add 2 ml of 25 mM sodium selenite aqueous solution, stir magnetically for 5 minutes, and then immediately adjust the pH to 6.5 with 1 M NaOH, adjust the pH and subsequently stir for a total of 30 minutes to prepare a nano-selenium solution.

[0096] The particle size of the prepared nano-selenium was tested with a particle size potential analyzer (Malvern Nano ZSE) for 3 times. The peak value of the particle size distribution of the nano-selenium can be accurately controlled within the range of 20nm-60nm, and the particle size is mainly distributed within the range of 10nm-150nm. The results are as follows: Figure 5 .

[0097] Example 8

[0098] Preparation method of nano-selenium solution using BSA as stabilizer

[0099] Weigh 4 mg of BSA into a 25 ml beaker, add 8 ml of 37.5 mM GSH aqueous solution, stir magnetically for 40 min until BSA is completely dissolved, slowly add 2 ml of 25 mM sodium selenite aqueous solution, and stir magnetically to mix, then immediately adjust the pH to 7.2 with 1 M NaOH, adjust the pH and stir for a total of 30 min to prepare a nano-selenium solution.

[0100] The particle size distribution peak of the prepared nano-selenium can be accurately controlled at 20nm by using a particle size potential analyzer (Malvern Nano ZSE), and the particle size is mainly distributed at 150nm. The results are as follows Figure 6 .

[0101] Example 9

[0102] Preparation method of nano-selenium solution using BSA as stabilizer

[0103] Weigh 60 mg of BSA into a 25 ml beaker, add 8 ml of 37.5 mM GSH aqueous solution, stir magnetically for 40 min until BSA is completely dissolved, slowly add 2 ml of 25 mM sodium selenite aqueous solution, stir magnetically to mix, then immediately adjust the pH to 7.2 with 1 M NaOH, adjust the pH and stir for a total of 30 min to prepare a nano-selenium solution.

[0104] The particle size distribution peak of the prepared nano-selenium can be accurately controlled at 60nm by using a particle size potential analyzer (Malvern Nano ZSE), and the particle size is mainly distributed at 10nm. Figure 6 , 7 Highly similar.

[0105] Example 10

[0106] Preparation method of nano-selenium solution using BSA as stabilizer

[0107] Weigh 600 mg of BSA into a 25 ml beaker, add 8 ml of 37.5 mM GSH aqueous solution, stir magnetically for 40 min until BSA is completely dissolved, slowly add 2 ml of 25 mM sodium selenite aqueous solution, stir magnetically to mix, then immediately adjust the pH to 7.2 with 1 M NaOH, adjust the pH and stir for a total of 30 min to prepare a nano-selenium solution.

[0108] The particle size distribution peak of the prepared nano-selenium can be accurately controlled at 40nm by using a particle size potential analyzer (Malvern Nano ZSE), and the particle size is mainly distributed at 50nm. The results are as follows Figure 7 .

[0109] Embodiment 11

[0110] Preparation method of nano-selenium solution using sodium hyaluronate (molecular weight of about 200KD) as stabilizer

[0111] Take 4 ml of 0.5% sodium hyaluronate (molecular weight is about 200KD) aqueous solution, slowly add 4 ml of 75 mM GSH aqueous solution, stir evenly with magnetic stirring at room temperature, slowly add 2 ml of 25 mM sodium selenite aqueous solution, and stir magnetically to mix, then immediately adjust the pH to 8.0 with 1 M NaOH, adjust the pH and stir for 30 minutes to prepare a nano-selenium solution.

[0112] The particle size of the prepared nano-selenium was tested by a particle size potential analyzer (Malvern Nano ZSE) for 3 times. The peak value of the particle size distribution of the prepared nano-selenium can be accurately controlled within the range of 20nm-60nm, and the particle size is mainly distributed within the range of 10nm-150nm. The results are as follows: Figure 8 .

[0113] Example 12

[0114] Preparation method of nano-selenium solution using sodium hyaluronate (molecular weight of about 1000KD) as stabilizer

[0115] Take 4 ml of 0.5% sodium hyaluronate (molecular weight is about 200KD) aqueous solution, slowly add 4 ml of 75 mM GSH aqueous solution, stir evenly with magnetic stirring at room temperature, slowly add 2 ml of 25 mM sodium selenite aqueous solution, and stir magnetically to mix, then immediately adjust the pH to 8.0 with 1 M NaOH, adjust the pH and stir for 30 minutes to prepare a nano-selenium solution.

[0116] The particle size of the prepared nano-selenium was measured by a particle size potential analyzer (Malvern Nano ZSE) for 3 times. The peak value of the particle size distribution of the prepared nano-selenium can be accurately controlled within 20nm-60nm (about 28nm), and the particle size is mainly distributed within 10nm-150nm. The results are consistent with Figure 7 , 8 Highly similar.

[0117] Embodiment 13

[0118] Preparation method of nano-selenium solution using sodium hyaluronate (molecular weight of about 2000KD) as stabilizer

[0119] Take 4 ml of 0.5% sodium hyaluronate (molecular weight is about 2000KD) aqueous solution, slowly add 4 ml of 75 mM GSH aqueous solution, stir evenly with magnetic stirring at room temperature, slowly add 2 ml of 25 mM sodium selenite aqueous solution, and stir magnetically to mix, then immediately adjust the pH to 8.0 with 1 M NaOH, adjust the pH and stir for a total of 30 minutes to prepare a nano-selenium solution.

[0120] The particle size of the prepared nano-selenium was tested by a particle size potential analyzer (Malvern Nano ZSE) for 3 times. The peak value of the particle size distribution of the prepared nano-selenium can be accurately controlled within the range of 20nm-60nm, and the particle size is mainly distributed within the range of 10nm-150nm. Fig. 9 .

[0121] Test Example 1

[0122] Nano-selenium particle size detection

[0123] The nano-selenium samples were mixed and the particle size was measured using a particle size potential analyzer (Malvern Nano ZSE).

[0124] Test Example 2

[0125] Study on the stability of nano-selenium under fermentation conditions

[0126] According to the solution environment of probiotic fermentation, the stability test conditions of nano-selenium were set to pH 4.0 and temperature 40°C. According to the fermentation time of probiotics, the test duration was set to 63 hours. After the test, the particle size and concentration changes of nano-selenium were detected to verify the stability of nano-selenium under fermentation conditions.

[0127] The inspection conditions were divided into three groups:

[0128] (1) Stability of nano-selenium at pH 4.0 and 4°C for 63 hours

[0129] Take 25 ml of nano-selenium solution, adjust the pH to 4.0, place it in a 4°C environment, observe the changes in the solution, and after 63 hours, directly take a sample for particle size detection.

[0130] (2) Stability of nano-selenium at 40°C for 63 hours

[0131] Take 10 ml of the nano-selenium solution and put it into a 15 ml centrifuge tube, place it in a 40°C water bath for 63 hours, observe the changes in the solution, and take the supernatant for particle size detection.

[0132] (3) Stability of nano-selenium at pH 4.0 and 40°C for 63 hours

[0133] Take 25 ml of nano-selenium solution, adjust the pH to 4.0, separate 10 ml into a 15 ml centrifuge tube, place it in a 40°C water bath for 63 hours, and observe the changes in the solution. After 63 hours, centrifuge at 10,000 rpm for 10 minutes, and carefully take the supernatant for particle size detection.

[0134] The experimental results are shown in Tables 1 and 2. Under pH 4.0, the solution is clear and the particle size does not change much, so the stability is less affected. At 40°C and 63 hours, the solution is clear with only a small amount of precipitation, and the peak value of the particle size distribution increases to about 80 nm. The stability is slightly affected but still acceptable. After 24 hours of action at pH 4.0 and 40°C, the solution is clear, and after 63 hours, the solution becomes turbid and the particle size increases significantly. However, during the fermentation process, the pH value gradually increases, and pH 4.0 will not exceed 24 hours. Therefore, nano-selenium can remain stable under fermentation conditions. The solution stability of nano-selenium under fermentation conditions is shown in Table 1 (SeNPs-031901, SeNPs-031902, SeNPs-031903, SeNPs-031904, and SeNPs-031905 represent nano-selenium prepared by stabilizers epigallocatechin gallate EGCG, chitosan, gum arabic, bovine serum albumin BSA, and sodium hyaluronate, respectively):

[0135] Table 1

[0136]

[0137] The peak detection results of the stability particle size distribution of nano-selenium under fermentation conditions (unit: nm) are shown in Table 2:

[0138] Table 2

[0139]

[0140]

[0141] Note: 1, 2, and 3 in the above table represent the results of three tests on the same sample.

[0142] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and the scope of protection of the present invention is defined by the attached claims, description and their equivalents.

Claims

1. A method for preparing a nano-selenium solution, characterized in that The steps include: (1) Add stabilizer to a beaker; (2) slowly adding the aqueous solution containing the reducing agent into the beaker, and maintaining magnetic stirring during the addition process until the stabilizer is completely dissolved; (3) slowly adding the sodium selenite aqueous solution to the solution obtained in step (2), during which the solution in step (2) is under magnetic stirring; (4) After the sodium selenite aqueous solution is added, the pH is immediately adjusted to a predetermined range using a sodium hydroxide solution, and then the magnetic stirring is continued for 30 minutes to obtain a red nano-selenium solution.

2. The method for preparing a nano-selenium solution according to claim 1, wherein: In step (1), the stabilizer is selected from at least one of epigallocatechin gallate (EGCG), chitosan, gum arabic, bovine serum albumin (BSA) or sodium hyaluronate.

3. The method for preparing a nano-selenium solution according to claim 1, wherein: In step (2), the reducing agent is selected from at least one of reduced glutathione GSH or vitamin C.

4. The method for preparing the nano-selenium solution according to claim 2, wherein: In step (1), the concentration range of epigallocatechin gallate EGCG is 0.1mM-40mM; the concentration range of chitosan is 0.01%-0.7%, and the molecular weight range of chitosan is 100KD-1000KD; the concentration range of gum arabic is 0.04%-0.4%, and the molecular weight range of gum arabic is 200KD-2000KD; the concentration range of bovine serum albumin BSA is 0.4mg / ml-60mg / ml; the concentration range of sodium hyaluronate is 0.02%-0.25%, and the molecular weight range of sodium hyaluronate is 200KD-2000KD.

5. The method for preparing the nano-selenium solution according to claim 1, characterized in that: In step (2), the final concentration of the reducing agent in the reaction system is 5mM-50mM (GSH) and 5mM-100mM (Vc).

6. The method for preparing the nano-selenium solution according to claim 1, characterized in that: In step (3), the final concentration of sodium selenite in the reaction system is 5 mM.

7. The method for preparing the nano-selenium solution according to claim 1, characterized in that: In step (4), in the step of adjusting the pH, the pH value ranges from 5.0 to 9.

0.

8. The method for preparing the nano-selenium solution according to claim 1, characterized in that: The peak value of the nano-selenium particle size distribution prepared by the above steps can be precisely controlled within a range of 20nm-60nm.

9. A nano-selenium solution prepared by the method according to any one of claims 1 to 8, characterized in that: The nano-selenium exhibits good stability under probiotic fermentation conditions.

Citation Information

Patent Citations

  • Functional nano-selenium probe as well as preparation method of functional nano-selenium probe and application of functional nano-selenium probe in preparation of medicine for diagnosing and treating bacterial infection

    CN107179403A

  • Preparation of quercetin-loaded nano-selenium and application of quercetin-loaded nano-selenium in treating Alzheimer's disease

    CN110664838A

  • Preparation method of tannic acid-zinc coordinated chitosan-selenium nanoparticles

    CN115919801A

  • Method Of Treating, Reducing, Or Alleviating A Medical Condition In A Patient

    US20210228619A1